A dispersion comprising a carbon material and vinylpyrrolidone copolymer, and uses thereof

A carbon nanotube dispersion with a copolymer dispersant of vinyl pyrrolidone or vinylcaprolactam and acrylic acid enhances dispersibility, addressing uniformity issues and improving battery performance.

WO2026236641A1PCT designated stage Publication Date: 2026-11-12HERCULES LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/027325
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-08
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing technologies face challenges in uniformly dispersing carbon materials such as carbon nanotubes in solvents or binders, which affects their performance in battery components and electronic devices, necessitating improved dispersants for enhanced electrical conductivity and mechanical strength.

Method used

A carbon nanotube dispersion using a copolymer dispersant comprising more than 80 wt.% of vinyl pyrrolidone or vinylcaprolactam and less than 20 wt.% of functionalized or unfunctionalized monomers like acrylic acid, combined with a solvent and optionally an amine-based pH neutralizer, to enhance dispersibility and electro-chemical properties.

Benefits of technology

The dispersion provides improved electrical conductivity, mechanical strength, and electro-chemical properties, leading to higher energy density, extended cycle life, and better power efficiency in lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026027325_12112026_PF_FP_ABST
    Figure US2026027325_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure relates to carbon material dispersions comprising dispersant (A) a copolymer of: (i) more than 80 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20 wt.% of at least one functionalized or unfunctionalized monomer selected from acrylic acid, methacrylic acid, itaconic acid, maleic acid and maleic anhydride. The present disclosure further provides a carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20 wt.% of acrylic acid; (B) carbon nanotubes; (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.
Need to check novelty before this filing date? Find Prior Art

Description

A DISPERSION COMPRISING A CARBON MATERIAL AND VINYLPYRROLIDONE COPOLYMER, AND USES THEREOFFIELD

[0001] The presently disclosed process(es), procedure(s), method(s), product(s), result(s), and / or concept(s) (collectively referred to hereinafter as the “present disclosure”) relates generally to carbon material dispersions comprising a dispersant comprising a copolymer of: (i) more than 80 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20 wt.% of at least one functionalized or unfunctionalized monomer selected from acrylic acid, methacrylic acid, itaconic acid, maleic acid and maleic anhydride.BACKGROUND

[0002] Carbon materials are widely used in lithium-ion batteries to improve electrical conductivity, enhance mechanical strength, and increase battery performance. In electrode substrates, carbon materials form a conductive network that helps electrons move efficiently, improving charge-discharge rates and cycle stability. Their nanoscale structure also supports better contact between active materials and current collectors, reducing internal resistance. When used to form electroconductive films, battery components, or in the fabrication of various electronic devices, carbon materials need to be effectively dispersed in matrices such as solutions or binders. Extensive attempts have been made to develop novel dispersants or methods for uniformly dispersing carbon materials in solvents or binders.

[0003] The present disclosure focuses on developing a carbon material dispersion, specifically a carbon nanotube dispersion using a copolymer dispersant that provides enhanced dispersibility and better electro-chemical properties. The carbon material dispersions of the present disclosure are useful as highly efficient conductive agents for battery components, which can replace traditional conductive agents such as carbon black, acetylene black, graphene nanotubes, graphene sheets, graphite and carbon fiber. It has excellent characteristics including high length-to-diameter (LD) ratio, considerable specific surface area (SSA) value and low volume resistivity.SUMMARY

[0004] The present disclosure provides a dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20 wt.% of at least one functionalized or unfunctionalized monomer selected from acrylic acid, methacrylic acid, itaconic acid, maleic acid and maleic anhydride; (B) carbon materials; (C) a solvent; and (D) optionally, an amine-based pH neutralizer.

[0005] Another aspect of the present disclosure provides a carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20 wt.% of acrylic acid; (B) carbon nanotubes; (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0006] Another aspect of the present disclosure provides a carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone and, (ii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0007] Another aspect of the present disclosure provides a carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinylcaprolactam, and (ii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C)N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0008] Another aspect of the present disclosure provides a carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, (ii) less than 10 wt.% vinylcaprolactam, and (iii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0009] Another aspect of the present disclosure provides a carbon nanotube dispersion used as an adhesive conductive layer coating on substrates including, but are not limited to aluminum foil, copper foil, and polyester film, wherein the coating exhibits no-feathering and lower-cratering properties.BRIEF DESCRIPTION OF THE FIGURES

[0010] Illustrative embodiments of the present disclosure are described in detail below with reference to the attached drawing figures, which are incorporated by reference herein and wherein:

[0011] FIG. 1 illustrates impedance measurements of lithium iron phosphate (LFP) cathodes fabricated using carbon nanotube (CNT) dispersions, wherein the dispersions include (i) dispersant sample C19, (ii) no dispersant (blank), and (iii) dispersant sample Cl (PVP K-30).

[0012] FIG. 2 illustrates specific capacity measurements of lithium iron phosphate (LFP) cathodes fabricated using carbon nanotube (CNT) dispersions, wherein the dispersions include (i) dispersant sample C19, (ii) no dispersant (blank), and (iii) dispersant sample Cl (PVP K-30).

[0013] FIG. 3 demonstrates no-feathering and lower-cratering properties of the adhesive conductive layer coating tested using the carbon nanotube dispersion of the present disclosure.DETAILED DESCRIPTION

[0014] Before explaining at least one aspect of the disclosed and / or claimed inventive concept(s) in detail, it is to be understood that the disclosed and / or claimed inventive concept(s) is not limited in its disclosure to the details of construction and the arrangement of the components or steps or methodologies set forth in the following description or illustrated in the drawings. The disclosed and / or claimed inventive concept(s) is capable of other aspects or of being practiced or carried out in various ways. Also, it is to be understood that the phraseology and terminology employed herein is for the purpose of description and should not be regarded as limiting.

[0015] Unless otherwise defined herein, technical terms used in connection with the disclosed and / or claimed inventive concept(s) shall have the meanings that are commonly understood by those of ordinary skill in the art. Further, unless otherwise required by context, singular terms shall include pluralities, and plural terms shall include the singular.

[0016] The singular forms "a," "an," and "the" include plural forms unless the context clearly dictates otherwise specified or clearly implied to the contrary by the context in which the reference is made. The term “Comprising” includes the more restrictive claims such as “Consisting essentially of’ and “Consisting of.”

[0017] For purposes of the following detailed description, other than in any operating examples, or where otherwise indicated, numbers that express, for example, quantities of ingredients used in the specification and claims are to be understood as being modified in all instances by the term "about". The numerical parameters set forth in the specification and attached claims are approximations that may vary depending upon the desired properties to be obtained in carrying out the invention.

[0018] All percentages, parts, proportions, and ratios as used herein, are by weight of the total composition, unless otherwise specified. All such weights as they pertain to listed ingredients are based on the active level and, therefore; do not include solvents or by-products that may be included in commercially available materials, unless otherwise specified.

[0019] All publications, articles, papers, patents, patent publications, and other references cited herein are hereby incorporated herein in their entirety for all purposes to the extent consistent with the disclosure herein.

[0020] The use of the term “at least one” will be understood to include one as well as any quantity more than one, including but are not limited to, 1, 2, 3, 4, 5, 10, 15, 20, 30, 40, 50, 100, etc. The term “at least one” may extend up to 100 or 1000 or more depending on the term to which it is attached. In addition, the quantities of 100 / 1000 are not to be considered limiting as lower or higher limits may also produce satisfactory results.

[0021] As used herein, the words “comprising” (and any form of comprising, such as “comprise” and “comprises”), “having” (and any form of having, such as “have” and “has”), “including” (and any form of including, such as “includes” and “include”) or “containing” (and any form of containing, such as “contains” and “contain”) are inclusive or open-ended and do not exclude additional, unrecited elements or method steps.

[0022] The term “and combinations thereof’ as used herein refers to all permutations and combinations of the listed items preceding the term. For example, “A, B, C, and combinations thereof’ is intended to include at least one of: A, B, C, AB, AC, BC, or ABC, and if order is important in a particular context, also BA, CA, CB, CBA, BCA, ACB, BAC, or CAB. Continuing with this example, expressly included are combinations that contain repeats of one or more item or term, such as BB, AAA, MB, BBC, AAABCCCC, CBBAAA, CABABB, and so forth. The skilled artisan will understand that typically there is no limit on the number of items or terms in any combination, unless otherwise apparent from the context.

[0023] The term "branched and unbranched alkyl groups" refers to alkyl groups, which may be straight chained or branched. Branched groups include isopropyl, tert-butyl, and the like.

[0024] References herein to “one embodiment” or “one aspect” or “one version” or “one objective” of the disclosure include one or more such embodiment, aspect, version, or objective, unless the context clearly dictates otherwise.

[0025] The term “dispersion” refers to a dispersion composition comprising a dispersant, carbon materials, at least one solvent, and optionally, an amine-based pH neutralizer.

[0026] The term “polymer” refers to a compound comprising repeating structural units (monomers) connected by covalent chemical bonds. Polymers may be further derivatized, crosslinked, grafted or end capped.

[0027] The term “copolymer” refers to a polymer consisting essentially of two or more differenttypes of monomers polymerized to obtain the copolymer. Non-limiting examples of polymers include copolymers, terpolymers, tetrapolymers, quaternary polymers, and homologues.

[0028] The term “carbon material” refers to a diverse class of carbon-based substances that include structures such as carbon nanotubes, carbon nanofibers, short nanotubes, carbon particles, carbon black, acetylene black, ketjen black, graphene, graphite, and their combinations. These materials exhibit unique electrical, thermal, and mechanical properties, making them essential in applications ranging from energy storage devices, electronics devices to coatings and advanced composites.

[0029] The term “no-feathering” refers to a property of a coated film that ensures its edges remain sharp, well-defined, and unblended, preventing any unintended diffusion, feathering, or spread of the coating beyond its applied boundaries.

[0030] The term “low-cratering” refers to a property of a coated film that minimizes the formation of small pits, holes, or depressions on its surface, ensuring a smooth and uniform finish.

[0031] The term “battery” used herein includes a single electrochemical cell, or unicell, and / or one or more electrochemical cells connected in series and / or in parallel as known by those of skill in the art. Furthermore, the term “battery” includes, but is not limited to, rechargeable batteries and / or secondary batteries and / or electrochemical cells. It shall also be understood that the term “lithium-ion” battery as used herein, and as well known in the art, encompasses rechargeable or secondary lithium-ion batteries.

