Melt composition analysis method and device for ladle refining process
Through the dynamic model and component mass fraction calculation formula, the composition changes of liquid steel, slag phase, and inclusions during ladle refining are analyzed, and the problem of difficult control of inclusion components in the existing technology is solved, and the accuracy of liquid steel components is achieved Controllability of forecasting and production processes.
Patent Information
- Application Number
- CN202010589868.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-06-24
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-06-24
AI Technical Summary
During the ladle refining process, due to insufficient reaction time between the steel-refining slag-inclusions, the thermodynamic equilibrium cannot be achieved, and the inclusion components and morphological changes are complex, and the prior art is difficult to accurately predict and control the components of non-metallic inclusions. .
Provide a melt component analysis method and device to calculate the timing change curve of mass fractions of liquid steel, slag phase, inclusions and refractory materials through dynamic models, and simulate ladle refining based on process parameters and preset component mass fraction calculation formulas. The mass fraction of each component in the reaction vessel during the process changes.
The precise kinetic prediction of the liquid steel, slag phase, and inclusion components during the ladle refining process is achieved, the control level of non-metallic inclusions is improved, and the accuracy of the liquid steel composition and the controllability of the production process are improved.
Smart Images

Figure CN111737927B_ABST
Abstract
Description
Background Art
[0002] Ladle Furnace (LF) is a molten steel refining method that integrates arc heating, gas stirring and vacuum degassing. The LF method uses argon stirring, graphite electrode submerged arc heating and slag refining under atmospheric pressure. For degassing, a vacuum system can also be used. Through LF ladle refining furnace refining, the molten steel can be highly purified and homogenized in a short time, thereby achieving various metallurgical purposes.
[0003] In the LF ladle refining process, the reaction time between molten steel, refining slag and inclusions is insufficient, so the thermodynamic equilibrium state cannot be reached. In addition, the composition and morphology of inclusions in molten steel are constantly changing from the beginning of generation to the end of refining and even during continuous casting. The reaction between inclusions and molten steel is always ongoing, and its composition is directly affected by the composition and temperature of molten steel. The alloy, refining slag, refractory materials and furnace atmosphere are constantly changing the composition of molten steel due to the reaction or material exchange with molten steel, which indirectly affects the behavior of inclusions. Therefore, breaking the traditional idea of only using thermodynamic equilibrium calculation to predict the composition of inclusions and using kinetic models to study the composition changes of inclusions in molten steel has extremely important theoretical value and practical significance for improving the control level of non-metallic inclusions in steel.
[0004] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present disclosure, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention
[0005] The purpose of the present disclosure is to provide a melt composition analysis method, device and electronic equipment for a ladle refining process, which are used to obtain a kinetic prediction model that is consistent with the actual production process, and output simulation calculation results of the time-series changes in the mass fraction of each component in the reaction vessel during the ladle refining process that conforms to the actual production process.
[0006] According to a first aspect of an embodiment of the present disclosure, a melt composition analysis method for a ladle refining process is provided, comprising: obtaining process parameters in response to a data input message from a user, the process parameters including at least a reaction vessel size, a reaction time, a reaction temperature, a jet pressure, a jet flow rate, an initial composition of the molten steel, an initial composition of inclusions, an initial composition of the slag phase, and an initial mass of a refractory material; determining a time-series variation curve of the mass fraction of molten steel components, a time-series variation curve of the mass fraction of inclusion components, and a time-series variation curve of the mass fraction of slag phase components according to the process parameters and a preset component mass fraction calculation formula group; and responding to a curve viewing instruction from the user, displaying the time-series variation curve of the mass fraction of molten steel components, the time-series variation curve of the mass fraction of inclusion components, and the time-series variation curve of the mass fraction of slag phase components according to the curve viewing instruction.
[0007] In an exemplary embodiment of the present disclosure, determining the time series variation curve of the mass fraction of the molten steel component, the time series variation curve of the mass fraction of the inclusion component, and the time series variation curve of the mass fraction of the slag phase component according to the process parameters and the preset component mass fraction calculation formula group includes: determining the volume parameter according to the initial composition of the molten steel, the initial composition of the inclusion, the initial composition of the slag phase, and the initial mass of the refractory material, the volume parameter at least including the volume of the molten steel, the volume of the inclusion, the number of inclusions of different diameters, the volume of the slag phase, and the volume of the refractory material; determining the contact area parameter according to the size of the reaction vessel and the volume parameter The contact area parameters at least include the contact area between the molten steel and the slag phase, the contact area between the molten steel and the inclusions, the contact area between the molten steel and the refractory material, and the contact area between the refractory material and the slag phase; the volume parameters and the contact area parameters are brought into a preset component mass fraction calculation formula group to determine the molten steel composition, the inclusion composition, and the slag phase composition corresponding to multiple time points; according to the molten steel composition, the inclusion composition, and the slag phase composition corresponding to the multiple time points, the molten steel component mass fraction time series change curve, the inclusion component mass fraction time series change curve, and the slag phase component mass fraction time series change curve are determined.
[0008] In an exemplary embodiment of the present disclosure, the volume parameter and the contact area parameter are brought into the preset component mass fraction calculation formula group to determine the molten steel composition, inclusion composition, and slag phase composition corresponding to multiple time points, including: determining the current molten steel composition, the current slag phase composition, the current inclusion composition, and the current refractory material mass, wherein in the first calculation, the current molten steel composition, the current slag phase composition, the current inclusion composition, and the current refractory material mass are respectively equal to the initial composition of the molten steel, the initial composition of the slag phase, the initial composition of the inclusions, and the initial mass of the refractory material; determining the mass fraction of each component on the molten steel-slag interface corresponding to the current molten steel composition according to the volume parameter and the contact area parameter; determining the first molten steel composition and the first slag phase composition according to the first preset component mass fraction calculation formula group and the current molten steel composition, the current slag phase composition, and the mass fraction of each component on the molten steel-slag interface corresponding to the current molten steel composition; determining the mass fraction of each component on the molten steel-inclusion interface corresponding to the first molten steel composition according to the first molten steel composition and the current inclusion composition; determining the mass fraction of each component on the molten steel-inclusion interface corresponding to the first molten steel composition according to the second preset component mass fraction calculation formula group and the The second molten steel composition and the first inclusion composition are determined by the mass fractions of each component on the molten steel-inclusion interface corresponding to the first molten steel composition; the third molten steel composition, the first mass of the refractory material, and the second slag phase composition formed by the dissolution of the refractory material into the molten steel and the slag phase and the reaction of the refractory material with the molten steel are determined according to the third preset component mass fraction calculation formula group and the current mass of the refractory material; the mass proportion of oxygen element in the molten steel under the influence of the secondary oxidation reaction of the air on the molten steel is determined according to the fourth preset component mass fraction calculation formula group and the third molten steel composition, contact area parameters, jet pressure, jet flow rate, and reaction temperature; the floating removal reaction of the inclusions is calculated according to the fifth preset component mass fraction calculation formula group to determine the second inclusion composition and the third slag phase composition under the floating condition; the current molten steel composition is updated according to the third molten steel composition and the mass proportion of oxygen element, the current inclusion composition is updated according to the second inclusion composition, the current slag phase composition is updated according to the third slag phase composition, and the current refractory material mass is updated according to the first mass of the refractory material.
