Oxidation and corrosion resistant coatings for turbine components
TiAlTaSiN coatings with tailored atomic compositions address oxidation and hot corrosion in turbine components, forming a dense oxide layer for improved durability and resistance.
Patent Information
- Application Number
- PCT/EP2026/053176
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-14
- Filing Date
- 2026-02-06
- Publication Date
- 2026-11-19
AI Technical Summary
Turbine components made of Ti or Ni-based alloys face challenges from oxidation and hot corrosion, particularly at elevated temperatures, with existing coatings lacking sufficient thermal stability and erosion resistance.
Application of TiAlTaSiN coatings with specific atomic compositions (TiaAlbTacSidN, where 0.30 ≤ b ≤ 0.50, 0.05 ≤ c ≤ 0.20, and 0.005 ≤ d ≤ 0.05) to enhance oxidation and hot corrosion resistance while maintaining mechanical properties.
The TiAlTaSiN coatings provide improved resistance to oxidation and hot corrosion, forming a dense protective oxide layer that minimizes cracking and pores, and exhibit enhanced mechanical properties like hardness and erosion resistance.
Smart Images

Figure EP2026053176_19112026_PF_FP_ABST
Abstract
Description
Oxidation and corrosion resistant coatings for turbine components
[0001] The present invention relates to the use of coatings to improve oxidation resistance and corrosion resistance of functional substrates, in particular components of turbines.
[0002] Turbines for aerospace comprise a multitude of components, from inlet over different pressure sections to outlet. The temperature and operating conditions are different depending on where in the turbine the components are located. At elevated operating temperatures, in particular from 500 °C to 900 °C or higher, oxidation and corrosion preset challenges for the components. Alloys based on Ti or Ni, such as alloys of the type of Ti-6Al-4V or super-alloys of the type Inconel 718 or C263 are commonly used to achieve high temperature resistance. However, Ti or Ni based alloys are often susceptible to oxidation and molten salt-induced corrosion, also known as hot corrosion. Elements like Al and Cr are often kept at reduced levels in superalloys to achieve high temperature strength and microstructural stability. This has the effect that native oxides like Al2O3and Cr2O3, are formed only to low extent or not at all, and are therefore insufficient for protection of components.
[0003] Oxidation is a challenge for components with prolonged exposure to elevated operating temperatures in an oxygen containing atmosphere. The prolonged exposure may also constitute repeated sequences at elevated temperature, where each exposure lasts for one hour or more. Total exposure times at elevated temperatures for components in use may be several hundred hours, for example 200-300 hours, 500 hours, or even longer.
[0004] Hot corrosion in turbines is a challenge when salt-rich aerosols, for example from marine environments, enter the turbine through the air intake. Salt-rich aerosols typically include NaCl, KCl, and / or MgCl2. The salt-rich aerosols react with oxygen and sulphur-compounds present from impurities in the fuel to form high-melting sulfate salts, e.g. Na2SO4, MgSO4, which build up on turbine components in hot sections of the turbine. Hot corrosion refers to corrosion mechanisms occurring between salt deposits and the material of the underlying surface. Hot corrosion encompasses the subtypes low temperature hot-corrosion (LTHC), where the salt adheres in a solid form, typically in the temperature range 575 ºC – 800 ºC, and high temperature hot-corrosion (HTHC), where the salt adheres in molten form, typically in the temperature range 800 ºC – 950 ºC.
[0005] Use of coatings to protect turbine components against oxidation and hot corrosion is well known. Approaches in prior-art include coatings applied with thermal spray technologies and PVD (Physical Vapor Deposition) technologies. However, known solutions face drawbacks such as limiting thermal stability of the coating itself, or reduced performance on other metrics like erosion resistance. To further enhance performance of turbine components, solutions are therefore required that can enhance protection against oxidation and hot corrosion while maintaining thermal stability and erosion resistance.Objective of the Invention
[0006] The objective of the invention is to provide a solution that can help to protect turbine components against oxidation and hot corrosion. Improved protection should contribute to increased useful lifetime of the turbine components.Description of the Invention
[0007] The above-mentioned objective is attained by using TiAlTaSiN coatings with adjusted composition of Ta and Si.
[0008] The inventors observed that if TiAlTaSiN coatings are used on turbine engine components, the resistance of the components against oxidation and hot corrosion can be vastly improved. Improvements were seen compared to components in uncoated conditions as well as compared to components coated with other coatings like TiAlN.
[0009] According to the present invention, the TiAlTaSiN coating may have composition in atomic concentration is given by the formula (TiaAlbTacSid)N with
[0010] a+b+c+d = 1,
[0011] 0.30 ≤ b ≤ 0.50,
[0012] 0.05 ≤ c ≤ 0.20, and
[0013] 0.005 ≤ d ≤ 0.05.
[0014] The composition is stated as atomic percentage on the metal sublattice, i.e. considering Ti, Al, Ta, and Si atoms.
[0015] The amount of Ta is as such in the range from 5 at% to 20 at%. Further preferred is the range from 10 at% to 16 at% Ta.
[0016] The amount of Si is as such in the range from 0.5 at% to 5 at%. Further preferred is the range from 2 at% to 3 at% Si.
[0017] In a most preferred embodiment, the amount of Ta is in the range from 10 at% to 16 at and the Si content is in the range from 2 at% to 3 at%. The most preferred embodiment thus has a composition with 0.30 ≤ b ≤ 0.50, 0.10 ≤ c ≤ 0.16, and 0.02 ≤ d ≤ 0.03.
[0018] The inventors have observed that TiAlTaSiN coatings with adjusted Ta and Si content are particularly effective for protection against oxidation and hot corrosion. TiAlTaSiN coatings may therefore be advantageous used as oxidation resistant layer and as hot corrosion resistant layer on turbine components.
[0019] The Ta- and Si-content of the TiAlTaSiN coating should preferably be kept below 20 at%, as a too high concentration of Ta and Si promotes formation of hexagonal phases in the coatings. It is desired to avoid substantial fractions of hexagonal phases in order to avoid negative effects on mechanical properties, like lower hardness.
[0020] The combination of Ta and Si in the TiAlTaSiN coating is particularly advantageous as the incorporation of Ta provides for improvement of mechanical properties like hardness and Young’s modulus, while Si provides for grain refinement. The combination of Ta and Si furthermore provides a synergistic effect as coatings of single fcc cubic phase can be synthesized with Ta content above 8 at%. A transition to formation of hexagonal phases is expected when the sum of the content of Ta and Si exceed the range of approximately 15-20 %, where the transition point is also influenced by the Al-content of the coating.
