A core-shell composite negative electrode material, preparation method and application thereof
By using core-shell composite anode material in lithium-ion batteries, using the core and conductive carbon layer structure of sheet-shaped silicon-based and graphite materials, the cyclic stability and conductivity problems of lithium-ion battery anode material are solved, and high capacity and Long-life battery performance.
Patent Information
- Application Number
- CN201910411238.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-05-16
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2039-05-16
AI Technical Summary
Existing lithium-ion battery anode materials such as graphite and silicon-based materials have problems such as low capacity, expansion and crushing, and poor conductivity during the cycle, making it difficult to meet the needs of high energy density and long cycle life.
Core-shell composite anode material is used to form the core through sheet-shaped silicon-based material and sheet-shaped graphite material, and cover the outside with a dense conductive carbon layer to optimize the aspect ratio and particle size distribution to improve binding force, conductivity and circulation stability.
High specific capacity (capacity >400mAh/g), excellent cycle life and electrochemical properties are achieved, reducing material expansion and side reactions, and simplifying the production process.
Smart Images

Figure CN111952550B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the application field of negative electrode materials for lithium-ion batteries, and relates to a composite negative electrode material, a preparation method and application thereof, and in particular to a core-shell type high-capacity long-cycle composite negative electrode material for lithium-ion batteries, a preparation method thereof and a lithium-ion battery comprising the composite material. Background Art
[0002] Lithium-ion batteries have been widely used and closely watched by all parties due to their long cycle life, high specific energy and good safety performance. As a traditional negative electrode material for lithium-ion batteries, graphite material has stable electrochemical properties, but its specific capacity is not high. The theoretical capacity is only 372mAh / g, which cannot meet the increasing demand for high-energy-density lithium-ion batteries in the current market. Silicon-based negative electrode materials have a high theoretical specific capacity, but their volume expansion is large during the process of lithium extraction / insertion, resulting in the fragmentation and pulverization of silicon-based material particles, making the material inactive, and ultimately causing serious attenuation of cycle performance; in addition, the electrical conductivity of silicon-based materials is poor, which affects the material rate performance, etc.
[0003] CN 109273692A discloses a method for preparing a carbon-coated silicon / graphite composite material, comprising: dissolving 5-7 parts of sucrose in 60-70 parts of anhydrous ethanol, stirring and dissolving on a magnetic stirrer, adding 20-30 parts of industrial silicon powder, stirring and dispersing, and then ultrasonically dispersing for 2-3 hours, then placing the mixture in a high-energy ball mill, ball milling at 450r / min for 25-27 hours, drying the ball-milled mixture at a constant temperature of 45-55°C in a vacuum drying oven for 23-25 hours, and then placing it in a tubular furnace in an argon atmosphere. Under protection, the temperature is raised to 580-590℃ at a heating rate of 2℃ / min and calcined for 3.5-4.5h. After natural cooling, a carbon-coated silicon material is obtained; 5-15 parts of the carbon-coated silicon material prepared above and 30-40 parts of natural graphite are added to 75-85 parts of ethanol, ultrasonically dispersed for 2-3h, the obtained mixture is ball-milled at 450r / min for 25-27h, the obtained mixture is stirred and evaporated at 45-55℃, and further vacuum dried at 65-75℃ for 14-16h, and cooled to obtain; each raw material is weight part. The carbon-coated silicon / graphite composite material prepared by this method has good reversible specific capacity, good rate performance and cycle stability, but its performance improvement is limited and it is difficult to meet the needs of practical applications.
[0004] Although the cycling, expansion and rate performance of silicon-based materials can be improved to a certain extent through methods such as silicon-based material nano-sizing, graphite composites, and carbon coating, the disadvantages of silicon-based materials are still quite obvious and their applications are limited. Summary of the invention
[0005] In view of the above-mentioned problems existing in the prior art, the purpose of the present invention is to provide a composite negative electrode material, a preparation method and application thereof, and in particular to a core-shell type high-capacity long-cycle composite negative electrode material for lithium-ion batteries, a preparation method thereof and a lithium-ion battery containing the composite material.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a core-shell type composite negative electrode material, characterized in that the core-shell type composite negative electrode material comprises: an inner core formed by a first active substance and a second active substance, and an outer shell of a carbon coating layer as a third active substance, wherein the first active substance is a flaky silicon-based material, and the second active substance is a flaky graphite material.