[0009] In an exemplary embodiment of the present disclosure, the process parameters also include an initial alloy composition, and determining the first molten steel composition and the first slag phase composition according to a first preset component mass fraction calculation formula group and the current molten steel composition, the current slag phase composition, and the mass fractions of each component on the molten steel-slag phase interface corresponding to the current molten steel composition includes: determining the current alloy composition, when the current alloy composition is equal to the initial alloy composition in the first calculation; determining the fourth molten steel composition and the first alloy composition according to a sixth preset component mass fraction calculation formula group and the current alloy composition and the current molten steel composition; determining the first molten steel composition and the first slag phase composition according to the first preset component mass fraction calculation formula group and the fourth molten steel composition, the current slag phase composition, and the mass fractions of each component on the molten steel-slag phase interface corresponding to the current molten steel composition; and updating the current alloy composition according to the first alloy composition.
[0010] In an exemplary embodiment of the present disclosure, it also includes: obtaining actual refining process sampling results corresponding to the group of process parameters, the actual refining process sampling results including the measured molten steel composition, measured inclusion composition, and measured slag phase composition corresponding to multiple time points; correcting the parameter values of the preset component mass fraction calculation formula group according to the difference between the actual refining process sampling results and the molten steel composition, inclusion composition, and slag phase composition at the time points corresponding to the time series change curve of the molten steel component mass fraction, the time series change curve of the inclusion component mass fraction, and the time series change curve of the slag phase component mass fraction.
[0011] In an exemplary embodiment of the present disclosure, it also includes: obtaining the time-series change curves of the mass fraction of molten steel components, the time-series change curves of the mass fraction of inclusion components, and the time-series change curves of the mass fraction of slag phase components corresponding to multiple sets of process parameters; determining the preferred process parameters according to preset indicators and the time-series change curves of the mass fraction of molten steel components, the time-series change curves of the mass fraction of inclusion components, and the time-series change curves of the mass fraction of slag phase components corresponding to multiple sets of process parameters.
[0012] In an exemplary embodiment of the present disclosure, displaying the time-series change curve of the mass fraction of the molten steel components, the time-series change curve of the mass fraction of the inclusion components and the time-series change curve of the mass fraction of the slag phase components according to the curve viewing instruction includes at least one of the following methods: displaying the curve of the mass fraction of each component in the molten steel changing with temperature; displaying the curve of the mass fraction of each component in the inclusions changing with temperature; displaying the curve of the mass fraction of each component in the slag phase changing with temperature; displaying the curve of the mass fraction of each component in the molten steel changing with gas pressure; displaying the curve of the mass fraction of each component in the inclusions changing with gas pressure; displaying the curve of the mass fraction of each component in the slag phase changing with gas pressure; displaying the time-series change curve of the melt temperature.
[0013] According to a second aspect of an embodiment of the present disclosure, there is provided a melt composition analysis device for a ladle refining process, comprising: an input module, configured to obtain process parameters in response to a data input message from a user, the process parameters comprising at least reaction vessel size, reaction time, reaction temperature, jet pressure, jet flow rate, initial composition of molten steel, initial composition of inclusions, initial composition of slag phase and initial mass of refractory material; a calculation module, configured to determine a time series change curve of molten steel component mass fraction, a time series change curve of inclusion component mass fraction and a time series change curve of slag phase component mass fraction according to the process parameters and a preset component mass fraction calculation formula group; a curve display module, configured to respond to a curve viewing instruction from a user, and display the time series change curve of molten steel component mass fraction, the time series change curve of inclusion component mass fraction and the time series change curve of slag phase component mass fraction according to the curve viewing instruction.
[0014] According to a third aspect of the present disclosure, an electronic device is provided, comprising: a memory; and a processor coupled to the memory, wherein the processor is configured to execute any one of the above methods based on instructions stored in the memory.
[0015] According to a fourth aspect of the present disclosure, a computer-readable storage medium is provided, on which a program is stored, and when the program is executed by a processor, any of the above methods is implemented.
[0016] The disclosed embodiments calculate the influence of refractory materials on the composition of molten steel, the influence of refractory materials on the composition of slag phase, and the influence of the reaction between air and molten steel on the composition of molten steel in the "molten steel-slag phase-inclusions-refractory materials-air" system, and can accurately determine the time series variation curve of the mass fraction of each component in the molten steel, slag phase, and inclusions during the ladle refining process.
[0017] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.
[0019] Figure 1 is a flow chart of a melt composition analysis method in an exemplary embodiment of the present disclosure.
[0020] Figure 2 is a schematic diagram of the main parts of the ladle refining process in an exemplary embodiment of the present disclosure.
[0021] Figure 3 It is a schematic diagram of various reactions involved in the calculation of the embodiments of the present disclosure.
[0022] Figure 4 It is a schematic diagram of sub-steps of step S102 in one embodiment of the present disclosure.
[0023] Figure 5 It is a flowchart of the calculation process shown in step S1023 in one embodiment of the present disclosure.
[0024] Figure 6 It is realized by presetting the group of component mass fraction calculation formulas Figure 5 Schematic diagram of the process steps.
[0025] Figure 7 is a flow chart of a calculation process taking alloy effects into account in one embodiment of the present disclosure.
[0026] Figure 8 It is a flow chart of a method for correcting parameters of a preset component mass fraction calculation formula group in one embodiment of the present disclosure.
[0027] Fig. 9 It is a block diagram of a melt composition analysis device for a ladle refining process in an exemplary embodiment of the present disclosure.
[0028] Fig.10 is a block diagram of an electronic device in an exemplary embodiment of the present disclosure. DETAILED DESCRIPTION
[0029] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in one or more embodiments in any suitable manner. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, components, devices, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.
[0030] In addition, the accompanying drawings are only schematic diagrams of the present disclosure, and the same reference numerals in the drawings represent the same or similar parts, so their repeated description will be omitted. Some of the block diagrams shown in the accompanying drawings are functional entities, which do not necessarily correspond to physically or logically independent entities. These functional entities can be implemented in software form, or implemented in one or more hardware modules or integrated circuits, or implemented in different networks and / or processor devices and / or microcontroller devices.
[0031] The exemplary embodiments of the present disclosure are described in detail below with reference to the accompanying drawings.
[0032] Figure 1 The flowchart of the melt composition analysis method in the exemplary embodiment of the present disclosure is schematically shown. Figure 1 , a melt composition analysis method 100 for a ladle refining process may include:
[0033] Step S101, obtaining process parameters in response to a user's data input message, wherein the process parameters at least include reaction vessel size, reaction time, reaction temperature, jet pressure, jet flow rate, initial composition of molten steel, initial composition of inclusions, initial composition of slag phase, and initial mass of refractory materials;
[0034] Step S102, determining a time series variation curve of the mass fraction of the molten steel components, a time series variation curve of the mass fraction of the inclusion components, and a time series variation curve of the mass fraction of the slag phase components according to the process parameters and a preset component mass fraction calculation formula group;
[0035] Step S103, responding to a curve viewing instruction from a user, displaying the steel liquid component mass fraction time series variation curve, the inclusion component mass fraction time series variation curve, and the slag phase component mass fraction time series variation curve according to the curve viewing instruction.
[0036] The disclosed embodiments can accurately determine the time series variation curve of the mass fraction of each component in the molten steel, slag phase and inclusions during the ladle refining process by calculating the influence of refractory materials on the composition of molten steel, the influence of refractory materials on the composition of slag phase, and the influence of the reaction between air and molten steel on the composition of molten steel.
[0037] Next, each step of the melt composition analysis method 100 will be described in detail.
[0038] In step S101, process parameters are obtained in response to a user's data input message, wherein the process parameters include at least reaction vessel size, reaction time, reaction temperature, jet pressure, jet flow rate, initial composition of molten steel, initial composition of inclusions, initial composition of slag phase, and initial quality of refractory materials.
[0039] Different from the related art, the embodiment of the present disclosure calculates the influence of oxygen on the ladle refining process and the influence of refractory materials on the ladle refining process to improve the accuracy of calculating the composition of the reaction substances. Therefore, the reaction temperature, reaction time, and initial mass of the refractory materials are added to the process parameters that must be input.