[0032] In a non-limiting embodiment, the present disclosure provides a dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20 wt.% of at least one functionalized or unfunctionalized monomer selected from acrylic acid, methacrylic acid, itaconic acid, maleic acid and maleic anhydride; (B) carbon materials; (C) a solvent; and (D) optionally, an amine-based pH neutralizer.

[0033] In another embodiment the dispersant (A) comprises a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, and (ii) less than 20 wt.% acrylic acid. Present disclosure further discloses the amount of vinyl pyrrolidone monomer in the copolymer of dispersant (A) ranges from about 80.01 wt.% to about 85.0 wt.%, or from about 85.0 wt.% to about 90.0 wt.%, or from about 90.0wt.% to about 95.0 wt.%, or from about 95.0 wt.% to about 99.95 wt.% based on the total weight of the copolymer; the amount of acrylic acid monomer in the copolymer of dispersant (A) ranges from about 0.05 wt.% to about 5.0 wt.%, or from about 5.0 wt.% to about 10.0 wt.%, or from about 10.0 wt.% to about 15.0 wt.%, or from about 15.0 wt.% to about 19.99 wt.%, based on the total weight of the copolymer.

[0034] In another embodiment the dispersant (A) comprises a copolymer of: (i) more than 80 wt.% vinylcaprolactam, and (ii) less than 20 wt.% acrylic acid. Present disclosure further discloses the amount of vinylcaprolactam monomer in the copolymer of dispersant (A) ranges from about 80.01 wt.% to about 85.0 wt.%, or from about 85.0 wt.% to about 90.0 wt.%, or from about 90.0 wt.% to about 95.0 wt.%, or from about 95.0 wt.% to about 99.95 wt.% based on the total weight of the copolymer; the amount of acrylic acid monomer in the copolymer of dispersant (A) ranges from about 0.05 wt.% to about 5.0 wt.%, or from about 5.0 wt.% to about 10.0 wt.%, or from about 10.0 wt.% to about 15.0 wt.%, or from about 15.0 wt.% to about 19.99 wt.%, based on the total weight of the copolymer.

[0035] In another embodiment the dispersant (A) comprises a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, (ii) less than 10 wt.% vinylcaprolactam, and (iii) less than 20 wt.% acrylic acid. Present disclosure further discloses the amount of vinyl pyrrolidone monomer in the copolymer of dispersant (A) ranges from about 80.01 wt.% to about 85.0 wt.%, or from about 85.0 wt.% to about 90.0 wt.%, or from about 90.0 wt.% to about 95.0 wt.%, or from about 95.0 wt.% to about 99.95 wt.% based on the total weight of the copolymer; the amount of vinylcaprolactam monomer in the copolymer of the dispersant (A) ranges from about 0.01 wt.% to about 2.0 wt.%, or from about 2.0 wt.% to about 4.0 wt.%, or from about 4.0 wt.% to about 6.0 wt.%, or from about 6.0 wt.% to about 8 wt.%, or from about 8.0 wt.% to about 10.0 wt.%, based on the total weight of the copolymer; the amount of acrylic acid monomer in the copolymer of dispersant (A) ranges from about 0.01 wt.% to about 5.0 wt.%, or from about 5.0 wt.% to about 10.0 wt.%, or from about 10.0 wt.% to about 15.0 wt.%, or from about 15.0 wt.% to about 19.99 wt.%, based on the total weight of the copolymer.

[0036] In a non-limiting embodiment, the amount of dispersant (A) used in the dispersion of the present disclosure ranges from about 0.01 wt.% to about 2.0 wt.%, or from about 2.0 wt.% to about 4.0 wt.%, or from about 4.0 wt.% to about 6.0 wt.%, or from about 6.0 wt.% to about 8 wt.%, orfrom about 8.0 wt.% to about 10.0 wt.%, or from about 10.0 wt.% to about 12.0 wt.%, or from about 12.0 wt.% to about 14.0 wt.%, or from about 14.0 wt.% to about 16.0 wt.%, or from about 16.0 wt.% to about 18.0 wt.%, or from about 18.0 wt.% to about 20.0 wt.%.

[0037] In another non-limiting embodiment of the present disclosure, the weight average molecular weight of the dispersant (A) can range from about 3,000 Daltons to about 100,000 Daltons, or from about 100,000 Daltons to about 200,000 Daltons, or from about 200,000 Daltons to about 300,000 Daltons, wherein the weight average molecular weight of the dispersant (A) is measured using size-exclusion chromatography (SEC).

[0038] In another non-limiting embodiment of the present disclosure, the viscosity of the dispersion measured at a temperature of 25°C with Brookfield viscometer with spindle 63 or 64 at a rotational speed of 30 rpm can range from about 100 cPs to about 1,000 cPs, or from about 1,000 cPs to about 2,000 cPs, or from about 2,000 cPs to about 3,000 cPs, or from about 3,000 cPs to about 4,000 cPs, or from about 4,000 cPs to about 5,000 cPs, or from about 5,000 cPs to about 6,000 cPs, or from about 6,000 cPs to about 7,000 cPs, or from about 7,000 cPs to about 8,000 cPs, or from about 8,000 cPs to about 9,000 cPs, or from about 9,000 cPs to about 10,000 cPs.

[0039] In another specific embodiment of the present disclosure, the viscosity of the dispersion, measured at 25 °C using a Brookfield viscometer with spindle 63 or 64 at a rotational speed of 30 rpm, ranges from about 100 cPs to about 3,000 cPs, or about 100 cPs to about 2,000 cPs. In another specific embodiment, the viscosity of the dispersion ranges from about 100 cPs to about 1,500 cPs, or from about 100 cPs to about 1,000 cPs or from about 300 cPs to about 1,000 cPs.

[0040] Another non-limiting embodiment of the present disclosure provides a dispersant (A) comprising a copolymer of (i) more than 80 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20 wt.% of at least one functionalized or unfunctionalized monomer selected from acrylic acid, methacrylic acid, itaconic acid, maleic acid and maleic anhydride; wherein the copolymer is soluble in both N-methyl-2-pyrrolidone (NMP) and water but remains insoluble and stable in the electrolyte, which can help retain the copolymer on the electrode and reduce leaching, thereby contributing to improved battery stability and cycling life. As a result, the dispersed carbon materials can enhance battery performance by providing higher energy density, extended cycle life, and improved power efficiency.

[0041] In another specific embodiment of the present disclosure, the dispersant (A) comprises a copolymer of vinyl pyrrolidone and acrylic acid, wherein the copolymer comprises from about 85 wt.% to about 95 wt.% vinyl pyrrolidone and from about 5 wt.% to about 15 wt.% acrylic acid, and wherein the copolymer is soluble in both N-methyl-2-pyrrolidone (NMP) and water but remains insoluble and stable in the electrolyte, which can help retain the copolymer on the electrode and reduce leaching, thereby contributing to improved battery stability and cycling life. As a result, the dispersed carbon materials can enhance battery performance by providing higher energy density, extended cycle life, and improved power efficiency.

[0042] Non-limiting examples for carbon nanotubes that can be used in the present disclosure include multi-walled CNTs (MWCNTs), thin-walled CNTs, single-walled CNTs (SWCNTs), double-walled CNTs (DWCNTs), few-walled CNTs (FWCNTs), and combinations thereof.

[0043] In another specific embodiment, the carbon material (B) comprises carbon nanotubes (CNTs).

[0044] In another embodiment, examples of the carbon materials (B) further include graphene, and graphite-based composites, carbon fiber, natural graphite, artificial graphite, graphite fiber, expanded graphite, glassy carbon, or amorphous carbon, graphene oxide, reduced graphene oxide, mesoporous carbon, doped carbon structures and combinations thereof.

[0045] In a non-limiting embodiment, the amount of carbon materials (B) used in the dispersion of the present disclosure ranges from about 0.01 wt.% to about 2.0 wt.%, or from about 2.0 wt.% to about 4.0 wt.%, or from about 4.0 wt.% to about 6.0 wt.%, or from about 6.0 wt.% to about 8 wt.%, or from about 8.0 wt.% to about 10.0 wt.%, or from about 10.0 wt.% to about 12.0 wt.%, or from about 12.0 wt.% to about 14.0 wt.%, or from about 14.0 wt.% to about 16.0 wt.%, or from about 16.0 wt.% to about 18.0 wt.%, or from about 18.0 wt.% to about 20.0 wt.%, or from about 20.0 wt.% to about 22.0 wt.% , or from about 22.0 wt.% to about 24.0 wt.%, or from about 24.0 wt.% to about 26.0 wt.%, or from about 26.0 wt.% to about 28.0 wt.%, or from about 28.0 wt.% to about 30.0 wt.%.

[0046] Another embodiment of the present disclosure provides examples of solvent (C) include but are not limited to N-methyl-2-pyrrolidone, methyl ethyl ketone (MEK), alcohol-based solvents, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), amine-based solvents, methyl isobutyl ketone (MIBK), methoxy propyl acetate (PMA), n-butyl acetate and water.

[0047] In another embodiment, the solvent (C) comprises a mixed solvent system comprising two or more solvents selected from N-methyl-2-pyrrolidone (NMP), methyl ethyl ketone (MEK), tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), methyl isobutyl ketone (MIBK), methoxy propyl acetate (PMA), n-butyl acetate, water, and alcohol-based solvents.

[0048] In another specific embodiment, the solvent (C) comprises N-methyl-2-pyrrolidone (NMP) or a mixed solvent system comprising N-methyl-2-pyrrolidone (NMP) and water.

[0049] In another embodiment, the solvent (C) comprises an electrolyte solvent mixture of ethylene carbonate and ethyl methyl carbonate, wherein the weight ratio of ethylene carbonate to ethyl methyl carbonate ranges from about 1 :9 to about 9: 1, or from about 2:8 to about 8:2, or from about 3:7 to about 7:3.

[0050] In embodiments comprising a mixed solvent system, the relative amounts of the solvents are selected to dissolve the dispersant (A), facilitate dispersion of the carbon material (B), and provide a desired viscosity of the dispersion.