[0021] The combination of Ta and Si in the TiAlTaSiN coatings furthermore provides a synergistic effect on the oxidation kinetics. The inventors found that TiAlTaSiN coatings display a much slower oxide layer growth compared to TiAlN, TiAlTaN and TiAlSiN coatings. The slower oxide layer growth is to a large extent dependent on that Ta and Si influences the formation of oxide phases in that the rutile-TiO2phase is stabilized when TiAlTaSiN coatings are oxidized, which is very beneficial for forming a dense and compact protective oxide layer on the surface of the coating.
[0022] The advantages are particularly clear in a comparison with TiAlN according to prior art, i.e. TiAlN without Ta and Si as alloying elements. Oxidation of TiAlN results in a first step in the formation of the metastable anatase-TiO2phase. In a second step, after further oxidation and / or heating, the anatase-TiO2phase transforms to the thermodynamically stable rutile-TiO2phase. The density of anatase-TiO2and rutile-TiO2are different, which leads to a volume change of the coating, which may cause the formation of cracks and pores within the coating. This is an undesirable effect since cracks may lead to deterioration of coating properties and / or delamination of coating from the substrate. In TiAlTaSiN coatings, a large fraction of the oxides is instantly formed in the rutile-TiO2phase and the phase transformation from anatase-TiO2to rutile-TiO2is therefore largely avoided. The formation of cracks and pores is therefore minimized or completely avoided. Consequently, a dense and protective oxide layer is formed on TiAlTaSiN, which provides for improved oxidation resistance.
[0023] During oxidation, TiAlTaSiN coatings advantageously form an oxide scale comprising two layers. The TiAlTaSiN coating is thereby covered by two oxide layers. The first oxide layer closest to the TiAlTaSiN coating comprises Ti, Al, Ta, Si, and O. The crystallographic phase structure of the first oxide layer comprises rutile-TiO2. In addition, the presence of Si and Ta in the first oxide layer (r-TiO2) deaccelerates the oxidation kinetics, as it supports a densification. The presence of Si and Ta in the rutile-TiO2phase have been found particularly advantageous. The second oxide layer follows on top of the first oxide layer and is an oxide of Al, i.e. essentially comprises the elements Al and O. The crystallographic phase structure of the second oxide layer consists of hexagonal Al2O3phase.
[0024] Turbine components in scope of the present invention may be made of superalloys, in particular nickel-based superalloys (Ni-based superalloys), iron-nickel based superalloys (Fe-Ni-based superalloys) and / or cobalt-based superalloys (Co-based superalloys). The material of which the turbine components are made is also referred to as substrate, substrate material, and material of the substrate. Ni-based superalloys are in particular understood to include solid-solution strengthened alloys and age-hardenable alloys, where the age hardenable alloys typically comprise an austenistic (fcc) matrix dispersed with coherent precipitation of an Ni3(Al,Ti) intermetallic with an fcc structure. An example of Ni-based superalloys is Inconel 718.
[0025] Fe-Ni-based superalloys are in particular understood as superalloys with Fe as main element. The Fe-Ni-based superalloys include alloys with an fcc matrix strengthened by precipitation of intermetallic compounds.
[0026] Co-based superalloys are in particular understood as superalloys with Co as main element. Typically, Co-based superalloys display an austenitic fcc matrix within which small quantities of carbides are distributed.
[0027] Turbine components in scope of the invention may also be made of titanium alloys, such as titanium-aluminides like Ti-6Al-4V. Titanium alloys typically have lower temperature stability compared to superalloys, but may be a cost-effective solution in parts of the turbine that do not experience very high temperatures.
[0028] Turbine components in scope of the invention include compressor blades, vanes and blisks, also known as integrated blade rotors (IBR). These components operate in hot sections of the turbine and are often susceptible to oxidation and hot corrosion.
[0029] The inventors propose the use of TiAlTaSiN coatings on turbine components where oxidation and / or hot corrosion are major failure mechanisms, in particular use of TiAlTaSiN coatings on compressor blades, vanes and blisks. It is noted that turbine components may often be exposed to a combination of oxidation and hot corrosion; oxidation due to the exposure to high temperatures in presence of oxygen and hot corrosion additionally at parts of the components where salt deposits have formed. TiAlTaSiN coatings are therefore very useful as protective coatings against oxidation and hot corrosion.
[0030] The inventors further note that turbine components susceptible to oxidation and hot corrosion are often as well exposed to solid particle erosion due to sand particles or debris which may be present in the air going through the turbine. The solid particle erosion resistance of the proposed TiAlTaSiN coatings have therefore been tested and a good level of solid particle resistance can be confirmed. TiAlTaSiN coatings according to the invention therefore provides the advantageous combination of high oxidation resistance, high hot corrosion resistance and good solid particle resistance.Examples
[0031] The invention will now be described based on exemplary embodiments. The exemplary embodiments are intended for better understanding of the invention and do not limit the scope of the invention.
[0032] Coatings according to the invention with four different compositions were performed on an industrial scale Oerlikon Balzers INNOVA 1.0 system using 6” powder metallurgically produced targets. A reference coating of TiAlN was additionally deposited. All coatings were grown on IN718, Nimonic C-263 and sapphire ( -oriented substrates. IN718 and Nimonic C-263 are substrate materials corresponding to materials of turbine components. Sapphire ( -oriented substrates were included to facilitate analytical investigation of the grown coatings. All substrates which were ultrasonically pre-cleaned in Ethanol and Acetone for 5 minutes each, before mounting them onto the sample holder. Before the coating step, a central-beam plasma etching step in pure Argon was performed for 30 minutes. The TiAlTaSiN films were deposited in a reactive N2atmosphere with a constant pressure of 3.2 Pa at 450 °C and a substrate bias of -40 V. An arc current 200 A was chosen for all six sources. The coatings according to Examples 3 & 4 were deposited using APO confinement ring configuration, and parameters adjusted to operate the arc source at stronger and weaker magnetic fields.
[0033] Microstructure and morphology as well as the coating thickness were assessed by means of a Zeiss Sigma 500 VP scanning electron microscope (SEM) with an acceleration voltage of 5 kV. Therefore, fracture cross-sections were prepared by breaking sapphire substrates in half. Cross-sectional fracture images are presented inand 4.
[0034] The elemental composition of the thin films was analyzed using a combination of energy-dispersive X-ray spectroscopy (EDX) with a EDAX Octane detector mounted in the above-named SEM instrument, calibrated with thin film standards. Additionally, the results were cross-referenced using elastic recoil detection analysis (ERDA) and X-ray photoelectron spectroscopy (XPS). The elemental composition of the coatings are displayed in Table 1.