[0040] Figure 2 is a schematic diagram of the main parts of the ladle refining process in an exemplary embodiment of the present disclosure.
[0041] refer to Figure 2 The main parts involved in the ladle refining process include at least a reaction vessel 11 (ladle), a refractory material 12, molten steel 13, inclusions 14, a slag phase 15, air 16 and a jet nozzle 17.
[0042] Among them, the cross-section of the reaction container 11 is generally an inverted trapezoid. At this time, the size of the reaction container may include the angle between the cross-section and the bottom surface, the bottom area, the molten pool depth, etc. In other embodiments, the reaction container 11 may also be other shapes. At this time, the size of the reaction container may include more content, and the present disclosure does not impose any special restrictions on this.
[0043] The refractory material 12 is arranged on the inner surface of the reaction vessel, and its main component is magnesium oxide (MgO), and is used to separate the melt (molten steel 13, inclusions 14 and slag phase 15) from the reaction vessel 11. Figure 2 It can be seen that the parameters such as the refractory thickness and the refractory surface area can be calculated through the initial mass of the refractory material and the size of the reaction vessel.
[0044] The initial composition of the molten steel 13 includes, for example, data such as the mass of the molten steel, the volume of the molten steel, and the mass proportion of each component in the molten steel, wherein the mass proportion of each component in the molten steel can be measured according to a common detection method.
[0045] The liquid steel 13 is doped with solid inclusions 14, and the inclusions 14 are mostly small particles. The composition, average diameter and number density of the inclusions 14 in the molten steel 13 can be measured by general detection means, and then the number of inclusions 14 contained in the molten steel and the mass proportion of each component can be calculated according to the volume of the molten steel 13.
[0046] The solid slag phase 15 floats on the surface of the molten steel 13, and its main components are various oxides.
[0047] Parameters such as reaction temperature, reaction time, jet (argon) flow rate, jet pressure, etc. can be set by those skilled in the art according to actual working conditions. Among them, the reaction temperature can include, for example, the initial temperature of the melt and the subsequent heating strategy, which is not particularly limited in the present disclosure.
[0048] In some embodiments, if an alloy needs to be added to the molten steel, the initial composition of the alloy also needs to be provided in the process parameters, that is, at least one or more of the alloy mass, alloy volume, and mass proportion of each component in the alloy.
[0049] It is understandable that, in addition to the above-mentioned process parameters, the input parameters involved in the operation may include other conventional parameter settings, which are not listed one by one in the present disclosure.
[0050] The method 100 may be implemented by establishing a software tool. In this step, the process parameters input by the user may be received through the parameter input interface of the software.
[0051] In step S102, the steel liquid component mass fraction time series variation curve, the inclusion component mass fraction time series variation curve and the slag phase component mass fraction time series variation curve are determined according to the process parameters and the preset component mass fraction calculation formula group.
[0052] In the embodiments disclosed herein, a kinetic model of a six-phase multi-component system of "molten steel-slag phase-inclusions-refractory material-alloy-air" is established mainly based on coupled reactions to perform kinetic calculations, so as to calculate the mass transfer process and chemical reaction process between the solid-liquid-gas three phases during the ladle refining process, and obtain the changes in system composition at any time during the ladle refining process.
[0053] Figure 3 It is a schematic diagram of various reactions involved in the calculation of the embodiments of the present disclosure.
[0054] refer to Figure 3 In the embodiments disclosed herein, the main considerations include the influence of the reaction between the slag phase and the molten steel on the slag phase composition and the influence on the molten steel composition, the influence of the reaction between the inclusions and the molten steel on the inclusion composition and the molten steel composition, the influence of the reaction between the refractory material and the molten steel on the molten steel composition, the influence of the dissolution of the refractory material on the slag phase composition, the influence of the secondary oxidation of the molten steel by air on the molten steel composition, and the influence of the flotation of inclusions on the inclusion composition and the slag phase composition. In the embodiments of adding alloys, the influence of the dissolution of the alloy on the molten steel composition and the influence of the deoxidation products of the alloy on the inclusion composition are also considered.
[0055] Figure 4 It is a schematic diagram of sub-steps of step S102.
[0056] refer to Figure 4 , step S102 may include:
[0057] Step S1021, determining volume parameters according to the initial composition of the molten steel, the initial composition of the inclusions, the initial composition of the slag phase, and the initial mass of the refractory material, wherein the volume parameters at least include the volume of the molten steel, the volume of the inclusions, the number of inclusions of different diameters, the volume of the slag phase, and the volume of the refractory material;
[0058] Step S1022, determining contact area parameters according to the size and volume parameters of the reaction container, the contact area parameters at least including the contact area between the molten steel and the slag phase, the contact area between the molten steel and the inclusions, the contact area between the molten steel and the refractory material, and the contact area between the refractory material and the slag phase;
[0059] Step S1023, bringing the volume parameter and the contact area parameter into a preset component mass fraction calculation formula group to determine the molten steel composition, inclusion composition, and slag phase composition corresponding to multiple time points;
[0060] Step S1024, determining a molten steel component mass fraction time series variation curve, an inclusion component mass fraction time series variation curve, and a slag phase component mass fraction time series variation curve according to the molten steel composition, inclusion composition, and slag phase composition corresponding to multiple time points.
[0061] refer to Figure 4 , in order to ensure the smooth calculation of the preset component mass fraction calculation formula group, it is necessary to use other formula groups to provide parameters for the preset component mass fraction calculation formula group according to the input process parameters and other default parameters. For example, the contact area parameter can be first determined according to the size of the reaction vessel, and the contact area parameter at least includes the contact area between the molten steel and the slag phase, the contact area between the molten steel and a single inclusion, the contact area between the molten steel and the refractory material, and the contact area between the refractory material and the slag phase; then the volume parameter is determined according to the initial composition of the molten steel, the initial composition of the inclusions, the initial composition of the slag phase, and the initial mass of the refractory material, and the volume parameter at least includes the volume of the molten steel, the volume of the inclusions, the number of inclusions of different diameters, the volume of the slag phase, and the volume of the refractory material; finally, the contact area parameter and the volume parameter are brought into the preset component mass fraction calculation formula group, and the molten steel composition, the inclusion composition, and the slag phase composition corresponding to multiple time points are calculated by the preset component mass fraction calculation formula group. The types of the above volume parameters and contact area parameters are only examples. In actual calculations, the types of volume parameters and contact area parameters can be adjusted according to different working conditions.
[0062] Of course, the calculation process of the preset component mass fraction calculation formula group also involves default parameters. These default parameters do not change with the change of input values. They belong to the parameters of the mathematical model itself or objective existence and can be obtained by looking up the table.
[0063] Figure 5 It is a flowchart of the calculation process shown in step S1023 in one embodiment of the present disclosure.
[0064] refer to Figure 5 , the calculation process may include:
[0065] Step S501, obtaining process parameters;
[0066] Step S502, determine whether the specified number of calculations has been reached, if not, proceed to step S503, if yes, end the calculation;
[0067] Step S503, determine whether to add alloy, if yes, go to step S505, if no, directly go to step S505;
[0068] Step S504, calculating the influence of alloy dissolution and alloy deoxidation products on the composition of molten steel;
[0069] Step S505, calculating the concentration of each component on the molten steel-slag interface;
[0070] Step S506, calculating the composition of the molten steel and the composition of the slag phase according to the concentration of each component on the molten steel-slag phase interface;
[0071] Step S507, calculating the effect of the dissolution of the refractory material into the molten steel and the slag phase on the composition of the molten steel and the slag phase;
[0072] Step S508, calculating the effect of secondary oxidation of molten steel by air on the composition of molten steel;
[0073] Step S509, calculating the concentration of each component on the molten steel-inclusion interface;
[0074] Step S510, calculating the inclusion composition and the molten steel composition according to the concentration of each component on the molten steel-inclusion interface;
[0075] Step S511, calculating the inclusion composition after the inclusion floats up;
[0076] Step S512, increase the number of calculations by one, and return to step S502.