[0051] In a non-limiting embodiment, the amount of solvent (C) used in the dispersion of the present disclosure ranges from about 0.01 wt.% to about 5.0 wt.%, or from about 5.0 wt.% to about 10.0 wt.%, or from about 10.0 wt.% to about 15.0 wt.%, or from about 15.0 wt.% to about 20 wt.%, or from about 20.0 wt.% to about 25.0 wt.%, or from about 25.0 wt.% to about 30.0 wt.%, or from about 30.0 wt.% to about 35.0 wt.%, or from about 35.0 wt.% to about 40.0 wt.%, or from about 40.0 wt.% to about 45.0 wt.%, or from about 45.0 wt.% to about 50.0 wt.%, or from about 50.0 wt.% to about 55.0 wt.% , or from about 55.0 wt.% to about 60.0 wt.%, or from about 60.0 wt.% to about 65.0 wt.%, or from about 65.0 wt.% to about 70.0 wt.%, or from about 70.0 wt.% to about 75.0 wt.% or from about 75.0 wt.% to about 80.0 wt.%, or from about 80.0 wt.% to about 85.0 wt.%, or from about 85.0 wt.% to about 90.0 wt.%, or from about 90.0 wt.% to about 95.0 wt.%, or from about 95.0 wt.% to about 99.99 wt.%. In embodiments comprising a mixed solvent system, the amount of solvent (C) refers to the total combined amount of all solvents present in the dispersion.

[0052] In another embodiment, examples of the amine-based pH neutralizer (D) used in the dispersion of the present disclosure include, but are not limited to monoethanolamine, diethanolamine, triethanolamine, N-[3-(dimethylamino)propyl]-4-hydroxybutyramide (DMAPHB), and combinations thereof.

[0053] Examples of amine-based pH neutralizer (D) of the present disclosure further include reaction product of (a) at least one polyamine; and (b) at least one lactone or lactide. The reaction product can be obtained from the partial reaction of at least one polyamine with at least one lactone or lactide; and comprises a mono-substituted product having at least one primary, secondary, or tertiary amino group and a hydroxy group wherein:(i) a mono-substituted product represented by Formula I (a) or Formula I (b);wherein n is an independently selected integer from 1 to 20; L is a linking group independently selected from the group consisting of functionalized and unfunctionalized alkyl, cycloalkyl, alkenyl, and aryl groups; Ri, R2 and R3 are independently selected from the group consisting of hydrogen or carbon atoms having functionalized and unfunctionalized alkyl, cycloalkyl, alkenyl, and aryl groups; and R4 and Rs are independently selected from the group consisting of hydrogen, hydroxy, alkoxy groups or carbon atoms having functionalized and unfunctionalized alkyl, cycloalkyl, alkenyl, and aryl groups;(ii) a di-substituted product as represented by Formula (II), and an unreacted polyamine;Formula (II)wherein n is an independently selected integer from 1 to 20; L is a linking group independently selected from the group consisting of functionalized alkyl, cycloalkyl, alkenyl, and aryl groups, wherein any of the beforementioned groups are having at least one amino group; Ri and R3 are independently selected from the group consisting of hydrogen or carbon atoms havingfunctionalized and unfunctionalized alkyl, cycloalkyl, alkenyl, and aryl groups; and R.4 and Rs are independently selected from the group consisting of hydrogen, hydroxy, alkoxy groups or carbon atoms having functionalized and unfunctionalized alkyl, cycloalkyl, alkenyl, and aryl groups.

[0054] In some embodiments, suitable reaction products of (a) at least one polyamine; and (b) at least one lactone or lactide, and methods of making the same, are described in WO2025058958A1, which is incorporated herein by reference.

[0055] Other suitable examples of the pH neutralizer (D) that can be used in the present disclosure include, but are not limited to sodium hydroxide, triethanolamine, sodium diacetate, sodium acetate, sodium succinate, di sodium succinate, sodium citrate, sodium formate, ammonium salts, and combinations thereof; alkaline pH neutralizers include alkali metal hydroxides, such as sodium hydroxide, and potassium hydroxide; ammonium hydroxide; organic bases, such as triethanolamine, diisopropylamine, dodecylamine, diisopropanolamine, aminomethyl propanol, cocamine, oleamine, morpholine, triamylamine, triethylamine, tromethamine (2-amino-2-hydroxymethyl)-l,3-propanediol), and tetrakis (hydroxypropyl) ethylenediamine; and alkali metal salts of inorganic acids, such as sodium borate (borax), sodium phosphate, sodium pyrophosphate, and the like, and mixtures thereof; acidic pH neutralizers including organic acids, including amino acids, and inorganic mineral acids and combinations thereof; examples for suitable acidic pH neutralizers include, but are not limited to acetic acid, citric acid, fumaric acid, glutamic acid, glycolic acid, hydrochloric acid, lactic acid, nitric acid, phosphoric acid, sodium bisulfate, sulfuric acid, tartaric acid, and combinations thereof.

[0056] In a non-limiting embodiment, the amount of amine-based pH neutralizer (D) used in the dispersion of the present disclosure ranges from about 0.01 wt.% to about 2.0 wt.%, or from about 2.0 wt.% to about 4.0 wt.%, or from about 4.0 wt.% to about 6.0 wt.%, or from about 6.0 wt.% to about 8 wt.%, or from about 8.0 wt.% to about 10.0 wt.%, or from about 10.0 wt.% to about 12.0 wt.%, or from about 12.0 wt.% to about 14.0 wt.%, or from about 14.0 wt.% to about 16.0 wt.%, or from about 16.0 wt.% to about 18.0 wt.%, or from about 18.0 wt.% to about 20.0 wt.%.

[0057] Another non-limiting embodiment provides the use of dispersion of the present disclosure in lithium-ion batteries, sodium-ion batteries, graphite electrodes, silicon-based electrodes, conductive films, carbon coated current collectors, lead-acid batteries, lithium-sulfur batteries, lithium-air batteries, solid state batteries, super capacitors, sensors, transistors, medical devices,solar cells, and adhesive conductive layer coatings, wherein the conductive layer coatings, after drying, exhibit no-feathering and lower-cratering properties. Other exemplary uses include lithium iron phosphate electrodes, lithium manganese iron phosphate electrodes, lithium cobalt oxide electrodes, low manganese electrodes, lithium nickel manganese cobalt oxides electrodes, lithium nickel cobalt aluminum oxides electrodes, lithium titanite oxide electrodes, graphite electrodes, and silicon-based electrodes.

[0058] In a specific embodiment, the dispersion of the present disclosure is a carbon nanotube dispersion.

[0059] In another specific embodiment, the present disclosure provides a carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20 wt.% of acrylic acid; (B) carbon nanotubes; (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0060] In another embodiment the dispersant (A) of carbon nanotube dispersion of the present disclosure is a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, and (ii) less than 20 wt.% acrylic acid. Present disclosure further discloses the amount of vinyl pyrrolidone monomer in the copolymer of dispersant (A) ranges from about 80.01 wt.% to about 85.0 wt.%, or from about 85.0 wt.% to about 90.0 wt.%, or from about 90.0 wt.% to about 95.0 wt.%, or from about 95.0 wt.% to about 99.95 wt.% based on the total weight of the copolymer; the amount of acrylic acid monomer in the copolymer of dispersant (A) ranges from about 0.05 wt.% to about 5.0 wt.%, or from about 5.0 wt.% to about 10.0 wt.%, or from about 10.0 wt.% to about 15.0 wt.%, or from about 15.0 wt.% to about 19.99 wt.%, based on the total weight of the copolymer.

[0061] In another embodiment the dispersant (A) of carbon nanotube dispersion of the present disclosure is a copolymer of: (i) more than 80 wt.% vinylcaprolactam, and (ii) less than 20 wt.% acrylic acid. Present disclosure further discloses the amount of vinylcaprolactam monomer in the copolymer of dispersant (A) ranges from about 80.01 wt.% to about 85.0 wt.%, or from about 85.0 wt.% to about 90.0 wt.%, or from about 90.0 wt.% to about 95.0 wt.%, or from about 95.0 wt.% to about 99.95 wt.% based on the total weight of the copolymer; the amount of acrylic acid monomer in the copolymer of dispersant (A) ranges from about 0.05 wt.% to about 5.0 wt.%, orfrom about 5.0 wt.% to about 10.0 wt.%, or from about 10.0 wt.% to about 15.0 wt.%, or from about 15.0 wt.% to about 19.99 wt.%, based on the total weight of the copolymer.

[0062] In another embodiment the dispersant (A) of carbon nanotube dispersion of the present disclosure is a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, (ii) less than 10 wt.% vinylcaprolactam, and (iii) less than 20 wt.% acrylic acid. Present disclosure further discloses the amount of vinyl pyrrolidone monomer in the copolymer of dispersant (A) ranges from about 80.01 wt.% to about 85.0 wt.%, or from about 85.0 wt.% to about 90.0 wt.%, or from about 90.0 wt.% to about 95.0 wt.%, or from about 95.0 wt.% to about 99.95 wt.% based on the total weight of the copolymer; the amount of vinylcaprolactam monomer in the copolymer of the dispersant (A) ranges from about 0.01 wt.% to about 2.0 wt.%, or from about 2.0 wt.% to about 4.0 wt.%, or from about 4.0 wt.% to about 6.0 wt.%, or from about 6.0 wt.% to about 8 wt.%, or from about 8.0 wt.% to about 10.0 wt.%, based on the total weight of the copolymer; the amount of acrylic acid monomer in the copolymer of dispersant (A) ranges from about 0.01 wt.% to about 5.0 wt.%, or from about 5.0 wt.% to about 10.0 wt.%, or from about 10.0 wt.% to about 15.0 wt.%, or from about 15.0 wt.% to about 19.99 wt.%, based on the total weight of the copolymer.

[0063] In a non-limiting embodiment, the amount of dispersant (A) used in the carbon nanotube dispersion of the present disclosure ranges from about 0.01 wt.% to about 2.0 wt.%, or from about 2.0 wt.% to about 4.0 wt.%, or from about 4.0 wt.% to about 6.0 wt.%, or from about 6.0 wt.% to about 8 wt.%, or from about 8.0 wt.% to about 10.0 wt.%, or from about 10.0 wt.% to about 12.0 wt.%, or from about 12.0 wt.% to about 14.0 wt.%, or from about 14.0 wt.% to about 16.0 wt.%, or from about 16.0 wt.% to about 18.0 wt.%, or from about 18.0 wt.% to about 20.0 wt.%.

[0064] In another non-limiting embodiment of the present disclosure, the viscosity of the carbon nanotube dispersion measured at a temperature of 25°C with Brookfield viscometer with spindle 63 or 64 at a rotational speed of 30 rpm can range from about 100 cPs to about 1,000 cPs, or from about 1,000 cPs to about 2,000 cPs, or from about 2,000 cPs to about 3,000 cPs, or from about 3,000 cPs to about 4,000 cPs, or from about 4,000 cPs to about 5,000 cPs, or from about 5,000 cPs to about 6,000 cPs, or from about 6,000 cPs to about 7,000 cPs, or from about 7,000 cPs to about 8,000 cPs, or from about 8,000 cPs to about 9,000 cPs, or from about 9,000 cPs to about 10,000 cPs.