[0035] Total composition(at.%)Composition on metal sublattice (at.%)SampleNTiAlTaSiTi(a)Al(b)Ta(c)Si(d)Example 151.923.717.16.11.249.335.612.72.5Example 251.819.4216.71.140.243.613.92.3Example 351.619.2208.11.239.641.216.72.5Example 453.019.0215.91.140.444.712.62.3Reference TiAlN47.129.122.756.243.8
[0036] Structural analysis was conducted utilizing X-ray diffraction (XRD) analysis, employing a Panalytical X'Pert MPDII diffractometer in Bragg-Brentano geometry equipped with a Cu-Kαradiation source (λ=1.5418 Å). All XRD measurements were conducted at angles ranging from 15° to 130° and the obtained diffractograms were subsequently analysed using the HighScore software package.
[0037] Hardness and Young's modulus were measured on IN718 substrates using a FemtoTools FT- I04 nanoindentation system equipped with a Berkovich diamond tip in continuous stiffness measurement (CSM) mode. For each sample, 36 displacement-controlled indents were performed, with a maximum depth of 10% of the coating thickness to minimize substrate effects. The load-displacement curves were analyzed using the Oliver-Pharr method to determine hardness and Young's modulus. A Poisson ratio of ν = 0.25 was assumed for TiAlTaSiN systems, and E = 1050 GPa and ν = 0.07 were used for the Berkovich tip. The Young’s modulus was plotted against indentation depth and extrapolated to zero using a power-law fit to exclude substrate influence. An area function was applied to correct for non-ideal tip geometry, with measurements taken on fused silica (E = 72.5 GPa, H = 10 GPa) as a reference. Hardness and Young's modulus of the inventive examples are presented in Table 2.
[0038] Residual stress measurements (in-plane) were undertaken using the sin²(ψ)-method. Therefore, XRD was performed in Bragg-Brentano configuration on a PANalytical Empyrean system, utilizing Cu-Kα radiation (λ=1.5418 Å). Using the above named Highscore software dhkl(ψ) could be extracted from the diffractograms after peak fitting. To calculate the residual stresses, diffraction elastic constants, and , for the (220) diffraction peak of cubic Ti0.5Al0.5N were used (inverse Kröner model via IsoDEC). Residual stress of the inventive examples is presented in Table 2.
[0039] SampleHardness[GPa]Young’s Modulus[GPa]Residual stress[GPa]Surface Roughness, Ra[µm]Example 132.7 ± 1.2339 ± 13-3.810.21 ± 0.06Example 229.4 ± 0.8370 ± 16-3.530.15 ± 0.01Example 333.4 ± 2.6447 ± 56 / / Example 426.3 ± 2.2332 ± 44 / / Reference TiAlN29.2 ± 1.6427 ± 12Oxidation in ambient air
[0040] To evaluate oxidation performance under conditions comparable to oxidative environments in turbines, oxidation experiments were performed for over timescales extending from 24 hours up to 500 hours. The coatings according to the invention deposited on superalloy substrates of IN718 were tested alongside a comparative TiAlN coating (Reference TiAlN) according to prior art and the results were compared.
[0041] The longterm oxidation experiments on coatings deposited on IN718 substrates were performed in a conventional furnace at 850 °C for 24 h, 48 h, 168 h and 500 h. Post-oxidation analysis was performed by XRD (with measurement details as described above), focused ion beam (FIB) and transmission electron microscopy (TEM). To obtain information about the oxide scale thickness FIB windows were prepared using a ThermoFisher Scios 2 instrument, operating at 30 kV and a current of 15 nA. For the TEM analysis a TECNAI F20 TEM system operating at 200 kV was employed to gain a detailed understanding of the constitution of the coating and the oxide layer (microstructure and morphology). Additionally, all samples were subjected to selected area electron diffraction (SAED) analysis and electron energy loss spectroscopy (EELS).
[0042] The oxidation scale thickness as function of oxidation time is presented inThe comparative TiAlN coating (Reference) displays a rapidly growing oxide scale thickness, which reaches more than 1900 nm after 24 hours. Between 24 and 48 hours, the comparative TiAlN coating completely failed and spalled off the substrate. Determination of the oxide thickness of the comparative TiAlN coating from 48 hours is therefore neither possible nor relevant. In comparison, the coatings according to the invention (Example 1-4) show oxide scales of 250 – 500 nm after 24 hours. Furthermore, coatings according to the invention display slow growth rates after the initial 24 hours. After 500 hours, the oxide scales of the inventive coatings ranged from 500 to 1100 nm. In particular, the coating according to Example 4 showed excellent results with the lowest oxide scale thickness.
[0043] Detailed evaluation of the oxide scale of the coating according to Example 2 is presented inTwo oxide layers have formed on the TiAlTaSiN coating during the oxidation experiment. Oxide layer 1 is highlighted in Figure 7b and characterized by SAED in the positions marked with d and e. The corresponding SAED patterns are shown in Figure 7e and 7d, respectively. The SAED pattern in Figure 7e shows rutile-TiO2and anatase-TiO2phases towards the bottom (closer to the unaffected TiAlTaSiN coating) of oxide layer 1. The SAED pattern in Figure 7d shows a mixture of rutile-TiO2, anatase-TiO2and hexagonal-Al2O3phases towards the top (closer to oxide layer 2) of oxide layer 1. Oxide layer 2 is highlighted in Figure 7c and characterized by SAED in the positions marked with f. The corresponding SAED pattern is shown in Figure 7f. The SAED pattern in Figure 7f. shows pure hexagonal-Al2O3phase in oxide layer 2. Figure 7j shows an EELS line scan through the cross-section of the oxide scale of Example 2, starting from the unaffected coating (distance 0 µm) and passing through oxide layer 1 and oxide layer 2 with increasing distance on the horizontal axis. From the EELS scan, it is evident that in oxide layer 1 not only Ti and Al are present but also Ta and Si, which is mainly contributing to a stabilization of the rutile-TiO2phase, which is found very beneficial for the oxidation resistance. In oxide layer 2, only Al and O is detected by EELS, which confirms the SAED analysis of a pure hexagonal Al2O3phase.