[0077] Figure 5 Each step in the above process can be realized mainly by presetting a group of component mass fraction calculation formulas.
[0078] Figure 6 It is realized by presetting the group of component mass fraction calculation formulas Figure 5 Schematic diagram of the process steps.
[0079] refer to Figure 6 , the detailed calculation process can include:
[0080] Step S601, determining the current molten steel composition, the current slag phase composition, the current inclusion composition, and the current refractory material quality. In the first calculation, the current molten steel composition, the current slag phase composition, the current inclusion composition, and the current refractory material quality are equal to the initial composition of the molten steel, the initial composition of the slag phase, the initial composition of the inclusions, and the initial quality of the refractory material, respectively;
[0081] Step S602, determining the mass fraction of each component on the molten steel-slag interface corresponding to the current molten steel composition according to the volume parameter and the contact area parameter;
[0082] Step S603, determining the first molten steel composition and the first slag phase composition according to the first preset component mass fraction calculation formula group, the current molten steel composition, the current slag phase composition, and the mass fractions of each component on the molten steel-slag phase interface corresponding to the current molten steel composition;
[0083] Step S604, determining the mass fraction of each component on the molten steel-inclusion interface corresponding to the first molten steel composition according to the first molten steel composition and the current inclusion composition;
[0084] Step S605, determining the second molten steel composition and the first inclusion composition according to the second preset component mass fraction calculation formula group and the first molten steel composition, the current inclusion composition, and the mass fraction of each component on the molten steel-inclusion interface corresponding to the first molten steel composition;
[0085] Step S606, determining a third molten steel composition formed by the dissolution of the refractory material into the molten steel and the slag phase, the first mass of the refractory material, and the second slag phase composition according to the third preset component mass fraction calculation formula group and the current mass of the refractory material;
[0086] Step S607, determining the mass proportion of oxygen in the molten steel under the influence of the secondary oxidation reaction of the air on the molten steel according to the fourth preset component mass fraction calculation formula group and the third molten steel composition, contact area parameter, jet pressure, jet flow rate, and reaction temperature;
[0087] Step S608, calculating the floating removal reaction of inclusions according to the fifth preset component mass fraction calculation formula group to determine the second inclusion composition and the third slag phase composition under the floating condition;
[0088] Step S609, updating the current molten steel composition according to the third molten steel composition and the oxygen element mass ratio, updating the current inclusion composition according to the second inclusion composition, updating the current slag phase composition according to the third slag phase composition, and updating the current refractory material quality according to the first quality of the refractory material.
[0089] In one embodiment, the first preset component mass fraction calculation formula group for calculating the reaction between the molten steel and the slag phase includes at least:
[0090]
[0091] Among them, d[%M] / dt and d(%MO n ) / dt represent the component M in the molten steel and the component MO in the slag phase respectively n The rate of change of mass fraction percentage, unit is s -1;[%M] and (%MO n ) represent the mass fractions of the components in the molten steel and slag phases, respectively. n is the serial number. The mass fractions of all components M in the molten steel in this calculation represent the first molten steel composition obtained in this calculation. Similarly, the mass fractions of all components MO in the slag phase n The mass fraction in this calculation represents the first slag phase composition obtained in this calculation; k m and k s Respectively represent the mass transfer coefficients in the molten steel and slag phases, in units of m / s; A steel-slag Represents the contact area between the molten steel and the slag phase, obtained in step S1022, in m 2 ; V steel and V slag Respectively represent the volume of molten steel and the volume of slag phase, obtained from step S1021, in units of m 3 ; The superscript b represents the parameters inside the molten steel or the slag phase, which are obtained from the current molten steel composition or the current slag phase composition; the superscript * represents the parameters on the interface layer between the molten steel and the slag phase, which are obtained by step S602.
[0092] The second preset component mass fraction calculation formula group for calculating the reaction between the molten steel and the inclusions includes at least:
[0093]
[0094] Among them, A steel-inc Represents the contact area between the molten steel and a single inclusion, determined according to the average diameter of the inclusion, obtained in step S1022, in m 2 ; V steel and V inc Respectively represent the volume of molten steel and the average volume of a single inclusion, obtained in step S1021, in units of m 3 ;n j Indicates that the diameter of the molten steel is d j The total number of inclusions is obtained according to the current inclusion composition; j represents the inclusion number; [%M] and (%MO n ) represent the mass fractions of components in the molten steel and inclusions respectively, n is the serial number, the mass fraction of all components in the molten steel is the second molten steel composition, and the mass fraction of all components in the inclusions is the first inclusion composition.
[0095] The third preset component mass fraction calculation formula group used to calculate the reaction between the refractory material and the slag phase, and the reaction between the refractory material and the molten steel includes at least:
[0096]
[0097] In the embodiments of the present disclosure, the modeling is performed under the assumption that the main component of the refractory material is magnesium oxide (MgO).
[0098] In formula (3), (%MgO) ref *Indicates the saturation concentration of MgO in the molten steel-slag interface layer, which is an objective parameter and can be obtained by looking up the table; (%MgO) b Indicates the concentration of MgO in the slag phase, obtained based on the first slag phase composition; [%M] b is the mass fraction of component M in the molten steel, obtained based on the composition of the second molten steel; [%M] * is the mass fraction of the steel component M on the steel-refractory interface layer, obtained by pre-calculation; A ref_slag Represents the contact area between refractory and slag phase, A lining-steel Represents the contact area between the refractory material and the molten steel, obtained through step S1022, and the unit is m 2 ; V slag Represents the slag phase volume, V steel Represents the volume of molten steel, obtained through step S1021, in m 3 ;k ref_MgO is the mass transfer coefficient of MgO from refractory to slag phase, k Mg It indicates the mass transfer coefficient of Mg in the refractory to the molten steel, and the unit is m / s. [%M] indicates the mass fraction of the component M in the molten steel, (%MgO) indicates the mass fraction of the component MgO in the slag phase, and the mass fraction of all components in the molten steel is the third molten steel component. The first mass of the refractory and the second slag phase component can be calculated based on the mass fraction of the component MgO in the slag phase.
[0099] The fourth preset component mass fraction calculation formula group for calculating the secondary oxidation reaction of air to molten steel includes at least:
[0100]
[0101] d[%O] / dt represents the rate of change of the mass percentage of oxygen in the molten steel; M O Indicates the atomic weight of oxygen element, in g / mol; A plume It indicates the area of the slag layer blown away by the gas column formed by blowing argon. It can be calculated by fluid mechanics based on parameters such as jet pressure and jet flow rate. The unit is m 2 ρ steel It indicates the density of molten steel, which can be obtained according to the composition of molten steel, and the unit is kg / m 3 ; V steel Indicates the volume of molten steel, in m 3 ;k O2 It represents the mass transfer coefficient of oxygen, in m / s; P O2 and P O2* represents the oxygen partial pressure at the slag layer surface and the slag interface, in Pa. This model assumes that the oxygen partial pressure at the slag interface is equal to 0. R is the gas constant, T is the reaction temperature, in Kelvin. [%O] is the mass fraction of oxygen in the molten steel. The mass fraction of oxygen in the molten steel can be obtained by calculation using formula (4).