[0065] In another specific embodiment of the present disclosure, the viscosity of the carbon nanotube dispersion, measured at 25 °C using a Brookfield viscometer with spindle 63 or 64 at a rotational speed of 30 rpm, ranges from about 100 cPs to about 3,000 cPs, or about 100 cPs to about 2,000 cPs. In another specific embodiment, the viscosity of the dispersion ranges from about 100 cPs to about 1,500 cPs, or from about 100 cPs to about 1,000 cPs or from about 300 cPs to about 1,000 cPs.

[0066] Non-limiting examples for carbon nanotubes (B) that can be used in the carbon nanotube dispersion of the present disclosure include multi-walled CNTs (MWCNTs), thin-walled CNTs, single-walled CNTs (SWCNTs), double-walled CNTs (DWCNTs), few-walled CNTs (FWCNTs), and combinations thereof.

[0067] In another specific embodiment, the present disclosure provides a carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, and (ii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0068] In another specific embodiment, the present disclosure provides a carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinylcaprolactam, and (ii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0069] In another specific embodiment, the present disclosure provides a carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, (ii) less than 10 wt.% vinylcaprolactam, and (iii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0070] In another non-limiting embodiment, present disclosure discloses a method of preparing carbon nanotube dispersion, wherein the dispersion is prepared by mixing the carbon nanotubes (CNTs) (B) with the dispersant (A) of the present disclosure in solvent (C) and optionally, adding an amine-based pH neutralizer (D). The dispersion is prepared by mixing the components by employing one or more equipments including an ultrasonicator, a homogenator, a spiral mixer, a planetary mixer, a disperser, a blending mixer, and a ball miller.

[0071] In another embodiment, a method of preparing the dispersion comprises dissolving the dispersant (A) in N-methyl-2-pyrrolidone (NMP), adding carbon nanotubes (CNTs), mixing on a Vortexer and / or Thinky mixer, sonicating, and optionally homogenizing, with cooling as needed.

[0072] In another non-limiting embodiment, the present disclosure provides a method of preparing a carbon nanotube dispersion, wherein the method comprises: dissolving the dispersant (A) in a solvent (C); optionally neutralizing the dispersant (A) by addition of an amine-based pH neutralizer (D); adding carbon nanotubes (B) to the solution comprising the dispersant (A); and dispersing the carbon nanotubes (B) by one or more mixing and / or dispersion operations selected from vortex mixing, planetary mixing, sonication, and high-shear homogenization, optionally with cooling between operations, to provide the carbon nanotube dispersion.

[0073] In another embodiment, the carbon nanotube dispersion of the present disclosure is further characterized by a particle size (D50). Particle size distribution (PSD) of the dispersion is measured using a Horiba LA-950 laser-scattering particle size analyzer and is reported as D50 (pm). In further embodiments the D50 ranges from about 0.6 pm to greater than about 100 pm; or from about 0.6 pm to about 110 pm; or from about 0.6 pm to about 100 pm; or from about 0.6 pm to about 80 pm; or from about 0.6 pm to about 60 pm; or from about 0.6 pm to about 40 pm; or from about 0.6 pm to about 20 pm; or from about 0.6 pm to about 10 pm.

[0074] In another embodiment, the carbon nanotube dispersion of the present disclosure is further characterized by the resistivity of the dispersion. Resistivity of the dispersion is measured using a TMAX-BSR2300 and is reported in kfi. In further embodiments, resistivity ranges from about 1 kQ to about 260 kQ.

[0075] In another embodiment, a Lithium iron phosphate (LFP) cathode prepared using the carbon nanotube dispersion of the present disclosure exhibits reduced impedance and increased specific capacity compared to corresponding cathodes prepared without a dispersant or with polyvinylpyrrolidone (PVP K-30) as the dispersant, wherein the impedance is determined by electrochemical impedance measurements and the specific capacity is determined by chargedischarge testing.

[0076] In another embodiment, a lithium iron phosphate (LFP) cathode prepared using the carbon nanotube dispersion of the present disclosure exhibits a reduced impedance as comparedto corresponding cathodes prepared without a dispersant or with polyvinylpyrrolidone (PVP K-30) as the dispersant.

[0077] In another embodiment, a lithium iron phosphate (LFP) cathode prepared using the carbon nanotube dispersion of the present disclosure exhibits an increased specific capacity as compared to corresponding cathodes prepared without a dispersant or with polyvinylpyrrolidone (PVP K-30) as the dispersant.

[0078] Another non-limiting embodiment discloses the use of the carbon nanotube dispersion of the present disclosure in lithium-ion batteries, sodium-ion batteries, graphite electrodes, silicon-based electrodes, conductive films, carbon coated current collectors, lead-acid batteries, lithium¬ sulfur batteries, lithium-air batteries, solid state batteries, super capacitors, sensors, transistors, medical devices, solar cells, and adhesive conductive layer coatings.

[0079] In another specific embodiment, the carbon nanotube dispersion is used as an adhesive conductive layer coating on substrates including, but are not limited to aluminum foil, copper foil, and polyester film, wherein the coating exhibits no-feathering and lower-cratering properties.

[0080] In another non-limiting embodiment, examples of substrates suitable for use with the carbon nanotube dispersion include nickel foil, stainless steel foil, carbon paper, carbon cloth, graphite foil, polyimide film, polyethylene terephthalate (PET) film, metal-coated polymer films, and combinations thereof.

[0081] Other exemplary uses of the carbon nanotube dispersion of the present disclosure include, but are not limited to lithium iron phosphate electrodes, lithium manganese iron phosphate electrodes, lithium cobalt oxide electrodes, low manganese electrodes, lithium nickel manganese cobalt oxides electrodes, lithium nickel cobalt aluminum oxides electrodes, lithium titanite oxide electrodes, graphite electrodes, and silicon-based electrodes.

[0082] Present disclosure further discloses the carbon nanotube dispersion in the form of a suspension or a slurry, is used as a conductive agent in the electrode formulations for lithium-ion batteries, sodium-ion batteries, lead-acid batteries, lithium-sulfur batteries, lithium-air batteries, solid state batteries, carbon coated current collectors, graphite electrodes, and silicon-based electrodes.

[0083] The following examples illustrate the presently disclosed and / or claimed inventive concept(s), parts and percentages being by weight, unless otherwise indicated. Each example is provided by way of explanation of the presently disclosed and / or claimed inventive concept(s), not limitation of the presently disclosed and / or claimed inventive concept(s). In fact, it will be apparent to those skilled in the art that various modifications and variations can be made in the presently disclosed and / or claimed inventive concept(s) without departing from the scope or spirit of the invention. For instance, features illustrated or described as part of one embodiment, can be used on another embodiment to yield a still further embodiment. Thus, it is intended that the presently disclosed and / or claimed inventive concept(s) covers such modifications and variations as come within the scope of the appended claims and their equivalents.EXAMPLES

[0084] Example 1: Copolymerizing vinylpyrrolidone and acrylic acid (VP / AA 75:25 w / w)

[0085] A 1-L reactor with anchor agitator was placed under nitrogen atmosphere. Heptane (415.55 g) was charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, the reactor vent was closed, and a pressure of 2-5 psig of nitrogen was maintained throughout the reaction. The heptane was heated to 65 °C, and 0.18 g of Zc / 7-butyl peroxypivalate (Lupersol-11) and 0.42 g of 2,5-bis( / ez7-butylperoxy)-2,5-dimethylhexane (Lupersol-101) were added. N- Vinylpyrrolidone (62.3 g) and 20.8 g of acrylic acid were added continuously by pump over 4 hours. After completion of the addition of monomers, the reaction was held at 65 °C for 1 hour and then heated to 125 °C. 2,5-Bis(tez7-butylperoxy)-2,5-dimethylhexane (0.42 g) was added, and the reaction was held at 125-130 °C for 8 hours, during which the internal pressure rose to 40-50 psig. A third shot of 2,5-bis(tez7-butylperoxy)-2,5-dimethylhexane (0.42 g) was added, and the reaction was held at 125-130 °C for another 8 hours. The reaction mixture was cooled to 50 °C, and the slurry was stripped of heptane by filtration or rotary evaporation. The resulting solid was dried under vacuum at 80 °C overnight. By SEC, the polymer had Mw205,057 and Mn28,329. By13C NMR, the polymer comprised 76.6 weight % VP and 23.4 weight % AA.

[0086] Example 2: Copolymerizing vinylpyrrolidone and acrylic acid (VP / AA 25:75 w / w)

[0087] A 1-L reactor with anchor agitator was placed under nitrogen atmosphere. Heptane (328.30 g) was charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, the reactor vent was closed, and a pressure of 2-5 psig of nitrogen was maintained throughout the reaction. The heptane was heated to 65 °C, and 0.14 g of / c / 7-butyl peroxypivalate and 0.33 g of 2,5-bis( / e / 7-butylperoxy)-2,5-dimethylhexane were added. A- Vinylpyrrolidone (18.05 g) and 54.16 g of acrylic acid were added continuously by pump over 4 hours. After completion of the addition of monomers, the reaction was held at 65 °C for 1 hour and then heated to 115 °C. Three 0.33-g portions of 2, 5 -bi s( / c / 7-butylperoxy)-2, 5 -dimethylhexane were added at t = 0, 2 and 4 hours, during which the internal pressure rose to 40-50 psig. After the third portion of 2, 5 -bi s(tert-butylperoxy)-2, 5 -dimethylhexane, the mixture was held at 115 °C for two hours. The reaction mixture was cooled to 50 °C, and the slurry was stripped of heptane by filtration or rotary evaporation. The resulting solid was dried under vacuum at 80 °C overnight. By SEC, the polymer had Mw48,244 and Mn 14,957. By13C NMR, the polymer comprised 39.0 weight % VP and 61.0 weight % AA.