[0044] Example 2 thus illustrates the advantageous benefits of the inventive coatings for oxidation resistance. A comparison with TiAlN, without Ta and Si as alloying elements, further illustrates the advantages. If pure TiAlN is oxidized, then first the metastable anatase-TiO2phase is formed, which upon further oxidation transforms to the thermodynamically stable rutile-TiO2phase. The phase transformation from anatase-TiO2to rutile-TiO2leads to a volume change, which can cause formation of cracks and pores. Cracks may lead to deterioration of coating properties and / or delamination of coating from the substrate, which may be an explanation for the failure of the comparative TiAlN coating as described above. With the presence of Ta and Si, i.e. in TiAlTaSiN coatings, a large fraction of the oxides is instantly formed in the rutile-TiO2phase. The phase transformation from anatase-TiO2to rutile-TiO2is therefore largely avoided. The formation of cracks and pores is therefore minimized or completely avoided. Consequently, a dense and protective oxide layer is formed on TiAlTaSiN, which provides for improved oxidation resistance.Hot corrosion
[0045] To evaluate hot corrosion protection performance under conditions comparable to corrosive environments in turbines, hot gas corrosion testing were performed. The coatings according to the invention deposited on superalloy substrates of C263 were tested. An uncoated superalloy substrate was included as reference. The results of the inventive coatings were compared with uncoated substrate material as reference.
[0046] The hot gas corrosion experiment was performed in a gas mixture with a total flow of 2500 sccm was chosen, comprised of 2118 sccm Ar, 375 sccm O2, and 7.5 sccm SO2. For each coating composition (coating example) a control-arrangement consisting of one sample were no salt was added and one sample prepared with a salt-coupon was tested. The salt coupons consisted of a mixture of anhydrous MgSO4and Na2SO4(Merck KGaA) with a molar ratio of 20:80(=mass ratio of 15.21:84.78).
[0047] In order to test different concentrations of SO2, the flow of Ar was varied between different experimental runs. At the conditions of the highest Ar-flow (2118 sccm), the 7.5 sccm SO2corresponds to 0.3 % of SO2of the total gas flow. To increase the SO2concentration, the Ar content was reduced. Under conditions with a flow of 368 sccm Ar, the SO2concentration corresponded to 1% of the total gas flow. Under conditions with a flow of 118 sccm Ar, the SO2concentration corresponded to 1.5 % of the total gas flow. Under conditions with no flow Ar (0 sccm), the SO2concentration corresponded to 2% of the total gas flow.
[0048] shows the appearance of the samples after corrosion with salt deposits at 700 °C for 15 h with varying SO2concentrations.shows XRD diffractograms taken after the corrosion experiment for the samples with lowest (0.3%) and highest (2.0%) SO2concentration.
[0049] Results of the hot corrosion experiment is summarized in Table 3. Coatings according to the invention successfully prevented breakthrough of the coating, which can be seen in that no substrate oxides (oxides of the substrate material) were formed during the test. Oxides formed from the coating are present under the tested conditions, and peaks in the diffractograms corresponding to the coating (coating peaks) remain under the tested conditions. The degree of corrosion is substantially improved as compared to uncoated conditions.
[0050] SampleSubstrate Oxides (breakthrough)Coating OxidesRemaining coating peaksDegree of corrosion(visual assessment)0.3 % SO22.0 % SO20.3 % SO22.0 % SO20.3 % SO22.0 % SO20.3 % SO22.0 % SO2uncoatedyesyes(-)(-)(-)(-)↑↑↑↑↑Example 1nonoyesyesyesyes↑↑ to ↑↑Example 2nonoyesyesyesyes↑↑ to ↑↑ Legend: light↑ medium↑↑severe↑↑↑Solid particle erosion test
[0051] To evaluate resistance against solid particle erosion under conditions comparable to environments in turbines, solid particle erosion (SPE) experiments were performed according to a standardized method. The coatings according to the invention deposited on superalloy substrates of IN718 were tested alongside a comparative TiAlN coating according to prior art and uncoated samples, and the results were compared.
[0052] The solid particle erosion (SPE) experiments were conducted using a Ducom Air Jet Erosion Tester on IN718 substrates. All experiments were performed at room temperature. As erodent white corundum (Al2O3) with a particle size of 50 µm (F240) was used. For testing the nozzle distance was set to 15 mm, the particle speed was 70 m / s and the abrasive feed rate was 2 g / min. All samples were tested at impingement angles of 90° and part of the samples also at impingement angles of 30°. To obtain the mass erosion rate, the samples were weighted before and after the SPE tests and the erosion rate (µg / g) was calculated using Equation 1. Therefore, the difference in weight before and after the SPE tests (=mass loss) was determined. (1)
[0053] The volume erosion rate (mm³ / g) was calculated using Equation 2. Therefore, the crater volume (volume loss) was determined using an optical profilometer (Nanovea PS50). (2)
[0054] shows the results of the solid particle erosion experiments, whereby a low erosion rate is desirable. The solid particle erosion tests show the erosion rate of the inventive coatings to be on a similar performance level as compared to the comparative TiAlN coating according to prior art. Comparing coatings according to the inventive examples with the TiAlN reference coatings, it is observed that the erosion rate does not deteriorate due to alloying with Ta and Si. On the metric of volume erosion rate, coatings according to Example 1 show even better erosion resistance.Further embodiments and characterization
[0055] Coatings according to one further embodiment of the invention, Example 5, was produced using conditions similar to Example 3 & 4 using APO confinement ring configuration, but with parameters adjusted to operate the arc source at yet stronger magnetic fields compared to the conditions used for Examples 3 & 4. The coating is described with respect to composition in Table 4 and with respect to mechanical properties in Table 5.
[0056] Total composition(at.%)Composition on metal sublattice (at.%)SampleNTiAlTaSiTi(a)Al (b)Ta(c)Si(d)Example 551.319.620.28.91.13941182
[0057] SampleHardness[GPa]Young’s Modulus[GPa]Residual stress[GPa]Surface Roughness, Ra[µm]Example 532.4 ± 2.5479 ± 81 / /
[0058] Based on the data presented inand data acquired analogously for Example 5, oxidation rate constants were calculated to gain a deeper understanding on the oxidation kinetics. To capture a wide range of possible oxidation mechanisms, a generic power rate law was used (see Equation 1) in a first step. Here,doxdenotes the scale thickness,tthe time,koxthe rate constant andna constant. (1)
[0059] Table 6 displays the resultingnvalues and the goodness of fit R2for the investigated coatings. It is evident for all samples that neither the common parabolic (n=2) nor cubic (n=3) rate laws are applicable. Still, the differences in oxidation resistance observed for the five thin films (see) are emphasized.
[0060] The best description of the TiAlTaSiN coatings was found to be a logarithmic rate law and the resulting logarithmic rate constants klogare provided in Table 6. Calculation of klogwas performed according to Equation 2, wheredoxdenotes the oxide scale thickness,tthe time andklogthe logarithmic rate constant . (2)
[0061] The rate constants for the TiAlTaSiN thin films range between 0.243 ± 0.020 µm×h-1(Example 4) and 0.379 ± 0.019 µm×h-1(Example 1). These values demonstrate that the Al concentration in the thin films is also a decisive factor. Example 4 has the highest Al content of the five compositions and exhibits the slowest oxidation kinetics.