[0102] In this step, Fluent (computational fluid dynamics software) can be used to first perform numerical simulation on the ladle bottom argon blowing process, study and understand the turbulent characteristics of the molten steel in the ladle during the ladle bottom argon blowing process, and combine the ladle flow field with the multivariate reaction kinetic model to optimize the calculation parameters in the kinetic model and determine the multiple parameters used in the calculation process of formula (4).
[0103] The fifth preset component mass fraction calculation formula group for calculating the floating removal reaction of inclusions includes:
[0104]
[0105] Where n j Indicates the total number of inclusions in the reaction vessel; H indicates the depth of the molten pool, in m; u 0 It indicates the average rising speed of molten steel in the plume area, which is determined by computer numerical simulation and is related to the jet flow rate, jet pressure, and molten pool depth. The unit is m / s; u slip,j It indicates the relative velocity between inclusions and molten steel in the plume area, which is determined by computer numerical simulation and is related to the diameter of the inclusions and the jet flow rate. The unit is m / s; V steel Indicates the volume of molten steel, in m 3 ; V plume It represents the volume of the plume area, determined by computer numerical simulation, in m 3 .
[0106] The result of one calculation of the preset component mass fraction calculation formula group (1) to (5) can obtain the mass fraction ratio of each component in the molten steel, slag phase and inclusions. The result of one calculation is used as the input value of the next calculation of the preset component mass fraction calculation formula group (1) to (5), and the calculation is iterated to obtain the curve of the component mass fraction ratio of each reaction substance at different time points changing with time, that is, the time series change curve of the mass fraction of the molten steel component, the time series change curve of the mass fraction of the inclusion component and the time series change curve of the mass fraction of the slag phase component.
[0107] It is worth mentioning that the preset component mass fraction calculation formula group (1) to (5) can be run in sequence or simultaneously in one calculation. When running in sequence, the running order of the formula can be changed and is not limited to the above calculation order.
[0108] In one embodiment of the present disclosure, the effect of adding alloys on the composition of molten steel is also considered. At this time, the input process parameters include the initial composition of the alloy, that is, the mass fraction ratio of each component in the alloy.
[0109] Figure 7 is a flow chart of a calculation process taking alloy effects into account in one embodiment of the present disclosure.
[0110] refer to Figure 7 , when considering alloy additions, Figure 6 In the calculation process shown, step S603 may include:
[0111] Step S6031, determining the current alloy composition, the current alloy composition being equal to the initial alloy composition during the first calculation;
[0112] Step S6032, determining a fourth molten steel composition and a first alloy composition according to a sixth preset component mass fraction calculation formula group, the current alloy composition, and the current molten steel composition;
[0113] Step S6033, determining the first molten steel composition and the first slag phase composition according to the first preset component mass fraction calculation formula group, the fourth molten steel composition, the current slag phase composition, and the mass fractions of each component on the molten steel-slag phase interface corresponding to the current molten steel composition;
[0114] Step S6034: update the current alloy composition according to the first alloy composition.
[0115] The sixth preset component mass fraction calculation formula group for calculating the dissolution time of the alloy in the molten steel includes at least:
[0116]
[0117] Where, t alloy Indicates the dissolution time of the alloy in the molten steel, in seconds; C p,A Represents the specific heat capacity of the alloy, in J / (kg·K); ρ A Indicates the density of the alloy in kg / m 3 ;d A represents the average diameter of the alloy particles, in m; h represents the thermal conductivity of the alloy particle surface, in W / (m 2 ·K); T solid Indicates the solidification temperature of molten steel, T M Indicates the temperature of molten steel, T 0 represents the initial temperature of the alloy particles, T s Indicates the solidification temperature of the alloy. The unit of the above temperature is K.
[0118] Since the formula group for calculating the effect of alloy dissolution on the composition of molten steel is prior art, this application will not provide any special explanation here, and those skilled in the art can set the number and types of formulas included in the sixth preset component mass fraction calculation formula group according to actual working conditions.
[0119] Depend on Figure 7 It can be seen from the illustrated embodiments that in the present disclosure, the calculation of alloy effect can be performed before the calculation of molten steel-slag phase effect.
[0120] Through the above calculation process, the change value of melt composition in the six-phase multi-component system of "molten steel-slag phase-inclusions-refractory material-alloy-air" can be obtained.
[0121] In the embodiments of the present disclosure, a solution is also provided for improving the parameters of the preset component mass fraction calculation formula group.
[0122] Figure 8 It is a flow chart of a method for correcting parameters of a preset component mass fraction calculation formula group in one embodiment of the present disclosure.
[0123] refer to Figure 8 , the method 100 may further include:
[0124] Step S801, obtaining actual refining process sampling results corresponding to the set of process parameters, wherein the actual refining process sampling results include actual steel liquid composition, actual inclusion composition, and actual slag phase composition corresponding to multiple time points;
[0125] Step S802, correcting the parameter values of the preset component mass fraction calculation formula group according to the difference between the actual refining process sampling result and the steel liquid component mass fraction time series change curve, the inclusion component mass fraction time series change curve and the slag phase component mass fraction time series change curve at the corresponding time points of the steel liquid composition, inclusion composition and slag phase component mass fraction time series change curve.
[0126] The accuracy of the model can be effectively improved by correcting the model parameters through sampling results from the actual ladle refining process.
[0127] In step S103, in response to a curve viewing instruction from a user, the time series variation curve of the mass fraction of the molten steel component, the time series variation curve of the mass fraction of the inclusion component and the time series variation curve of the mass fraction of the slag phase component are displayed according to the curve viewing instruction.
[0128] In one embodiment of the present disclosure, not only can the component mass fraction time series change curves be provided according to the molten steel, inclusions, and slag phase (where each category includes component mass fraction change curves of multiple components), but one or more of the following curves can also be displayed in response to the user's curve viewing quality: reaction temperature time series change curve, mass fraction of each component in the molten steel with temperature change curve, mass fraction of each component in the inclusions with temperature change curve, mass fraction of each component in the slag phase with temperature change curve, mass fraction of each component in the molten steel with gas pressure change curve, mass fraction of each component in the inclusions with gas pressure change curve, mass fraction of each component in the slag phase with gas pressure change curve, so as to facilitate the multi-dimensional display of the output results of the model, so as to facilitate the user to better analyze the effect of the input value. The above curve types are only examples. In practical applications, more dimensional display methods can be provided, and the present disclosure is not limited to this.
[0129] In addition, it is also possible to respond to user requirements to obtain preset indicators input by the user. When the user inputs multiple sets of process parameters, or when multiple sets of process parameters are generated according to user requests, the component mass fraction time-series change curves corresponding to the multiple sets of process parameters are obtained, and then the preferred process parameters are determined based on the preset indicators and the component mass fraction time-series change curves corresponding to the multiple sets of process parameters.
[0130] For example, the user can input the purity value of the molten steel and multiple sets of process parameters. At this time, the time series change curves of the mass fractions of the molten steel components corresponding to the multiple sets of process parameters are automatically calculated.
[0131] If the user sets the reaction time, the time series variation curve of the mass fraction of the molten steel component that reaches the steel liquid purity value within the specified reaction time can be automatically selected, and the process parameters corresponding to the time series variation curve of the mass fraction of the component, the time when the steel liquid purity reaches the steel liquid purity value, and the highest steel liquid purity within the specified reaction time can be determined.
[0132] If the user does not set the reaction time, the time series change curves of the mass fraction of the molten steel components corresponding to multiple sets of process parameters can be calculated according to the preset multiple reaction times, and the time when the time series change curves of the mass fraction of the molten steel components reach the value of the purity of the molten steel can be determined, and the time and process parameters corresponding to the time series change curves of the mass fraction of the component reaching the value of the purity of the molten steel can be returned to the user for the user to select.