[0088] Example 3: Copolymerizing vinyl caprolactam and acrylic acid (VCL / AA 75:25 w / w)

[0089] A 1-L reactor with anchor agitator was placed under nitrogen atmosphere. Heptane (357.60 g) was charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, the reactor vent was closed, and a pressure of 2-5 psig of nitrogen was maintained throughout the reaction. The heptane was heated to 65 °C, and 0.20 g of tert-butyl peroxypivalate was added. Two monomers, a solution of 60.0 g of A'-vinylcaprolactam in 60.0 g of heptane and 20.0 g of acrylic acid, were added separately and continuously by pump over 4 hours. After completion of the addition of monomers, the reaction was held at 65 °C for 1 hour and then heated to 90 °C. Four 0.55-g portions of tert-amyl 2-ethylperoxyhexanoate (Trigonox 121) were added at t = 0, 1, 2 and 3 hours. After the fourth portion of tert-amyl 2-ethylperoxyhexanoate, the mixture was held at 90 °C for two hours. The reaction mixture was cooled to 50 °C, and the slurry was stripped of heptane by filtration or rotary evaporation. The resulting solid was dried under vacuum at 80 °C overnight. By SEC, the polymer had Mw67,454 and Mn13,861. By13C NMR, the polymer comprised 82.3 weight % VCL and 17.7 weight % AA.

[0090] Example 4: Copolymerizing vinyl caprolactam and acrylic acid (VCL / AA 50:50 w / w)

[0091] A 1-L reactor with anchor agitator was placed under nitrogen atmosphere. Heptane (340.83 g) was charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, the reactor vent was closed, and a pressure of 2-5 psig of nitrogen was maintained throughout the reaction. The heptane was heated to 65 °C, and 0.18 g of Zc / 7-butyl peroxypivalate was added. Two monomers, a solution of 36.0 g of A- vinyl caprolactam in 36.0 g of heptane and 36.0 g of acrylic acid, were added separately and continuously by pump over 4 hours. After completing the addition of monomers, the reaction was held at 65 °C for 1 hour and then heated to 90 °C. Zc / 7-Amyl 2-ethylperoxyhexanoate (0.50 g) was added, and the mixture was held at 90 °C for 2 hours. A second 0.50 g of ZcrZ-amyl 2-ethylperoxyhexanoate was added, and the mixture was held at 90 °C for two hours. The reaction mixture was cooled to 50 °C, and the slurry was stripped of heptane by filtration or rotary evaporation. The resulting solid was dried under vacuum at 80 °C overnight. By SEC, the polymer had Mw46,444 and Mn 14,047. By13C NMR, the polymer comprised 63.2 weight % VCL and 36.8 weight % AA.

[0092] Example 5: Copolymerizing vinyl caprolactam and acrylic acid (VCL / AA 25:75 w / w)

[0093] A 1-L reactor with anchor agitator was placed under nitrogen atmosphere. Heptane (358.92 g) was charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, the reactor vent was closed, and a pressure of 2-5 psig of nitrogen was maintained throughout the reaction. The heptane was heated to 65 °C, and 0.09 g of te / -butyl peroxypivalate was added. Two monomers, a solution of 18.0 g of / V-vinylcaprolactam in 18.0 g of heptane and 54.0 g of acrylic acid, were added separately and continuously by pump over 4 hours. After completing the addition of monomers, the reaction was held at 65 °C for 1 hour and then heated to 90 °C. tert- Amyl 2-ethylperoxyhexanoate (0.50 g) was added, and the mixture was held at 90 °C for 2 hours. A second 0.50 g of Zc / 7-amyl 2-ethylperoxyhexanoate was added, and the mixture was held at 90 °C for two hours. The reaction mixture was cooled to 50 °C, and the slurry was stripped of heptane by filtration or rotary evaporation. The resulting solid was dried under vacuum at 80 °C overnight. By SEC, the polymer had Mw46,444 and Mn 14,047. By13C NMR, the polymer comprised 25.0 weight % VCL and 75.0 weight % AA.

[0094] Example 6: Copolymerizing vinylpyrrolidone and acrylic acid (VP / AA 90:10 w / w) in NMP

[0095] A 2-L reactor with anchor agitator was placed under nitrogen atmosphere. N-Methylpyrrolidone (NMP) (1128.87 g) was charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, a 1 scfh flow of nitrogen was maintained over the surface of the reaction, the NMP was heated to 65 °C, and 1.96 g of / c' / 7-butyl peroxypivalate and 4.42 g of 2,5-bis( / cr / -butylperoxy)-2,5-dimethylhexane were added. V- Vinylpyrrolidone (791.93 g) and a solution of 87.99 g of acrylic acid in 175.98 g of NMP were added simultaneously and continuously over 2 hours and 4 hours, respectively. After completion of the addition of monomers, the reaction was held at 65 °C for 1 hour and then heated to 130 °C. 2,5-Bis( / c / 7-butylperoxy)-2,5-dimethylhexane (4.42 g) was added, and the reaction was held at 125-130 °C for 2 hours. A third shot of 4.42 g of 2, 5 -bi s( / c77-butylperoxy)-2, 5 -dimethylhexane was added, and the reaction was held at 125-130 °C for 16 hours. The reaction mixture was cooled to 50 °C, neutralized with 165 g of triethanolamine, and discharged from the reactor. By SEC, the polymer had Mw23,965 and Mn7,440. By13C NMR, the polymer comprised 87.3 weight % VP and 12.7 weight % AA.

[0096] Example 7: Method of preparing terpolymer of vinylpyrrolidone, vinyl caprolactam and acrylic acid (VP / VCL / AA 85:5:10 w / w / w) in NMP

[0097] A 2-L reactor with anchor agitator was placed under nitrogen atmosphere. NMP (1128.87 g) was charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, a 1 scfh flow of nitrogen was maintained over the surface of the reaction, the NMP was heated to 65 °C, and 1.96 g of te / 7-butyl peroxypivalate and 4.42 g of 2,5-bis(terz-butylperoxy)-2,5-dimethylhexane were added. A mixture of 747.93 g of A-vinylpyrrolidone and 44.00 g of N-vinylcaprolactam was added continuously over 2 hours, and a solution of 87.99 g of acrylic acid in 175.98 g of NMP was added continuously over 4 hours. After completion of the addition of monomers, the reaction was held at 65 °C for 1 hour and then heated to 130 °C. 2,5-Bis( / c 7-butylperoxy)-2,5-dimethylhexane (4.42 g) was added, and the reaction was held at 125-130 °C for 2 hours. A third shot of 4.42 g of 2, 5 -bi s( / c77-buty I peroxy )-2, 5 -dimethylhexane was added, and the reaction was held at 125-130 °C for 16 hours. The reaction mixture was cooled to 50 °C, neutralized with 166.0 g of triethanolamine, and discharged from the reactor. By SEC, the polymerhad Mw28,605 and Mn 9,267. By13C NMR, the polymer comprised 81.7 weight % VP, 4.4 weight % VCL and 13.9 weight % AA.

[0098] Example 8: Copolymerizing vinylpyrrolidone and acrylic acid (VP / AA 85 / 15 w / w)

[0099] A 1-L reactor with anchor agitator was placed under nitrogen atmosphere. Heptane (390.65 g) was charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, the reactor vent was closed, and a pressure of 2-5 psig of nitrogen was maintained throughout the reaction. The heptane was heated to 65 °C, and 0.18 g of Ze / 7-butyl peroxypivalate and 0.42 g of 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane were added. A- Vinyl pyrrolidone (70.6 g) and a solution of 12.5 g of acrylic acid in 24.9 g of heptane were added continuously by pump over 4 hours. After completion of the addition of monomers, the reaction was held at 65 °C for 1 hour and then heated to 125 °C. 2,5-Bis(ter / -butylperoxy)-2,5-dimethylhexane (0.42 g) was added, and the reaction was held at 125-130 °C for 8 hours, during which the internal pressure rose to 40-50 psig. A third shot of 2,5-bis(ter / -butylperoxy)-2,5-dimethylhexane (0.42 g) was added, and the reaction was held at 125-130 °C for another 8 hours. The reaction mixture was cooled to 50 °C, and the slurry was stripped of heptane by fdtration or rotary evaporation. The resulting solid was dried under vacuum at 80 °C overnight. By SEC, the polymer had Mw 246,244 and Mn30,377. By13C NMR, the polymer comprised 85.0 weight % VP and 15.0 weight % AA.

[0100] Example 9: Copolymerizing vinylpyrrolidone and acrylic acid (VP / AA 90 / 10 w / w)

[0101] A 1-L reactor with anchor agitator was placed under nitrogen atmosphere. Heptane (398.95 g) was charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, the reactor vent was closed, and a pressure of 2-5 psig of nitrogen was maintained throughout the reaction. The heptane was heated to 65 °C, and 0.18 g of tert-butyl peroxypivalate and 0.42 g of 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane were added. A- Vinylpyrrolidone (74.7 g) and a solution of 8.3 g of acrylic acid in 16.6 g of heptane were added continuously by pump over 4 hours. After completion of the addition of monomers, the reaction was held at 65 °C for 1 hour and then heated to 125 °C. 2,5-Bis(terAbutylperoxy)-2,5-dimethylhexane (0.42 g) was added, and the reaction was held at 125-130 °C for 8 hours, during which the internal pressure rose to 40-50 psig. A third shot of 2,5-bis(ter / -butylperoxy)-2,5-dimethylhexane (0.42 g) was added, and the reaction was held at 125-130 °C for another 8 hours. The reaction mixture was cooled to 50 °C, and the slurry was stripped of heptane by fdtration or rotary evaporation. The resulting solid wasdried under vacuum at 80 °C overnight. By SEC, the polymer had Mw196,495 and Mn26,347. By13C NMR, the polymer comprised 91.0 weight % VP and 9.0 weight % AA.

[0102] Example 10: Copolymerizing vinylpyrrolidone and acrylic acid (VP / AA 90 / 10 w / w)

[0103] A 1-L reactor with anchor agitator was placed under nitrogen atmosphere. Heptane (517.3 g) was charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, the reactor vent was closed, and a pressure of 2-5 psig of nitrogen was maintained throughout the reaction. The heptane was heated to 85 °C, and 1.92 g of / c / 7-butyl peroxypivalate was added. A-Vinylpyrrolidone (96.9 g) and a solution of 10.76 g of acrylic acid in 21.5 g of heptane were added continuously by pump over 4 hours. After completion of the addition of monomers, the reaction was held at 85 °C for 1 hour. The reaction mixture was cooled to 50 °C, and the slurry was stripped of heptane by filtration or rotary evaporation. The resulting solid was dried under vacuum at 80 °C overnight. By SEC, the polymer had Mw95,628 and Mn 6,773. By13C NMR, the polymer comprised 90.5 weight % VP and 9.5 weight % AA.