[0062] Table6. Calculated oxidation rate constants forexemplary embodimentsby using different rate laws.Sample NamePower lawParabolic lawLogarithmic lawnR²kp(µm²×h-1)R²klog(µm×h-1)R²Example 13.640.943.16 ± 0.74×10-30.820.379 ± 0.0190.97Example 23.570.861.94 ± 0.48×10-30.800.279 ± 0.0210.93Example 37.560.731.89 ± 0.79×10-30.360.309 ± 0.0190.93Example 412.080.671.15 ± 0.53×10-30.170.243 ± 0.0200.87Example 55.230.961.98 ± 0.62×10-30.630.307 ± 0.0110.98
[0063] For better comparison with prior art, the oxidation kinetics of the TiAlTaSiN coatings according to the exemplary embodiments were determined according to a parabolic law, with resulting parabolic constants (kp) as listed in Table 6. For the calculation Equation 3, where denotes the scale thickness,tthe time andkpthe rate constant, was used. (3)
[0064] The calculated kpvalues range from a maximum kp ~ 3.16 ± 0.74×10-3 µm2×h-1for Example 1 to a minimum kp ~ 1.15 ± 0.53×10-3 µm2×h-1for the coating with the best oxidation properties (Example 4). Oxidation rate constants for some Ti1-xAlxN-based materials are available according to literature. Unalloyed Ti1-xAlxN obtains values roughly between kp ~ 8×10-1 µm2×h-1and kp ~ 1×10-1 µm2×h-1for oxidation experiments at 850 °C. Alloying with Ta or Si leads to enhanced (lower) oxidation rates kp ~ 7×10-2 µm2×h-1to kp ~ 1×10-2µm2×h-1for Ta-alloyed versions and kp ~ 5×10-2 µm2×h-1for the Si containing coatings. A comparison of these results with the data according to the invention highlights that the combined alloying of Ta and Si significantly improves oxidation properties. Furthermore, it is crucial to have both alloying elements present, as the kpvalues reported in this study are an entire order of magnitude lower.
[0065] TiAlTaSiN coatings according to the invention may be characterized by having rate constants kplower than 4×10-3 µm2.
[0066] Additional analysis including XRD, TEM and nanoindentation post-oxidation gain insight into structural changes and the architecture of the oxide scale. Detailed analysis of two coatings according to Example 1 and Example 4 will be presented in the following.
[0067] XRD diffraction patterns acquired as a function of oxidation time for the two further investigated coatings according to Example 1 and Example 4 are shown in Figure 11a and 11b, respectively. As demonstrated in, the lower Al containing sample (Example 1) exhibits a single-phase cubic Ti(Al,Ta,Si)N crystal structure. A slight shift of the c-Ti(Al,Ta,Si)N peaks towards lower diffraction angles with increasing time hints towards initiated spinodal decomposition. Upon increasing the oxidation time to max. 500 h, the presence of w-Al(Ti,Ta,Si)N phase is detected, based on the ongoing decomposition via Al-rich phases to the stable wurtzite structure. It should be noted that the presence of XRD-peaks from silver is attributed to the residual conductive silver utilized during the fabrication of the FIB cross-sections and is not related to the behavior of the sample during oxidation. In contrast, the higher Al-containing sample of Example 4 (Figure 11b) demonstrates a dual phase structure in the as deposited state, as seen from the XRD patterns inIn a similar manner as with Example 1, the coating according to Example 4 displays during annealing a shift of the c-Ti(Al,Ta,Si)N peaks, where the peak shift indicates the onset of spinodal decomposition. Additionally, with increasing annealing time the peak belonging to the w-Al(Ti,Ta,Si)N phase (2θ~33.2°) seems to have slightly less intensity. Retarded decomposition processes due to the already present w-Al(Ti,Ta,Si)N phase could also contribute to the excellent oxidation resistance, since diffusion is reduced when the thermodynamically stable phases are already present.
[0068] For the samples shown in Figure 11a and 11b, only peaks identified as t-TiO2(rutile configuration) are detected after 24 h and 48 h. It is assumed, that a dense Al2O3top-oxide is formed, however still too thin to be detected by XRD. Increased intensities of the oxide peaks are found after increasing the time to 168 h and 500 h. Distinct corundum α-Al2O3peaks are observed for both compositions from 168 h onwards.
[0069] Figure 11c and 11d illustrate the progression of the hardness as a function of the oxidation time for Example 1 and Example 4.illustrates the progression of the hardness as a function of the oxidation time for Example 2, Example 3 and Example 5. All samples demonstrate an initial increase in hardness up to an oxidation time of 48 h. This is followed by a reduction in H for the low Al-containing sample according to Example 1 (Figure 11c) and a consistent H for the high Al-containing sample according to Example 4 (Figure 11d). Such behavior can be attributed to the well-known age-hardening mechanism. Hardness values obtained for Example 4 (Figure 11d) are in general lower compared to Example 1 due to the presence of w-AlN, as previously described.
[0070] Coatings according to some embodiments of the invention may have hardness values in the range of 35 – 42 GPa, in particular 32 – 37 GPa. Coating hardness values may be achieved after annealing and / or oxidation for sufficient time, in particular after at least 48 hours or at least 168 hours at a predetermined temperature. The predetermined temperature may be selected at 850 °C. Operating conditions of turbine components often include frequent segments at elevated temperatures.
[0071] Subsequent to the oxidation experiments after 168 h at 850 °C, cross-sectional TEM analysis of the coating according to Example 1 reveals a dense multi-layered oxide scale as illustrated in Figure 13a (with a close-up view depicted in Figure 13b). Three distinct oxide layers are visible in the bright-field images: a thick layer directly on top of the remaining coating, which consists of two different sublayers, marked with (ii) and (iii) in Figure 13b and a thinner oxide scale on top, marked with (iv). A more detailed analysis of the oxide scale was performed by employing SAED and EDX line-scans to gain knowledge on the structures and elemental distribution. The resulting SAED pattern are summarized in Figure 13c. First, the remaining coating (Figure 13c.-i) exhibits a c-Ti(Al,Ta,Si)N crystal structure which is in perfect agreement with the XRD diffractograms in the as-deposited state shown inIn addition, both sublayers of the bottom oxide scale (Figure 13c.-ii and 13c-iii) exhibit solely peaks identified as rutile TiO2structure. Lastly, the uppermost scale contains only corundum Al2O3(Figure 13c.-iv). This also agrees will with the findings shown in
[0072] Coatings according to the invention may have an outermost layer comprising or consisting of hexagonal Al2O3phase. The hexagonal Al2O3phase may preferably be corundum with crystallographic structure of space group (SG) 167, international short symbol R-3C, according to crystallographic notation. Al2O3phase may preferably corundum with crystallographic structure of space group 167 is also designated α-Al2O3. Hexagonal crystal structures can be more precisely defined by the notation with space groups, to distinguish specific crystal structures within the hexagonal crystal family.