[0133] Of course, the user may also input different types of preset indicators, and accordingly, different screening may be performed according to different types of preset indicators, and the present disclosure does not impose any special restrictions on this.
[0134] Corresponding to the above method embodiments, the present disclosure also provides a melt composition analysis device for a ladle refining process, which can be used to execute the above method embodiments.
[0135] Fig. 9 A block diagram schematically shows a melt composition analysis device for a ladle refining process according to an exemplary embodiment of the present disclosure.
[0136] refer to Fig. 9 , the melt composition analysis device 900 may include:
[0137] An input module 901 is configured to obtain process parameters in response to a data input message from a user, wherein the process parameters include at least reaction vessel size, reaction time, reaction temperature, jet pressure, jet flow rate, initial composition of molten steel, initial composition of inclusions, initial composition of slag phase, and initial mass of refractory materials;
[0138] A calculation module 902 is configured to determine a time series variation curve of the mass fraction of a molten steel component, a time series variation curve of the mass fraction of an inclusion component, and a time series variation curve of the mass fraction of a slag phase component according to the process parameters and a preset group of calculation formulas for the mass fraction of a component;
[0139] The curve display module 903 is configured to respond to a curve viewing instruction from a user and display the steel liquid component mass fraction time series variation curve, the inclusion component mass fraction time series variation curve and the slag phase component mass fraction time series variation curve according to the curve viewing instruction.
[0140] In an exemplary embodiment of the present disclosure, the calculation module 902 is configured to: determine volume parameters according to the initial composition of the molten steel, the initial composition of the inclusions, the initial composition of the slag phase and the initial mass of the refractory material, the volume parameters at least including the volume of the molten steel, the volume of the inclusions, the number of inclusions of different diameters, the volume of the slag phase and the volume of the refractory material; determine contact area parameters according to the size of the reaction vessel and the volume parameters, the contact area parameters at least including the contact area between the molten steel and the slag phase, the contact area between the molten steel and the inclusions, the contact area between the molten steel and the refractory material, and the contact area between the refractory material and the slag phase; bring the volume parameters and the contact area parameters into a preset component mass fraction calculation formula group to determine the molten steel composition, inclusion composition and slag phase composition corresponding to multiple time points; determine the molten steel component mass fraction time series change curve, the inclusion component mass fraction time series change curve and the slag phase component mass fraction time series change curve according to the molten steel composition, inclusion composition and slag phase composition corresponding to multiple time points.
[0141] In an exemplary embodiment of the present disclosure, the calculation module 902 is configured to: determine the current molten steel composition, the current slag phase composition, the current inclusion composition, and the current refractory material mass, and in the first calculation, the current molten steel composition, the current slag phase composition, the current inclusion composition, and the current refractory material mass are respectively equal to the initial composition of the molten steel, the initial composition of the slag phase, the initial composition of the inclusions, and the initial mass of the refractory material; determine the mass fraction of each component on the molten steel-slag phase interface corresponding to the current molten steel composition according to the volume parameter and the contact area parameter; determine the first molten steel composition and the first slag phase composition according to the first preset component mass fraction calculation formula group and the mass fraction of each component on the molten steel-slag phase interface corresponding to the current molten steel composition, the current slag phase composition, and the current molten steel composition; determine the mass fraction of each component on the molten steel-inclusion interface corresponding to the first molten steel composition according to the first molten steel composition and the current inclusion composition; determine the mass fraction of each component on the molten steel-inclusion interface corresponding to the first molten steel composition according to the second preset component mass fraction calculation formula group and the first molten steel composition, the current inclusion composition, and the first molten steel composition corresponding to the first molten steel composition. The second molten steel composition and the first inclusion composition are determined according to the mass fraction of each component on the molten steel-inclusion interface; the third molten steel composition, the first mass of the refractory material, and the second slag phase composition formed by the dissolution of the refractory material into the molten steel and the slag phase and the reaction of the refractory material with the molten steel are determined according to the third preset component mass fraction calculation formula group and the current mass of the refractory material; the mass proportion of oxygen element in the molten steel under the influence of the secondary oxidation reaction of air on the molten steel is determined according to the fourth preset component mass fraction calculation formula group and the third molten steel composition, contact area parameters, jet pressure, jet flow rate, and reaction temperature; the floating removal reaction of the inclusions is calculated according to the fifth preset component mass fraction calculation formula group to determine the second inclusion composition and the third slag phase composition under the floating condition; the current molten steel composition is updated according to the third molten steel composition and the oxygen mass proportion, the current inclusion composition is updated according to the second inclusion composition, the current slag phase composition is updated according to the third slag phase composition, and the current refractory material mass is updated according to the first mass of the refractory material.
[0142] In an exemplary embodiment of the present disclosure, the process parameters also include the initial composition of the alloy, and the calculation module 902 is set to: determine the current alloy composition, which is equal to the initial composition of the alloy during the first calculation; determine the fourth molten steel composition and the first alloy composition according to the sixth preset component mass fraction calculation formula group and the current alloy composition and the current molten steel composition; determine the first molten steel composition and the first slag phase composition according to the first preset component mass fraction calculation formula group and the fourth molten steel composition, the current slag phase composition, and the mass fraction of each component on the molten steel-slag phase interface corresponding to the current molten steel composition; and update the current alloy composition according to the first alloy composition.
[0143] In an exemplary embodiment of the present disclosure, a parameter correction module 904 is also included, which is configured to: obtain the actual refining process sampling results corresponding to the group of process parameters, the actual refining process sampling results including the measured molten steel composition, measured inclusion composition, and measured slag phase composition corresponding to multiple time points; and correct the parameter values of the preset component mass fraction calculation formula group according to the difference between the actual refining process sampling results and the molten steel composition, inclusion composition, and slag phase composition at the time points corresponding to the time series change curve of the molten steel component mass fraction, the time series change curve of the inclusion component mass fraction, and the time series change curve of the slag phase component mass fraction.
[0144] In an exemplary embodiment of the present disclosure, it also includes a numerical screening module 905, which is configured to: obtain the time-series change curves of the mass fraction of the molten steel components, the time-series change curves of the mass fraction of the inclusion components, and the time-series change curves of the mass fraction of the slag phase components corresponding to multiple sets of process parameters; determine the preferred process parameters according to preset indicators and the time-series change curves of the mass fraction of the molten steel components, the time-series change curves of the mass fraction of the inclusion components, and the time-series change curves of the mass fraction of the slag phase components corresponding to multiple sets of process parameters.
[0145] In an exemplary embodiment of the present disclosure, the curve display module 903 is configured to perform at least one of the following display methods: displaying the curve of mass fraction of each component in the molten steel varying with temperature; displaying the curve of mass fraction of each component in the inclusions varying with temperature; displaying the curve of mass fraction of each component in the slag phase varying with temperature; displaying the curve of mass fraction of each component in the molten steel varying with gas pressure; displaying the curve of mass fraction of each component in the inclusions varying with gas pressure; displaying the curve of mass fraction of each component in the slag phase varying with gas pressure; displaying the curve of time series change of melt temperature.
[0146] Since the functions of the device 900 have been described in detail in the corresponding method embodiments, the present disclosure will not elaborate on them here.
[0147] It should be noted that, although several modules or units of the device for action execution are mentioned in the above detailed description, this division is not mandatory. In fact, according to the embodiments of the present disclosure, the features and functions of two or more modules or units described above can be embodied in one module or unit. On the contrary, the features and functions of one module or unit described above can be further divided into multiple modules or units to be embodied.
[0148] In an exemplary embodiment of the present disclosure, an electronic device capable of implementing the above method is also provided.