[0008] In the core-shell composite negative electrode material provided by the present invention, a flaky silicon-based material and a flaky graphite material form an inner core. Since the flaky silicon-based material particles have a large specific surface area and an irregular morphology, the bonding force and bonding tightness between the silicon-based material particles can be effectively improved, and the composite effect of the silicon-based material and the flaky graphite material can be improved. The flaky silicon-based material and the flaky graphite material have good bonding performance, and the flaky silicon-based material can be dispersed between multiple graphite sheets. The flaky graphite material forms a good conductive network inside the particles, thereby improving the internal conductivity of the material and buffering the expansion of the nano-silicon-based material. A dense conductive carbon layer is coated on the outside of the inner core formed by the two, which can improve the conductivity of the material, further reduce the gaps inside and outside the particles, effectively inhibit the expansion of the material, and reduce the side reactions between the material and the electrolyte.
[0009] As a preferred technical solution of the core-shell composite negative electrode material of the present invention, the aspect ratio of the flaky silicon-based material is 1.5 to 100 and does not include 1.5, such as 1.6, 1.8, 2, 2.5, 2.8, 3, 3.5, 4, 5, 5.5, 6, 8, 10, 15, 20, 23, 26, 30, 35, 40, 45, 50, 60, 65, 70, 80, 85, 90 or 100, etc., and the particle aspect ratio is the ratio of the maximum linear dimension to the minimum linear dimension of the particle. This preferred technical solution can improve its binding property with the flaky graphite material and improve the network structure formed by the two by limiting the aspect ratio of the flaky silicon-based material, thereby better improving the electrochemical performance.
[0010] Preferably, the particle aspect ratio of the flaky silicon-based material is 2-40.
[0011] Preferably, the particle aspect ratio of the flaky graphite material is 2 to 120 and does not contain 2, such as 2.2, 2.5, 3, 3.5, 4, 4.2, 4.6, 5, 5.5, 6, 6.5, 7, 8, 10, 15, 20, 25, 28, 32, 36, 40, 45, 50, 60, 70, 80, 85, 90, 100, 105, 110 or 120, etc., and the particle aspect ratio is the ratio of the maximum linear dimension to the minimum linear dimension of the particle. This preferred technical solution can improve its binding property with the flaky silicon-based material and improve the network structure formed by the two by limiting the type and aspect ratio of the flaky graphite material, thereby better improving the electrochemical performance.
[0012] Preferably, the aspect ratio of the flaky graphite material is 3-50.
[0013] In the present invention, the aspect ratio of the flaky material (such as flaky silicon-based material and flaky graphite material) is the ratio of the maximum linear dimension to the minimum linear dimension of the particle. The maximum linear dimension of the flaky material is the maximum length of the two-dimensional plane of the flaky material, and the minimum linear dimension is the thickness of the flaky material.
[0014] The flaky material and the aspect ratio in the present invention have the following relationship: for silicon-based materials, an aspect ratio of less than 1.5 is a non-flaky silicon-based material; for graphite materials, an aspect ratio of less than 2 is a non-flaky graphite.
[0015] Preferably, the carbon coating layer is converted from an organic carbon source by sintering, for example, using an organic carbon source such as polyester, sugar, organic acid or asphalt, and sintering at 500° C. to 1200° C. in an inert atmosphere to convert the organic carbon source into the carbon coating layer.
[0016] Preferably, the thickness of the carbon coating layer is 0.05 to 3 um, for example, 0.05 um, 0.1 um, 0.2 um, 0.5 um, 1 um, 1.2 um, 1.5 um, 1.8 um, 2 um, 2.4 um, 2.7 um or 3 um.