[0073] To gain an even more detailed insight, the corresponding (S)TEM image is included in the result of the EDX line scan (see Figure 11d). Analysis of the acquired line-scan data reveals the presence of a narrow zone at the interface between coating and oxide layer (ii). This zone displays an increase in Ti signal, concurrently with a depletion of Al at the diffusion front between unaffected coating and oxide. Within the first oxide sublayer (ii) the elemental analysis shows Ta and Si alongside Ti and O. This observation suggests that both Ta and Si are substituting Ti in TiO2. A gradual decrease in both Ta and Si is observed going further towards the top, distinguishing layer (iii). The outermost scale (iv) consists exclusively of Al and O, which perfectly corresponds to the SAED results.
[0074] shows analysis of a coating with high Al content according to Example 4. The analysis reveals a highly dense oxide scale that can be subdivided into three sublayers on the remaining nitride layer (see Figure 14a and Figure 14b). This observation aligns with the findings of the sample according to Example 1; yet the three distinct sublayers are more distinct as is shown in Figure 14a The two lower sublayers (ii) and (iii) consist of a rutile TiO2 crystal structure, as can be seen in Figure 14c. On top, analogous to the Example 1 sample a dense Al2O3 (iv) layer forms.
[0075] Figure 14d illustrates the compositional evolution after oxidation detected by EDX. At the interface between the remaining nitride film and the oxide scale, reduced Al, Si, and Ta contents are observed, accompanied by a pronounced increase in Ti, consistent with the coating shown inThe first sublayer (ii) adjacent to the pristine nitride is characterized by elevated Ta and Si concentrations, while Ti remains comparatively low, indicating the formation of Ta-Si-rich mixed oxide. In the second sublayer (iii), Ta and Si are slightly reduced and exhibit a gradual decrease toward the top-oxide. In contrast, Ti is significantly increased compared to the underlying sublayer and remains largely constant across this region. The outermost oxide layer consists exclusively of Al2O3, marked by strong Al enrichment and the absence of Ti, Ta, and Si.
[0076] Comparing oxidation behaviour of the investigated exemplary TiAlTaSiN thin films demonstrates that the Al content is a primary factor governing oxidation resistance. This is attributed to the formation of a dense outermost protective Al2O3scale. As shown in, the coating according to Example 4 obtains an oxide scale thickness below 600 nm after exposure for 500 h at 850 °C. For the coating containing a lower amount of Al (Example 1), Ta and Si likely substitute Ti within rutile TiO2and gradually decrease toward the surface. In contrast, Example 4 (higher Al content) obtains more sharply defined oxide sublayers, characterized by a Ta+Si-rich and Ti depleted first sublayer, followed by Ti-, Ta- and Si-rich sublayer.
[0077] The addition of Ta or Si in Ti1-xAlxN films significantly enhances oxidation resistance. Ti1-x-yAlxTayN coatings show improved properties compared to unalloyed versions due to the positive effect of Ta on oxide scale formation. An important mechanism may be that substituting Ti with Ta in the rutile TiO2scale reduces oxygen vacancy density and slows oxygen diffusion. Furthermore, Ta prevents the formation of anatase TiO2, facilitating direct rutile formation and eliminating volume changes that cause cracks and pores in the oxide scale. The different crystal structure of anatase TiO2and rutile TiO2leads to different volumes occupied by unit cells of each material. The density of rutile TiO2is higher than anatase TiO2due to more compact crystal structure. Consistent with these findings, no anatase TiO2formation was observed in the XRD diffractograms recorded after oxidation of the TiAlTaSiN thin films according to the embodiments of the invention. In addition to Ta, Si addition promotes the growth of the dense, protective Al2O3layer. This is attributed to enhanced diffusion of Al, while inward diffusion of oxygen is effectively hindered. While Ta and Si individually enhance oxidation resistance, their combined addition gives rise to synergistic effects that further improve the oxidation stability. In more detail, the direct formation of Ti-Ta-Si-containing rutile type oxide sublayer with no anatase transition may be a key, also retarding oxygen inward diffusion and promoting Al outward diffusion. The importance of the combined presence of Ta and Si is further emphasized, by the extremely low oxidation kinetics (see Table 6) found for the TiAlTaSiN coatings in this work. It is also noted that a dual phase structure does not negatively affect the oxidation resistance of the TiAlTaSiN thin films.Description of figures
[0078] : Schematic depiction of a substrate (10) coated with a TiAlTaSiN coating layer (20) according to the invention.
[0079] : Schematic depiction of a substrate (10) coated with a TiAlTaSiN coating layer (20) according to the invention after exposure to oxidating environment. Two oxide layers: oxide layer 1 (30) and oxide layer 2 (40) have formed.
[0080] : SEM fracture cross-sections Example 1 (a) and Example 2 (b) coatings in the as deposited state are shown. A coating thickness of ~ 10 µm was established.
[0081] : SEM fracture cross-sections of the coatings grown with APO configuration in the as deposited state are shown. In (a) Example 3 and in (b) Example 4 are presented. A coating thickness of ~ 10 to 15 µm was established.
[0082] : XRD diffractograms of all as deposited coating states on IN718 substrates. Additionally, the uncoated substrate is included (bottommost diffractogram) with grey color. The reference positions for the substrate (IN718), c-TiN, c-AlN, c-TaN and h-AlN are marked by the stars (ICDD: 04-001-3422), diamonds (ICDD: 00-038-1420), squares (ICDD: 00-025-1495), circles (ICDD: 00-032-1283) and hexagons (ICDD: 00-008-0262), respectively.
[0083] : Oxide scale thickness as a function of time. All experiments were performed on IN718 substrates at 850 °C in ambient air.
[0084] : TEM micrographs for Example 2 on IN718 oxidized for 500 h at 850 °C. Bright-field (BF) overview (a), detailed BF images in (b) and (c) with the positions of the SAED pattern marked and the corresponding SAED pattern in (d-f) are presented. The integrated profiles of the SAED pattern are shown in (g-i). EELS elemental line-scan of the oxide scale is shown in (j).
[0085] : Results of solid particle erosion test. In (a) the resulting mass erosion rate (ER) is given for the two impingement angles. The ER for two different impingement angles are presented – the left (fully colored) bar for each sample represents 90° impingement angle and the right (lightly colored) bar represent 30° impingement angle. The volume erosion rate for selected systems are depicted in (b), using the same color code and annotation for impingement angle 90° (left) and impingement angle 30° (right) for each tested sample.