[0104] Example 11: Copolymerizing vinylpyrrolidone and acrylic acid (VP / AA 95 / 5 w / w)

[0105] A 1-L reactor with anchor agitator was placed under nitrogen atmosphere. Heptane (511.90 g) was charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, the reactor vent was closed, and a pressure of 2-5 psig of nitrogen was maintained throughout the reaction. The heptane was heated to 85 °C, and 1.92 g of / c / 7-butyl peroxypivalate was added. A- Vinylpyrrolidone (102.26 g) and a solution of 5.38 g of acrylic acid in 26.9 g of heptane were added continuously by pump over 4 hours. After completion of the addition of monomers, the reaction was held at 85 °C for 1 hour. The reaction mixture was cooled to 50 °C, and the slurry was stripped of heptane by filtration or rotary evaporation. The resulting solid was dried under vacuum at 80 °C overnight. By SEC, the polymer had Mw 104,574 and Mn 7,401. By13C NMR, the polymer comprised 94.0 weight % VP and 6.0 weight % AA.

[0106] Example 12: Method of preparing terpolymer of vinylpyrrolidone, vinyl caprolactam and acrylic acid (VP / VCL / AA 85:5:10 w / w / w) in NMP

[0107] A 1-L reactor with anchor agitator was placed under nitrogen atmosphere. NMP (308 g) was charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, a 1 scfh flow of nitrogen was maintained over the surface of the reaction, the NMP was heated to65 °C, and 0.53 g of / c / 'Z-butyl peroxypivalate and 1.21 g of 2,5-bis( / er / -butylperoxy)-2,5-dimethylhexane were added. A mixture of 203.98 g of / V-vinylpyrrolidone and 12.00 g of N-vinylcaprolactam was added continuously over 2 hours, and a solution of 24.00 g of acrylic acid in 48.00 g of NMP was added continuously over 4 hours. After completion of the addition of monomers, the reaction was held at 65 °C for 1 hour and then heated to 130 °C. 2,5-Bis(tez7-butylperoxy)-2,5-dimethylhexane (1.21 g) was added, and the reaction was held at 125-130 °C for 8 hours. A third shot of 2,5-bis( / c / 7-butylperoxy)-2,5-dimethylhexane (1.21 g) was added, and the reaction was held at 125-130 °C for another 8 hours. The reaction mixture was cooled to 50 °C, neutralized with 49.68 g of triethanolamine, and discharged from the reactor. By SEC, the polymer had Mw10,570 and Mn2,640. By13C NMR, the polymer comprised 77.2 weight % VP, 5.2 weight % VCL and 17.6 weight % AA.

[0108] Example 13: Method of preparing terpolymer of vinylpyrrolidone, Sipomer® BEM, and acrylic acid (VP / Sipomer® BEM / AA 85:5:10 w / w / w) in NMP

[0109] A 1 -L reactor with anchor agitator was placed under nitrogen atmosphere. NMP (287 g) and 8.75 g of Sipomer® BEM (49-53% ethoxylated behenyl methacrylate, 22-24% methacrylic acid, 25-27% water) were charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, a 1 scfh flow of nitrogen was maintained over the surface of the reaction, the NMP was heated to 85 °C, and 0.39 g of ZerZ-butyl peroxypivalate and 0.88 g of 2,5-bis( / ez7-butylperoxy)-2,5-dimethylhexane were added. N- Vinylpyrrolidone (148.74 g) and a solution of 17.50 g of acrylic acid in 35.00 g of NMP were added separately and continuously over 4 hours. After completion of the addition of monomers, the reaction was held at 85 °C for 1 hour and then heated to 130 °C. 2,5-Bis(tert-butylperoxy)-2,5-dimethylhexane (0.88 g) was added, and the reaction was held at 125-130 °C for 8 hours. A third shot of 0.88 g of 2,5-bis( / er / -butylperoxy)-2,5-dimethylhexane was added, and the reaction was held at 125-130 °C for another 8 hours. The reaction mixture was cooled to 50 °C and discharged from the reactor. By SEC, the polymer had Mw 10,320 and Mn2,721.

[0110] Example 14: Copolymerizing vinylpyrrolidone and acrylic acid (VP / AA 90 / 10 w / w)

[0111] A 1-L reactor with anchor agitator was placed under nitrogen atmosphere. Heptane (395.01 g) and 3.29 g of isopropanol were charged to the reactor and then sparged with nitrogen for 30 minutes at 5 scfh. After sparging, the reactor vent was closed, and a pressure of 2-5 psig ofnitrogen was maintained throughout the reaction. The solvent was heated to 85 °C, and 1.83 g of / c' / 'Z-butyl peroxypivalate and 0.41 g of 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane were added. N- Vinylpyrrolidone (73.98 g) and a solution of 8.22 g of acrylic acid in 16.44 g of heptane were added separately and continuously by pump over 4 hours. After completion of the addition of monomers, the reaction was held at 85 °C for 1 hour and then heated to 130 °C. 2,5-Bis(te / 7-butylperoxy)-2,5-dimethylhexane (0.41 g) was added, and the reaction was held at 125-130 °C for 2 hours, during which the internal pressure rose to 40-50 psig. Another shot of 0.41 g of 2,5-bis( / / 7-butylperoxy)-2,5-di methyl hexane was added, and the reaction was held at 125-130 °C for another 7 hours. The reaction mixture was cooled to 50 °C, and the slurry was stripped of solvent by filtration or rotary evaporation. The resulting solid was dried under vacuum at 80 °C overnight. By SEC, the polymer had Mw38,487 and Mn3,881. By13C NMR, the polymer comprised 92.6 weight % VP and 7.4 weight % AA.

[0112] Example 15: Method of preparing a solvent-based CNT slurry (1%)

[0113] Each dispersant of Example 1-14 (0.5 weight %) was fully dissolved in NMP at a temperature of 5-35 °C, mixing at a speed of 200-1000 rpm for about 1-4 hours, until no undissolved particle was observed by eye. Carbon nanotubes (Cnano, 0.5 weight %) were added to the container containing the NMP solution, and the container was closed. The dispersion was mixed on a Vortexer for two 30-second periods or on a Thinky mixer for 5 minutes at 2000 rpm. The container was placed in a sonicating bath for 15 minutes and then on an ultrasonic mixer for 5-10 minutes, cycling on for 5 seconds and then off for 10 seconds. The container was removed from the mixer and cooled.

[0114] Example 16: Method of preparing a solvent-based CNT slurry (1%)

[0115] Each dispersant of Example 1-14 (0.75 weight %) was fully dissolved in NMP at a temperature of 5-35 °C, mixing at a speed of 200-1000 rpm for about 1-4 hours, until no undissolved particle was observed by eye. In some cases, the dispersant was neutralized by addition of triethanolamine (TEA); see Table 1. Carbon nanotubes (Cnano, 0.25 weight %) were added to the container containing the NMP solution, and the container was closed. The dispersion was mixed on a Vortexer for two 30-second periods or on a Thinky mixer for 5 minutes at 2000 rpm. The container was placed in a sonicating bath for 15 minutes and then on an ultrasonic mixerfor 5-10 minutes, cycling on for 5 seconds and then off for 10 seconds. The container was removed from the mixer and cooled.

[0116] Example 17: Method of preparing a solvent-based CNT slurry (4%)

[0117] Each dispersant of Example 1-14 (2 weight %) was fully dissolved in NMP at a temperature of 5-35 °C, mixing at a speed of 200-1000 rpm for about 1-4 hours, until no undissolved particle was observed by eye. In some cases, the dispersant was neutralized by addition of monoethanolamine (MEA), triethanolamine (TEA) or A-[3-(dimethylamino)propyl]-4-hydroxybutyramide (DMAPHB); see Table 1. Carbon nanotubes (Cnano, 2 weight %) were added to the container containing the NMP solution, and the container was closed. The dispersion was mixed on a Vortexer for two 30-second periods or on a Thinky mixer for 5 minutes at 2000 rpm. The container was placed in a sonicating bath for 15 minutes and then in a water bath to cool down. The container was then run on a homogenizer mixer at 5,000-10,000 rpm for 1-4 hours, removed, and cooled.

[0118] Example 18: Physical properties of CNT dispersions

[0119] The viscosity, particle size (D50, pm) and resistivity of CNT dispersions in NMP using the dispersants of the disclosure (Examples 1-14) were measured. Additionally, comparative examples using commercially available dispersants, PVP K-30 (Ashland), Ultrathix™ P-100 (Ashland), Ganex™ P904 LC (Ashland), BYK-LP® N 24711 (BYK), Soluryl® S-820 (Hanwha), and hydrogenated nitrile butadiene rubber (HNBR) were also characterized. Viscosity was measured using a Brookfield viscometer LV (USA), spindle 63 or 64 at 25 °C and 30 rpm. Particle size distribution (PSD) of CNT dispersions was measured using a Horiba LA-950 laser-scattering particle size analyzer. Resistivity of CNT dispersions was measured using a TMAX-BSR2300. Measurement results are tabulated in Table 1.Table 1. Physical Properties of CNT Dispersions3aAll CNT dispersions were made in Micropure™ NMP according to Example 15, 16 or 17. "Amines: MEA, monoethanolamine, TEA, triethanolamine; DMAPHB, V-[3- (dimethylamino)propyl]-4-hydroxybutyramide. "Comparative dispersant example.

[0120] In general, the dispersant copolymers with greater than 80 weight % of N-vinylpyrrolidone and V-vinylcaprolactam, combined, and less than 20 weight % of acrylic acid give CNT dispersions having low viscosity, small particle size (D50), and high dispersion, as evidenced by high resistivity.

[0121] Example 19: Method of preparing a solvent-based slurry of carbon nanotubes (CNTs) and Lithium nickel manganese oxide (NMC)

[0122] To 12.625 g of an 8 weight % solution of PVDF (polyvinylidene fluoride, Solef® 5130 (Solvay)) in NMP was added 20.167 g of a 4 weight % dispersion of CNTs (CHASM) in NMP. The slurry was mixed on a Thinky mixer at 2000 rpm for 5 minutes. Lithium nickel manganese oxide (NMC, Gelon , 58 g) was then added and hand mixed, and the slurry was mixed on a Thinky mixer at 2000 rpm for 5 minutes. About 5 g of extra NMP was added to achieve the desired solids content. The slurry was mixed again on a Thinky mixer at 2000 rpm for 5 minutes. The slurry was then transferred to a planetary mixer for a final 2-4 hours at 600 rpm.

[0123] Example 20: Physical properties of CNT and NMC dispersions

[0124] The physical properties of the dispersions made in Example 19 were measured according to the method described in Example 18. Additionally, comparative examples using commercially available dispersants, PVP K-30 (Ashland) and hydrogenated nitrile butadiene rubber (HNBR), were also characterized. The results are tabulated in Table 2.Table 2. Physical Properties of CNT / NMC Dispersions11"All CNT / NMC dispersions were made in Micropure™ NMP according to Example 19.6Amines: TEA, triethanolamine.cComparative dispersant example.