[0149] It will be appreciated by those skilled in the art that various aspects of the present invention may be implemented as a system, method or program product. Therefore, various aspects of the present invention may be specifically implemented in the following forms, namely: a complete hardware implementation, a complete software implementation (including firmware, microcode, etc.), or a combination of hardware and software, which may be collectively referred to herein as a "circuit", "module" or "system".
[0150] Refer to the following Fig.10 The electronic device 1000 according to this embodiment of the present invention will be described. Fig.10 The electronic device 1000 shown is only an example and should not bring any limitation to the functions and scope of use of the embodiments of the present invention.
[0151] like Fig.10 As shown, the electronic device 1000 is in the form of a general computing device. The components of the electronic device 1000 may include but are not limited to: the at least one processing unit 1010, the at least one storage unit 1020, and a bus 1030 connecting different system components (including the storage unit 1020 and the processing unit 1010).
[0152] The storage unit stores program codes, which can be executed by the processing unit 1010, so that the processing unit 1010 performs the steps according to various exemplary embodiments of the present invention described in the above “Exemplary Method” section of this specification. For example, the processing unit 1010 can perform the following steps: Figure 1 Follow the steps shown in .
[0153] The storage unit 1020 may include a readable medium in the form of a volatile storage unit, such as a random access storage unit (RAM) 10201 and / or a cache storage unit 10202 , and may further include a read-only storage unit (ROM) 10203 .
[0154] The storage unit 1020 may also include a program / utility 10204 having a set (at least one) of program modules 10205, such program modules 10205 including but not limited to: an operating system, one or more application programs, other program modules, and program data, each of which or some combination may include an implementation of a network environment.
[0155] Bus 1030 may represent one or more of several types of bus structures, including a memory unit bus or memory unit controller, a peripheral bus, an accelerated graphics port, a processing unit, or a local bus using any of a variety of bus architectures.
[0156] The electronic device 1000 may also communicate with one or more external devices 1100 (e.g., keyboards, pointing devices, Bluetooth devices, etc.), may also communicate with one or more devices that enable a user to interact with the electronic device 1000, and / or may communicate with any device that enables the electronic device 1000 to communicate with one or more other computing devices (e.g., routers, modems, etc.). Such communication may be performed via an input / output (I / O) interface 1050. Furthermore, the electronic device 1000 may also communicate with one or more networks (e.g., a local area network (LAN), a wide area network (WAN), and / or a public network, such as the Internet) via a network adapter 1060. As shown, the network adapter 1060 communicates with other modules of the electronic device 1000 via a bus 1030. It should be understood that, although not shown in the figure, other hardware and / or software modules may be used in conjunction with the electronic device 1000, including but not limited to: microcode, device drivers, redundant processing units, external disk drive arrays, RAID systems, tape drives, and data backup storage systems.
[0157] Through the description of the above implementation, it is easy for those skilled in the art to understand that the example implementation described here can be implemented by software, or by software combined with necessary hardware. Therefore, the technical solution according to the implementation of the present disclosure can be embodied in the form of a software product, which can be stored in a non-volatile storage medium (which can be a CD-ROM, a USB flash drive, a mobile hard disk, etc.) or on a network, including several instructions to enable a computing device (which can be a personal computer, a server, a terminal device, or a network device, etc.) to execute the method according to the implementation of the present disclosure.
[0158] In an exemplary embodiment of the present disclosure, a computer-readable storage medium is also provided, on which a program product capable of implementing the above method of the present specification is stored. In some possible implementations, various aspects of the present invention can also be implemented in the form of a program product, which includes a program code, and when the program product is run on a terminal device, the program code is used to enable the terminal device to execute the steps according to various exemplary embodiments of the present invention described in the above "Exemplary Method" section of the present specification.
[0159] The program product for implementing the above method according to an embodiment of the present invention can adopt a portable compact disk read-only memory (CD-ROM) and include program code, and can be run on a terminal device, such as a personal computer. However, the program product of the present invention is not limited thereto, and in this document, a readable storage medium can be any tangible medium containing or storing a program, which can be used by or in combination with an instruction execution system, an apparatus or a device.
[0160] The program product may use any combination of one or more readable media. The readable medium may be a readable signal medium or a readable storage medium. The readable storage medium may be, for example, but not limited to, an electrical, magnetic, optical, electromagnetic, infrared, or semiconductor system, device or device, or any combination of the above. More specific examples (non-exhaustive list) of readable storage media include: an electrical connection with one or more wires, a portable disk, a hard disk, a random access memory (RAM), a read-only memory (ROM), an erasable programmable read-only memory (EPROM or flash memory), an optical fiber, a portable compact disk read-only memory (CD-ROM), an optical storage device, a magnetic storage device, or any suitable combination of the above.
[0161] Computer readable signal media may include data signals propagated in baseband or as part of a carrier wave, in which readable program code is carried. Such propagated data signals may take a variety of forms, including but not limited to electromagnetic signals, optical signals, or any suitable combination of the above. Readable signal media may also be any readable medium other than a readable storage medium, which may send, propagate, or transmit a program for use by or in conjunction with an instruction execution system, apparatus, or device.
[0162] The program code embodied on the readable medium may be transmitted using any appropriate medium, including but not limited to wireless, wired, optical cable, RF, etc., or any suitable combination of the foregoing.
[0163] Program code for performing the operations of the present invention may be written in any combination of one or more programming languages, including object-oriented programming languages such as Java, C++, etc., and conventional procedural programming languages such as "C" or similar programming languages. The program code may be executed entirely on the user computing device, partially on the user device, as a separate software package, partially on the user computing device and partially on a remote computing device, or entirely on a remote computing device or server. In cases involving a remote computing device, the remote computing device may be connected to the user computing device through any type of network, including a local area network (LAN) or a wide area network (WAN), or may be connected to an external computing device (e.g., through the Internet using an Internet service provider).
[0164] In addition, the above-mentioned figures are only schematic illustrations of the processes included in the method according to an exemplary embodiment of the present invention, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.
[0165] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the invention disclosed herein. This application is intended to cover any variations, uses, or adaptations of the present disclosure that follow the general principles of the present disclosure and include common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The specification and examples are to be considered exemplary only, and the true scope and concept of the present disclosure are indicated by the claims.
Claims
1. A melt composition analysis method for ladle refining process, characterized in that: include: Acquiring process parameters in response to a data input message from a user, wherein the process parameters include at least reaction vessel size, reaction time, reaction temperature, jet pressure, jet flow rate, initial composition of molten steel, initial composition of inclusions, initial composition of slag phase, and initial quality of refractory materials; Determine the time series variation curve of the mass fraction of the molten steel components, the time series variation curve of the mass fraction of the inclusion components, and the time series variation curve of the mass fraction of the slag phase components according to the process parameters and the preset component mass fraction calculation formula group; In response to a curve viewing instruction from a user, displaying the steel liquid component mass fraction time series variation curve, the inclusion component mass fraction time series variation curve, and the slag phase component mass fraction time series variation curve according to the curve viewing instruction; Wherein, the determining of the steel liquid component mass fraction time series change curve, the inclusion component mass fraction time series change curve and the slag phase component mass fraction time series change curve according to the process parameters and the preset component mass fraction calculation formula group comprises: Determining volume parameters according to the initial composition of the molten steel, the initial composition of the inclusions, the initial composition of the slag phase and the initial mass of the refractory material, wherein the volume parameters at least include the volume of the molten steel, the volume of the inclusions, the number of inclusions of different diameters, the volume of the slag phase and the volume of the refractory material; Determining contact area parameters according to the size of the reaction vessel and the volume parameter, wherein the contact area parameters at least include the contact area between the molten steel and the slag phase, the contact area between the molten steel and the inclusions, the contact area between the molten steel and the refractory material, and the contact area between the refractory material and the slag phase; Substituting the volume parameter and the contact area parameter into the preset component mass fraction calculation formula group to determine the molten steel composition, inclusion composition, and slag phase composition corresponding to multiple time points; The molten steel component mass fraction time series variation curve, the inclusion component mass fraction time series variation curve and the slag phase component mass fraction time series variation curve are determined according to the molten steel components, inclusion components and slag phase components corresponding to the multiple time points.