[0086] : Top-view images showing samples corroded with salt deposits at 700 °C for 15 h with varying SO2concentrations (0.3 %. 1 %, 1.25% 1.5 % and 2 %) in the gas mixture. The first row shows uncoated C263 samples, the second row presents C263 substrates with a coating according to Example 2, and the third row presents C263 substrates coated with a coating according to Example 1. AD denotes reference images in as deposited condition, before the start of the test.
[0087] : XRD diffractograms post-corrosion for the samples corroded with salt deposits at 700 °C for 15 h with varying SO2concentrations: 0.3 % (bottom) and 2 % (top) in the gas mixture are featured in each respective graph (a)-(c). In (a) the results for Example 1, (b) Example 2 and (c) uncoated C263 substrate are shown.
[0088] : XRD diffractograms of Example 1 and Example 4 are depicted in (a) and (b), respectively. For both coating compositions, the diffractograms of the as deposited and oxidized states (24-500 h at 850 °C) are shown from bottom to top. The reference positions for substrate (IN718), c-TiN, c-AlN, c-TaN and w-AlN are marked by stars (ICDD: 04-001-3422), diamonds (ICDD: 00-038-1420), (ICDD: 00-025-1495), circles (ICDD: 00-032-1283) and hexagons (ICDD: 00-008-0262), respectively. The oxide reference positions, t-TiO2 (rutile, ICDD:04-008-7853) and α-Al2O3(corundum, SG167, ICDD:04-006-9730) are indicated by the black half-full diamonds and the red half-full triangles, respectively. The progression of the hardness over oxidation time is shown in (c) and (d) for Example 1 and Example 4 respectively.
[0089] : Progression of the hardness over oxidation time is shown in (a) for Example 2, (b) for Example 3 and (c) for Example 5.
[0090] : Cross-sectional bright-field TEM micrographs for a sample according to Example 1 oxidized at 850 °C for 168 h are depicted in (a) and (b). The corresponding SAED patterns, integrated over the regions marked (i–iv) in (a) and (b), are presented in (c). The diffraction peaks were indexed according to reference patterns for c-Ti(Al)N (ICDD: 04-005-5251), w-AlN (ICDD: 00-008-0262), t-TiO2(rutile, ICDD:04-008-7853), and α-Al2O3(corundum, SG167, ICDD:04-006-9730).. An EDX line-scan is provided in (d) to give insight into the elemental composition of the oxide scale. The slight layering visible in both the pristine coating and the oxide scale originates from the substrate rotation during deposition.
[0091] : Cross-sectional bright-field TEM micrographs for the sample according to Example 4 oxidized at 850 °C for 500 h are depicted in (a) and (b). The corresponding SAED patterns, integrated over the regions marked (i–iv) in (a) and (b), are presented in (c). The diffraction peaks were indexed according to reference patterns for c-Ti(Al)N (ICDD: 04-005-5251), w-AlN (ICDD: 00-008-0262), t-TiO2(rutile, ICDD:04-008-7853), and α-Al2O3(corundum, SG167, ICDD:04-006-9730). An EDX line-scan is provided in (d) to give insight into the elemental composition of the oxide scale. The slight layering visible in both the pristine coating and the oxide scale originates from the substrate rotation during deposition.
[0092] Disclosed is the use of TiAlTaSiN coatings for turbine components subjected to oxidation and / or hot corrosion, wherein the substrate of the turbine component is a superalloy or a Ti-based alloy, wherein the composition of the TiAlTaSiN coating in atomic concentration is given by the formula (TiaAlbTacSid)N with a+b+c+d = 1, 0.30 ≤ b ≤ 0.50, 0.05 ≤ c ≤ 0.20, and 0.005 ≤ d ≤ 0.05.
[0093] The TiAlTaSiN coatings used for turbine components may be characterized in that the turbine components is selected from the list of compressor blades, vanes, blisks and integrated blade rotors (IBR),
[0094] The TiAlTaSiN coatings used for turbine components may be characterized in that the thickness of the TiAlTaSiN coating is in the range from 3 µm to 50 µm, preferably 5 µm to 20 µm.
[0095] The TiAlTaSiN coatings used for turbine components may be characterized in that the turbine component is at a temperature in the range from 700 ºC to 1000 ºC, preferably 750 ºC to 900 ºC.
[0096] The TiAlTaSiN coatings used for turbine components may be characterized in that the TiAlTaSiN coating is covered by two oxide layers, wherein the two oxide layers are further away from the substrate than the TiAlTaSiN coating, wherein the first oxide layer is closer to the TiAlTaSiN coating than the second oxide layer, wherein the first oxide layer comprise the elements Ti, Al, Ta, Si, O, and wherein the second oxide layer essentially consist of the elements Al and O.
[0097] The crystalline phase structure of the first oxide layer may comprise rutile-TiO2phase, and that the crystalline phase structure of the second oxide layer may consists of hexagonal Al2O3, preferably corundum (SG 167)-Al2O3of space group 167.
[0098] The rutile-TiO2phase in the first oxide layer may comprise Si and Ta to reduce oxygen diffusion through the first oxide layer, preferably through densification of the first oxide layer.
[0099] The TiAlTaSiN coatings used for turbine components may be characterized in that the TiAlTaSiN coatings are used for protection against oxidation and / or for protection against hot corrosion.
[0100] The TiAlTaSiN coatings used for turbine components may be characterized in that the composition of the TiAlTaSiN coating in atomic concentration is given by the formula (TiaAlbTacSid)N with a+b+c+d = 1, 0.30 ≤ b ≤ 0.50, 0.10 ≤ c ≤ 0.16, and 0.02 ≤ d ≤ 0.03.
[0101] Disclosed are turbine components with a TiAlTaSiN coating for protection against oxidation and / or hot corrosion, wherein the substrate of the turbine component is a superalloy or a Ti-based alloy, wherein the composition of the TiAlTaSiN coating in atomic concentration is given by the formula (TiaAlbTacSid)N with a+b+c+d = 1, 0.30 ≤ b ≤ 0.50, 0.05 ≤ c ≤ 0.20, and 0.005 ≤ d ≤ 0.05.
[0102] The turbine components with a TiAlTaSiN coating may be characterized in that the turbine components is selected from the list of compressor blades, vanes, blisks and integrated blade rotors (IBR),
[0103] The turbine components with a TiAlTaSiN coating may be characterized in that the thickness of the TiAlTaSiN coating is in the range from 3 µm to 50 µm, preferably 5 µm to 20 µm.