[0125] Example 21: Solubility of dispersant copolymers

[0126] The solubility of dispersant polymers was determined in NMP and in the electrolyte used for lithium-ion battery (LIB) manufacturing. PVP K-30 was soluble in both NMP and the LIB electrolyte, poly(acrylic acid) (PAA) was soluble in neither NMP nor the LIB electrolyte. The dispersant of Example 9 (VP-AA 90:10) was soluble in NMP but insoluble in the LIB electrolyte.

[0127] These results show that the dispersant of Example 9 is soluble in NMP but insoluble in the lithium-ion battery electrolyte. This solubility profde can facilitate processing and can help retain the dispersant on the electrode, thereby reducing leaching and contributing to improved battery stability and cycling life.

[0128] Example 22: Cathode Preparation

[0129] A cathode was prepared for coating and testing using lithium iron phosphate LiFePO4 (LFP). A CNT dispersion was used as the conductive agent, PVDF was used as the binder, and NMP was used as the solvent. The cathode was prepared by coating the above slurry on an aluminum foil current collector to form a cathode and heating the cathode at 110 °C in a conventional oven overnight.

[0130] Example 23: Electrochemical Tests

[0131] Coin half-cells having a 20 mm diameter and a 3.2 mm height (CR-2032) were made using the cathodes prepared in Example 22 in combination with lithium metal counter electrodes, a polyolefin separator and an electrolyte of 1 M LiPFe in a mixture of ethylene carbonate and ethyl methyl carbonate (EC:EMC 3:7). The coin half-cells were tested to determine impedance and the rate capability at various rates. Table 3 lists the cathode half-cells prepared with conductive dispersion.Table 3. Cathodes Prepared According to Example 22

[0132] Example 24: Impedance Test

[0133] Impedance of the CR-2032 half-cells prepared in Example 23 from samples of blank, polyacrylic acid (PAA), Cl and C19 were tested for impedance. The battery impedance data was measured using a Solartron® 1260 from Solartron Analytical (Leicester, UK). The results shown in FIG. 1 indicate that the LFP cathode prepared with a CNT dispersion using C19 has lower impedance than those prepared without a dispersant (blank) or with Cl (PVP K-30) as the dispersant.

[0134] Example 25: Rate Capability Test

[0135] The rate capabilities of the CR-2032 half-cells prepared in Example 23 from samples of blank, polyacrylic acid (PAA), Cl and C19 were evaluated in a voltage window of 2.0 V to 4.2 V, for a range by charging and discharging the cells using CC / CC mode at a rate of 0.05C, 0.1C, 0.2C,0.5C, 1 C, 2C, 5C or 10C. The results shown in FIG. 2 indicate that the LFP cathode prepared with dispersant C19 has a higher specific capacity than those prepared without a dispersant (blank) or with Cl (PVP K-30) as the dispersant.

[0136] Example 26: Evaluation of Feathering and Cratering

[0137] FIG. 3 demonstrates the no-feathering and lower-cratering properties of the adhesive conductive layer coating tested using the dispersion of the present disclosure on substrates including aluminum foil, copper foil, and polyester film.

[0138] In accordance with the foregoing description, the invention can be further illustrated by the following non-limiting enumerated embodiments:

[0139] Embodiment AA: A dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80.0 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20.0 wt.% of at least one functionalized or unfunctionalized monomer selected from acrylic acid, methacrylic acid, itaconic acid, maleic acid and maleic anhydride; (B) at least one carbon material; (C) at least one solvent; and (D) optionally, at least one amine-based pH neutralizer.

[0140] Embodiment AB: The dispersion according to Embodiment AA, wherein the dispersant (A) is a copolymer of: (i) more than 80.0 wt.% vinyl pyrrolidone, and (ii) less than 20.0 wt.% acrylic acid.

[0141] Embodiment AC: The dispersion according to Embodiment AA, wherein the dispersant (A) is a copolymer of: (i) more than 80.0 wt.% vinylcaprolactam, and (ii) less than 20.0 wt.% acrylic acid.

[0142] Embodiment AD: The dispersion according to Embodiment AA, wherein the dispersant (A) is a copolymer of: (i) more than 80.0 wt.% vinyl pyrrolidone, (ii) less than 10.0 wt.% vinylcaprolactam, and (iii) less than 20.0 wt.% acrylic acid.

[0143] Embodiment AE: The dispersion according to Embodiment AA, wherein the amount of dispersant (A) ranges from about 0.01 wt. % to about 20.0 wt. %.

[0144] Embodiment AF: The dispersion according to Embodiment AA, wherein the carbon material (B) is selected from the group consisting of carbon nanotubes (CNTs), carbon nanofibers,short nanotubes, carbon particles, carbon black, acetylene black, ketjen black, graphene, graphite, and combinations thereof.

[0145] Embodiment AG: The dispersion according to Embodiment AA, wherein the amount of carbon material (B) ranges from about 0.01 wt. % to about 30.0 wt. %.

[0146] Embodiment AH: The dispersion according to Embodiment AA, wherein the solvent (C) is selected from the group consisting of N-methyl-2-pyrrolidone, methyl ethyl ketone (MEK), alcohol-based solvents, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), amine-based solvents, methyl isobutyl ketone (MIBK), methoxy propyl acetate (PMA), n-butyl acetate and water.

[0147] Embodiment Al: The dispersion according to Embodiment AA, wherein the amount of solvent (C) ranges from about 0.01 wt. % to about 99.99 wt. %.

[0148] Embodiment AJ: The dispersion according to Embodiment AA, wherein the amine-based pH neutralizer (D) is selected from the group consisting of monoethanolamine, diethanolamine, triethanolamine, A-[3-(dimethylamino)propyl]-4-hydroxybutyramide (DMAPHB), and combinations thereof.

[0149] Embodiment AK: The dispersion according to Embodiment AA, wherein the amount of amine-based pH neutralizer (D) ranges from about 0.01 wt. % to about 20.0 wt. %.

[0150] Embodiment AL: The dispersion according to Embodiment AA, wherein the dispersion is used in lithium-ion batteries, sodium-ion batteries, graphite electrodes, silicon-based electrodes, conductive films, carbon coated current collectors, lead-acid batteries, lithium-sulfur batteries, lithium-air batteries, solid state batteries, super capacitors, sensors, transistors, medical devices, solar cells, and adhesive conductive layer coatings.

[0151] Embodiment AM: The dispersion according to Embodiment AL, wherein the dispersion is used in adhesive conductive layer coatings wherein the adhesive conductive layer coatings, after drying, exhibit no-feathering and lower-cratering properties.

[0152] Embodiment AN: A carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20 wt.% of acrylic acid; (B) carbon nanotubes; (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0153] Embodiment AO: The carbon nanotube dispersion according to Embodiment AN, wherein the dispersant (A) is a copolymer of: (a) (i) more than 80.0 wt.% vinyl pyrrolidone, and (ii) less than 20.0 wt.% acrylic acid; (b) (i) more than 80.0 wt.% vinylcaprolactam, and (ii) less than 20.0 wt.% acrylic acid; or (c) (i) more than 80.0 wt.% vinyl pyrrolidone, (ii) less than 10.0 wt.% vinylcaprolactam, and (iii) less than 20.0 wt.% acrylic acid.

[0154] Embodiment AP: A carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, and (ii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0155] Embodiment AQ: A carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinylcaprolactam, and (ii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0156] Embodiment AR: A carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, (ii) less than 10 wt.% vinylcaprolactam, and (iii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0157] Embodiment AS: A dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80.0 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20.0 wt.% of at least one functionalized or unfunctionalized monomer selected from acrylic acid, methacrylic acid, itaconic acid, maleic acid and maleic anhydride; (B) at least one carbon material; (C) at least one solvent; and (D) optionally, at least one amine-based pH neutralizer.

[0158] Embodiment AT: The dispersion according to Embodiment AS, wherein the dispersant (A) is a copolymer of: (i) more than 80.0 wt.% vinyl pyrrolidone, and (ii) less than 20.0 wt.% acrylic acid.

[0159] Embodiment AU: The dispersion according to Embodiment AS, wherein the dispersant (A) is a copolymer of: (i) more than 80.0 wt.% vinylcaprolactam, and (ii) less than 20.0 wt.% acrylic acid.

[0160] Embodiment AV: The dispersion according to Embodiment AS, wherein the dispersant (A) is a copolymer of: (i) more than 80.0 wt.% vinyl pyrrolidone, (ii) less than 10.0 wt.% vinylcaprolactam, and (iii) less than 20.0 wt.% acrylic acid.

[0161] Embodiment AW: The dispersion according to Embodiment AS, wherein the carbon material (B) is selected from the group consisting of carbon nanotubes (CNTs), carbon nanofibers, short nanotubes, carbon particles, carbon black, acetylene black, ketjen black, graphene, graphite, and combinations thereof.

[0162] Embodiment AX: The dispersion according to Embodiment AS, wherein the solvent (C) is selected from the group consisting of N-methyl-2-pyrrolidone, methyl ethyl ketone (MEK), alcohol-based solvents, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), amine-based solvents, methyl isobutyl ketone (MIBK), methoxy propyl acetate (PMA), n-butyl acetate and water.

[0163] Embodiment AY: The dispersion according to Embodiment AS, wherein the amine-based pH neutralizer (D) is selected from the group consisting of monoethanolamine, diethanolamine, triethanolamine, V-[3-(dimethylamino)propyl]-4-hydroxybutyramide (DMAPHB), and combinations thereof.

[0164] Embodiment AZ: The dispersion according to Embodiment AS, wherein: (i) the amount of dispersant (A) ranges from about 0.01 wt. % to about 20.0 wt. %; (ii) the amount of carbon material (B) ranges from about 0.01 wt. % to about 30.0 wt. %; (iii) the amount of solvent (C) ranges from about 0.01 wt. % to about 99.99 wt. %; and (iv) optionally, the amount of amine-based pH neutralizer (D) ranges from about 0.01 wt. % to about 20.0 wt. %.

[0165] Embodiment BA: The dispersion according to Embodiment AS, wherein the dispersion is used in lithium-ion batteries, sodium-ion batteries, graphite electrodes, silicon-based electrodes, conductive fdms, carbon coated current collectors, lead-acid batteries, lithium-sulfur batteries, lithium-air batteries, solid state batteries, super capacitors, sensors, transistors, medical devices, solar cells, and adhesive conductive layer coatings.