2. The melt composition analysis method according to claim 1, characterized in that: The step of bringing the volume parameter and the contact area parameter into the preset component mass fraction calculation formula group to determine the molten steel composition, inclusion composition, and slag phase composition corresponding to multiple time points includes: Determine the current molten steel composition, the current slag phase composition, the current inclusion composition, and the current refractory material mass, wherein in the first calculation, the current molten steel composition, the current slag phase composition, the current inclusion composition, and the current refractory material mass are equal to the initial composition of the molten steel, the initial composition of the slag phase, the initial composition of the inclusion, and the initial mass of the refractory material, respectively; Determine the mass fraction of each component on the molten steel-slag interface corresponding to the current molten steel composition according to the volume parameter and the contact area parameter; Determine the first molten steel composition and the first slag phase composition according to the first preset component mass fraction calculation formula group and the current molten steel composition, the current slag phase composition, and the mass fractions of each component on the molten steel-slag phase interface corresponding to the current molten steel composition; Determine the mass fraction of each component on the molten steel-inclusion interface corresponding to the first molten steel composition according to the first molten steel composition and the current inclusion composition; Determine the second molten steel composition and the first inclusion composition according to the second preset component mass fraction calculation formula group and the first molten steel composition, the current inclusion composition, and the mass fraction of each component on the molten steel-inclusion interface corresponding to the first molten steel composition; Determine, according to the third preset component mass fraction calculation formula group and the current mass of the refractory material, a third molten steel component, a first mass of the refractory material, and a second slag phase component formed by the dissolution of the refractory material into the molten steel and the slag phase and the reaction of the refractory material with the molten steel; Determine the mass proportion of oxygen in the molten steel under the influence of the secondary oxidation reaction of air on the molten steel according to the fourth preset component mass fraction calculation formula group and the third molten steel composition, the contact area parameter, the jet pressure, the jet flow rate, and the reaction temperature; Calculating the floating removal reaction of inclusions according to the fifth preset component mass fraction calculation formula group to determine the second inclusion composition and the third slag phase composition under the floating condition; The current molten steel composition is updated according to the third molten steel composition and the oxygen element mass proportion, the current inclusion composition is updated according to the second inclusion composition, the current slag phase composition is updated according to the third slag phase composition, and the current refractory material quality is updated according to the first quality of the refractory material.
3. The melt composition analysis method according to claim 1, characterized in that: The process parameters also include the initial alloy composition, and the first molten steel composition and the first slag phase composition are determined according to the first preset component mass fraction calculation formula group and the current molten steel composition, the current slag phase composition, and the mass fractions of each component on the molten steel-slag phase interface corresponding to the current molten steel composition. The calculation formula group includes: Determining a current alloy composition, wherein the current alloy composition is equal to the initial alloy composition in a first calculation; Determine the fourth molten steel composition and the first alloy composition according to the sixth preset component mass fraction calculation formula group, the current alloy composition, and the current molten steel composition; Determine the first molten steel composition and the first slag phase composition according to the first preset component mass fraction calculation formula group, the fourth molten steel composition, the current slag phase composition, and the mass fractions of each component on the molten steel-slag phase interface corresponding to the current molten steel composition; The current alloy composition is updated according to the first alloy composition.
4. The melt composition analysis method according to claim 1, characterized in that: Also includes: Acquire sampling results of an actual refining process corresponding to the set of process parameters, wherein the sampling results of the actual refining process include measured molten steel composition, measured inclusion composition, and measured slag phase composition corresponding to multiple time points; The parameter values of the preset component mass fraction calculation formula group are corrected according to the differences between the actual refining process sampling results and the steel liquid component mass fraction time series variation curve, the inclusion component mass fraction time series variation curve and the slag phase component mass fraction time series variation curve at corresponding time points.
5. The melt composition analysis method according to claim 1, characterized in that: Also includes: Obtaining the time series variation curves of the mass fraction of the molten steel components, the time series variation curves of the mass fraction of the inclusion components, and the time series variation curves of the mass fraction of the slag phase components corresponding to multiple sets of process parameters; The preferred process parameters are determined according to the preset indicators and the time series variation curves of the mass fraction of the molten steel components, the time series variation curves of the mass fraction of the inclusion components and the time series variation curves of the mass fraction of the slag phase components corresponding to the multiple sets of process parameters.
6. The melt composition analysis method according to claim 1, characterized in that: The curve viewing instruction displays the steel liquid component mass fraction time series change curve, the inclusion component mass fraction time series change curve and the slag phase component mass fraction time series change curve, including at least one of the following methods: Display the curve of mass fraction of each component in molten steel changing with temperature; Display the curve of mass fraction of each component in inclusions changing with temperature; Display the curve of mass fraction of each component in the slag phase changing with temperature; Display the curve of mass fraction of each component in molten steel changing with gas pressure; Display the curve of mass fraction of each component in inclusions changing with gas pressure; Display the curve of mass fraction of each component in the slag phase changing with gas pressure; Display the melt temperature time series change curve.
7. A melt composition analysis device for ladle refining process, characterized in that: include: An input module is configured to obtain process parameters in response to a data input message from a user, wherein the process parameters include at least reaction vessel size, reaction time, reaction temperature, jet pressure, jet flow rate, initial composition of molten steel, initial composition of inclusions, initial composition of slag phase, and initial mass of refractory material; A calculation module is configured to determine a time series variation curve of the mass fraction of the molten steel component, a time series variation curve of the mass fraction of the inclusion component, and a time series variation curve of the mass fraction of the slag phase component according to the process parameters and a preset component mass fraction calculation formula group; A curve display module is configured to respond to a curve viewing instruction from a user and display the steel liquid component mass fraction time series change curve, the inclusion component mass fraction time series change curve and the slag phase component mass fraction time series change curve according to the curve viewing instruction; The calculation module is configured to: determine a volume parameter according to the initial composition of the molten steel, the initial composition of the inclusions, the initial composition of the slag phase, and the initial mass of the refractory material, wherein the volume parameter at least includes the volume of the molten steel, the volume of the inclusions, the number of inclusions of different diameters, the volume of the slag phase, and the volume of the refractory material; determine a contact area parameter according to the size of the reaction container and the volume parameter, wherein the contact area parameter at least includes the contact area between the molten steel and the slag phase, the contact area between the molten steel and the inclusions, the contact area between the molten steel and the refractory material, and the contact area between the refractory material and the slag phase; bring the volume parameter and the contact area parameter into the preset component mass fraction calculation formula group to determine the molten steel composition, inclusion composition, and slag phase composition corresponding to multiple time points; determine the molten steel component mass fraction time series change curve, the inclusion component mass fraction time series change curve, and the slag phase component mass fraction time series change curve according to the molten steel composition, inclusion composition, and slag phase composition corresponding to the multiple time points.
8. An electronic device, characterized in that: include: Memory; as well as A processor coupled to the memory, the processor being configured to execute the melt composition analysis method for ladle refining process according to any one of claims 1 to 6 based on instructions stored in the memory.
9. A computer-readable storage medium having a program stored thereon, wherein when the program is executed by a processor, the melt composition analysis method for ladle refining process according to any one of claims 1 to 6 is implemented.