[0104] The turbine components with a TiAlTaSiN coating may be characterized in that the TiAlTaSiN coating is covered by two oxide layers, wherein the two oxide layers are further away from the substrate than the TiAlTaSiN coating, wherein the first oxide layer is closer to the TiAlTaSiN coating than the second oxide layer, wherein the first oxide layer comprise the elements Ti, Al, Ta, Si, O, and wherein the second oxide layer essentially consist of the elements Al and O.
[0105] The turbine components with a TiAlTaSiN coating may be characterized in that the crystalline phase structure of the first oxide layer comprises rutile-TiO2phase, and that the crystalline phase structure of the second oxide layer consists of consists of hexagonal Al2O3, preferably corundum Al2O3of space group 167
[0106] The rutile-TiO2phase in the first oxide layer may comprises Si and Ta to reduce oxygen diffusion through the first oxide layer, preferably through densification of the first oxide layer.
[0107] The turbine components with a TiAlTaSiN coating may be characterized in that the composition of the TiAlTaSiN coating in atomic concentration is given by the formula (TiaAlbTacSid)N with a+b+c+d = 1, 0.30 ≤ b ≤ 0.50, 0.10 ≤ c ≤ 0.16, and 0.02 ≤ d ≤ 0.03
[0108] The turbine components with a TiAlTaSiN coating may be characterized in that the TiAlTaSiN coating exhibits hardness in the range from 35 GPa to 42 GPa, preferably 32 GPa – 37 GPa.
[0109] The TiAlTASiN coating may have achieved the hardness after the turbine component has been subjected to annealing and / or oxidation, preferably at a temperature of 850 ºC.List of Reference signs
[0110] 10 Substrate
[0111] 20 TiAlTaSiN coating layer
[0112] 30 Oxide layer 1 (first oxide layer)
[0113] 40 Oxide layer 2 (second oxide layer)
Claims
Use of TiAlTaSiN coatings for turbine components subjected to oxidation and / or hot corrosion, wherein the substrate of the turbine component is a superalloy or a Ti-based alloy,wherein the composition of the TiAlTaSiN coating in atomic concentration is given by the formula (TiaAlbTacSid)N with a+b+c+d = 1, 0.30 ≤ b ≤ 0.50, 0.05 ≤ c ≤ 0.20, and 0.005 ≤ d ≤ 0.05.Use of TiAlTaSiN coatings for turbine components according to claim 1, characterized in that the turbine components is selected from the list of compressor blades, vanes, blisks and integrated blade rotors (IBR),Use of TiAlTaSiN coatings according to claim 1 or 2, characterized in that the thickness of the TiAlTaSiN coating is in the range from 3 µm to 50 µm, preferably 5 µm to 20 µm.Use of TiAlTaSiN coatings according to any of the preceding claims, characterized in that the turbine component is at a temperature in the range from 700 ºC to 1000 ºC, preferably 750 ºC to 900 ºC.Use of TiAlTaSiN coatings according to any of the preceding claims, characterized in that the TiAlTaSiN coating is covered by two oxide layers, wherein the two oxide layers are further away from the substrate than the TiAlTaSiN coating, wherein the first oxide layer is closer to the TiAlTaSiN coating than the second oxide layer, wherein the first oxide layer comprise the elements Ti, Al, Ta, Si, O, and wherein the second oxide layer essentially consist of the elements Al and O.Use of TiAlTaSiN coatings according to claim 5, characterized in that the crystalline phase structure of the first oxide layer comprises rutile-TiO2phase, and that the crystalline phase structure of the second oxide layer consists of hexagonal Al2O3, preferably corundum)-Al2O3of space group 167.Use of TiAlTaSiN coatings according to claim 6, wherein the rutile-TiO2phase in the first oxide layer comprises Si and Ta to reduce oxygen diffusion through the first oxide layer, preferably through densification of the first oxide layer.Use of TiAlTaSiN coatings according to any one of the preceding claims, characterized in that the TiAlTaSiN coatings are used for protection against oxidation and / or for protection against hot corrosion.Use of TiAlTaSiN coatings according to any one of the preceding claims,characterized in that the composition of the TiAlTaSiN coating in atomic concentration is given by the formula (TiaAlbTacSid)N with a+b+c+d = 1, 0.30 ≤ b ≤ 0.50, 0.10 ≤ c ≤ 0.16, and 0.02 ≤ d ≤ 0.03.Turbine component with a TiAlTaSiN coating for protection against oxidation and / or hot corrosion,wherein the substrate of the turbine component is a superalloy or a Ti-based alloy,wherein the composition of the TiAlTaSiN coating in atomic concentration is given by the formula (TiaAlbTacSid)N with a+b+c+d = 1, 0.30 ≤ b ≤ 0.50, 0.05 ≤ c ≤ 0.20, and 0.005 ≤ d ≤ 0.05.Turbine component according to claim 10, characterized in that the turbine components is selected from the list of compressor blades, vanes, blisks and integrated blade rotors (IBR),Turbine component according to claim 10 or 11, characterized in that the thickness of the TiAlTaSiN coating is in the range from 3 µm to 50 µm, preferably 5 µm to 20 µm.Turbine component according to any one of the claims 10 to 12, characterized in that the TiAlTaSiN coating is covered by two oxide layers, wherein the two oxide layers are further away from the substrate than the TiAlTaSiN coating, wherein the first oxide layer is closer to the TiAlTaSiN coating than the second oxide layer, wherein the first oxide layer comprise the elements Ti, Al, Ta, Si, O, and wherein the second oxide layer essentially consist of the elements Al and O.Turbine component according to claim 13, characterized in that the crystalline phase structure of the first oxide layer comprises rutile-TiO2phase, and that the crystalline phase structure of the second oxide layer consists of consists of hexagonal Al2O3, preferably corundum)-Al2O3of space group 167..Turbine component according to claim 14, wherein the rutile-TiO2phase in the first oxide layer comprises Si and Ta to reduce oxygen diffusion through the first oxide layer, preferably through densification of the first oxide layer.Turbine component according to any one of claims 10-15,characterized in that the composition of the TiAlTaSiN coating in atomic concentration is given by the formula (TiaAlbTacSid)N with a+b+c+d = 1, 0.30 ≤ b ≤ 0.50, 0.10 ≤ c ≤ 0.16, and 0.02 ≤ d ≤ 0.03Turbine component according to any one of claims 10-16, characterized in that the TiAlTaSiN coating exhibits hardness in the range from 35 GPa to 42 GPa, preferably 32 GPa – 37 GPa.Turbine component according to claim 17, wherein the turbine component has been subjected to annealing and / or oxidation, preferably at a temperature of 850 ºC.