[0166] Embodiment BB: The dispersion according to Embodiment BA, wherein the dispersion is used in adhesive conductive layer coatings wherein the adhesive conductive layer coatings, after drying, exhibit no-feathering and lower-cratering properties.

[0167] Embodiment BC: A carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20 wt.% of acrylic acid; (B) carbon nanotubes; (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0168] Embodiment BD: The carbon nanotube dispersion according to Embodiment BC, wherein the dispersant (A) is a copolymer of: (a) (i) more than 80.0 wt.% vinyl pyrrolidone, and (ii) less than 20.0 wt.% acrylic acid; (b) (i) more than 80.0 wt.% vinylcaprolactam, and (ii) less than 20.0 wt.% acrylic acid; or (c) (i) more than 80.0 wt.% vinyl pyrrolidone, (ii) less than 10.0 wt.% vinylcaprolactam, and (iii) less than 20.0 wt.% acrylic acid.

[0169] Embodiment BE: A carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, and (ii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0170] Embodiment BF: A carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinylcaprolactam, and (ii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0171] Embodiment BG: A carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, (ii) less than 10 wt.% vinylcaprolactam, and (iii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

[0172] While the compositions and methods of the disclosed and / or claimed inventive concept(s) have been described in terms of particular aspects, it will be apparent to those of ordinary skill in the art that variations may be applied to the compositions and / or methods and in the steps or in the sequence of steps of the method described herein without departing from the concept, spirit and scope of the disclosed and / or claimed inventive concept(s). All such similar substitutes and modifications apparent to those skilled in the art are deemed to be within the spirit, scope and concept of the disclosed and / or claimed inventive concept(s).

Claims

What is Claimed is:

1. A dispersion comprising:(A) a dispersant comprising a copolymer of:(i) more than 80.0 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and(ii) less than 20.0 wt.% of at least one functionalized or unfunctionalized monomer selected from acrylic acid, methacrylic acid, itaconic acid, maleic acid and maleic anhydride;(B) at least one carbon material;(C) at least one solvent; and(D) optionally, at least one amine-based pH neutralizer.

2. The dispersion according to claim 1, wherein the dispersant (A) is a copolymer of: (i) more than 80.0 wt.% vinyl pyrrolidone, and (ii) less than 20.0 wt.% acrylic acid.

3. The dispersion according to claim 1, wherein the dispersant (A) is a copolymer of: (i) more than 80.0 wt.% vinylcaprolactam, and (ii) less than 20.0 wt.% acrylic acid.

4. The dispersion according to claim 1, wherein the dispersant (A) is a copolymer of: (i) more than 80.0 wt.% vinyl pyrrolidone, (ii) less than 10.0 wt.% vinylcaprolactam, and (iii) less than 20.0 wt.% acrylic acid.

5. The dispersion according to claim 1, wherein the amount of dispersant (A) ranges from about 0.01 wt. % to about 20.0 wt. %.

6. The dispersion according to claim 1, wherein the carbon material (B) is selected from the group consisting of carbon nanotubes (CNTs), carbon nanofibers, short nanotubes, carbon particles, carbon black, acetylene black, ketjen black, graphene, graphite, and combinations thereof.

7. The dispersion according to claim 1, wherein the amount of carbon material (B) ranges from about 0.01 wt. % to about 30.0 wt. %.

8. The dispersion according to claim 1, wherein the solvent (C) is selected from the group consisting of N-methyl-2-pyrrolidone, methyl ethyl ketone (MEK), alcohol-based solvents, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), amine-based solvents, methyl isobutyl ketone (MIBK), methoxy propyl acetate (PMA), n-butyl acetate and water.

9. The dispersion according to claim 1 , wherein the amount of solvent (C) ranges from about 0.01 wt. % to about 99.99 wt. %.

10. The dispersion according to claim 1, wherein the amine-based pH neutralizer (D) is selected from the group consisting of monoethanolamine, diethanolamine, triethanolamine, N-[3-(dimethylamino)propyl]-4-hydroxybutyramide (DMAPHB).

11. The dispersion according to claim 1, wherein the amount of amine-based pH neutralizer (D) ranges from about 0.01 wt. % to about 20.0 wt. %.

12. The dispersion according to claim 1, wherein the dispersion is used in lithium-ion batteries, sodium-ion batteries, graphite electrodes, silicon-based electrodes, conductive films, carbon coated current collectors, lead-acid batteries, lithium-sulfur batteries, lithium-air batteries, solid state batteries, super capacitors, sensors, transistors, medical devices, solar cells, and adhesive conductive layer coatings.

13. The dispersion according to claim 12, wherein the dispersion is used in adhesive conductive layer coatings wherein the adhesive conductive layer coatings, after drying, exhibit nofeathering and lower-cratering properties.

14. A carbon nanotube dispersion comprising:(A) a dispersant comprising a copolymer of: (i) more than 80 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20 wt.% of acrylic acid;(B) carbon nanotubes;(C) N-methyl-2-pyrrolidone (NMP) solvent; and(D) optionally, an amine-based pH neutralizer.

15. The carbon nanotube dispersion according to claim 14, wherein the dispersant (A) is a copolymer of:(a) (i) more than 80.0 wt.% vinyl pyrrolidone, and (ii) less than 20.0 wt.% acrylic acid; (b) (i) more than 80.0 wt.% vinylcaprolactam, and (ii) less than 20.0 wt.% acrylic acid; or (c) (i) more than 80.0 wt.% vinyl pyrrolidone, (ii) less than 10.0 wt.% vinylcaprolactam, and (iii) less than 20.0 wt.% acrylic acid.

16. A carbon nanotube dispersion comprising:(A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, and (ii) less than 20 wt.% acrylic acid;(B) carbon nanotubes (CNTs);(C) N-methyl-2-pyrrolidone (NMP) solvent; and(D) optionally, an amine-based pH neutralizer.

17. A carbon nanotube dispersion comprising:(A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinylcaprolactam, and (ii) less than 20 wt.% acrylic acid;(B) carbon nanotubes (CNTs);(C) N-methyl-2-pyrrolidone (NMP) solvent; and(D) optionally, an amine-based pH neutralizer.

18. A carbon nanotube dispersion comprising:(A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, (ii) less than 10 wt.% vinylcaprolactam, and (iii) less than 20 wt.% acrylic acid;(B) carbon nanotubes (CNTs);(C) N-methyl-2-pyrrolidone (NMP) solvent; and(D) optionally, an amine-based pH neutralizer.

19. A dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80.0 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20.0 wt.% of at least one functionalized or unfunctionalized monomer selected from acrylic acid, methacrylic acid, itaconic acid, maleic acid and maleic anhydride; (B) at least one carbon material; (C) at least one solvent; and (D) optionally, at least one amine-based pH neutralizer.

20. The dispersion according to claim 19, wherein the dispersant (A) is a copolymer of: (i) more than 80.0 wt.% vinyl pyrrolidone, and (ii) less than 20.0 wt.% acrylic acid.

21. The dispersion according to claim 19, wherein the dispersant (A) is a copolymer of: (i) more than 80.0 wt.% vinylcaprolactam, and (ii) less than 20.0 wt.% acrylic acid.

22. The dispersion according to claim 19, wherein the dispersant (A) is a copolymer of: (i) more than 80.0 wt.% vinyl pyrrolidone, (ii) less than 10.0 wt.% vinylcaprolactam, and (iii) less than 20.0 wt.% acrylic acid.

23. The dispersion according to claim 19, wherein the carbon material (B) is selected from the group consisting of carbon nanotubes (CNTs), carbon nanofibers, short nanotubes, carbon particles, carbon black, acetylene black, ketjen black, graphene, graphite, and combinations thereof.

24. The dispersion according to claim 19, wherein the solvent (C) is selected from the group consisting of N-methyl-2-pyrrolidone, methyl ethyl ketone (MEK), alcohol-based solvents, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), amine-based solvents, methyl isobutyl ketone (MIBK), methoxy propyl acetate (PMA), n-butyl acetate and water.

25. The dispersion according to claim 19, wherein the amine-based pH neutralizer (D) is selected from the group consisting of monoethanolamine, diethanolamine, triethanolamine, N-[3-(dimethylamino)propyl]-4-hydroxybutyramide (DMAPHB), and combinations thereof.

26. The dispersion according to claim 19, wherein: (i) the amount of dispersant (A) ranges from about 0.01 wt. % to about 20.0 wt. %; (ii) the amount of carbon material (B) ranges from about 0.01 wt. % to about 30.0 wt. %; (iii) the amount of solvent (C) ranges from about 0.01 wt. % to about 99.99 wt. %; and (iv) optionally, the amount of amine-based pH neutralizer (D) ranges from about 0.01 wt. % to about 20.0 wt. %.

27. The dispersion according to claim 19, wherein the dispersion is used in lithium-ion batteries, sodium-ion batteries, graphite electrodes, silicon-based electrodes, conductive films, carbon coated current collectors, lead-acid batteries, lithium-sulfur batteries, lithium-air batteries, solid state batteries, super capacitors, sensors, transistors, medical devices, solar cells, and adhesive conductive layer coatings.

28. The dispersion according to claim 27, wherein the dispersion is used in adhesive conductive layer coatings wherein the adhesive conductive layer coatings, after drying, exhibit nofeathering and lower-cratering properties.

29. A carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% of vinyl pyrrolidone, vinylcaprolactam, or combinations thereof; and (ii) less than 20 wt.% of acrylic acid; (B) carbon nanotubes; (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

30. The carbon nanotube dispersion according to claim 29, wherein the dispersant (A) is a copolymer of:(a) (i) more than 80.0 wt.% vinyl pyrrolidone, and (ii) less than 20.0 wt.% acrylic acid; (b) (i) more than 80.0 wt.% vinylcaprolactam, and (ii) less than 20.0 wt.% acrylic acid; or (c) (i) more than 80.0 wt.% vinyl pyrrolidone, (ii) less than 10.0 wt.% vinylcaprolactam, and (iii) less than 20.0 wt.% acrylic acid.

31. A carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, and (ii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

32. A carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinylcaprolactam, and (ii) less than 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.

33. A carbon nanotube dispersion comprising: (A) a dispersant comprising a copolymer of: (i) more than 80 wt.% vinyl pyrrolidone, (ii) less than 10 wt.% vinylcaprolactam, and (iii) lessthan 20 wt.% acrylic acid; (B) carbon nanotubes (CNTs); (C) N-methyl-2-pyrrolidone (NMP) solvent; and (D) optionally, an amine-based pH neutralizer.