[0017] As a preferred technical solution of the method of the present invention, the first active material comprises Si, SiO x Or a combination of at least two of Si-M alloys, for example, Si and SiO x Combination of Si and Si-M alloy, SiO x Combination of Si and Si-M alloy, Si, SiO x and a combination of Si-M alloys, wherein 0.5≤x≤1.5, for example, 0.5, 0.7, 0.8, 1, 1.2, 1.3 or 1.5; and M is any one of B, Fe, Cu, Sn, Ge, Ti, Mg, Ni or Ce, or a combination of at least two of them.
[0018] Preferably, in the first active substance, the absolute value of the difference in median particle size of different substances is 50nm to 1500nm, such as 50nm, 100nm, 125nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, 1100nm, 1200nm, 1300nm, 1400nm or 1500nm, etc. Using a combination of large and small particles in accordance with this preferred embodiment can improve the dispersibility of nano-silicon-based materials and reduce agglomeration between particles.
[0019] Preferably, the first active material is composed of Si and SiO in a mass ratio of 0.01 to 100. x The median particle size of Si is 10-300 nm, and SiO x The median particle size of Si is 150-5000nm, and the median particle size of Si is less than that of SiO x The mass ratio is, for example, 0.01, 0.05, 0.1, 0.2, 1, 2, 5, 10, 15, 20, 35, 50, 60, 65, 70, 80, 85, 95 or 100, etc.; the median particle size of Si is, for example, 10 nm, 30 nm, 50 nm, 100 nm, 150 nm, 170 nm, 185 nm, 200 nm, 220 nm, 240 nm, 280 nm or 300 nm, etc.; the SiO x The median particle size is, for example, 150nm, 200nm, 300nm, 400nm, 450nm, 500nm, 600nm, 800nm, 1000nm, 1250nm, 1500nm, 2000nm, 2500nm, 3000nm, 3500nm, 3800nm, 4000nm, 4500nm or 5000nm. This preferred technical solution uses Si with a median particle size of 10 to 300nm. At this particle size, the material has the lowest expansion (when the median particle size of the Si particles is greater than 300nm, the expansion increases sharply), the cycle stability is optimal, and the SiO with its own small expansion is used. x The median particle size is between 150 and 5000 nm. By using a combination of large and small particles, the dispersibility of nano-silicon-based materials is improved, the agglomeration between particles is reduced, the complementary effects are optimal, and the performance is optimal.
[0020] Preferably, the first active material is composed of Si and Si-M alloy in a mass ratio of 0.01 to 100, the median particle size of Si is 10 to 300 nm, the median particle size of Si-M alloy is 150 to 5000 nm, and the median particle size of Si is less than the median particle size of Si-M alloy. The mass ratio is, for example, 0.01, 0.05, 0.1, 0.2, 1, 2, 5, 10, 15, 20, 35, 50, 60, 65, 70, 80, 85, 95 or 100; the median particle size of Si is, for example, 10 nm, 30 nm, 50 nm, 100 nm, 150 nm, 170 nm, 185 nm, 200 nm, 220 nm, 240 nm, 280 nm or 300 nm; the SiO x The median particle size is, for example, 150nm, 200nm, 300nm, 400nm, 450nm, 500nm, 600nm, 800nm, 1000nm, 1250nm, 1500nm, 2000nm, 2500nm, 3000nm, 3500nm, 3800nm, 4000nm, 4500nm or 5000nm. This preferred technical solution uses Si with a median particle size of 10 to 300nm. At this particle size, the material has the lowest expansion and the best cycle stability. It is matched with Si-M alloys with smaller expansion, and the median particle size is 150 to 5000nm. At the same time, the combination of large and small particles is used to improve the dispersibility of nano-silicon-based materials, reduce the agglomeration between particles, and achieve the best complementary effect and the best performance.
[0021] Preferably, the first active material is composed of SiO x With Si-M alloy composition, SiO x The median particle size of the Si-M alloy is 150 to 400 nm (e.g., 150 nm, 170 nm, 185 nm, 200 nm, 220 nm, 240 nm, 280 nm, 300 nm, 350 nm, or 400 nm), the median particle size of the Si-M alloy is 200 to 5000 nm (e.g., 200 nm, 250 nm, 400 nm, 600 nm, 800 nm, 1000 nm, 1250 nm, 1500 nm, 2000 nm, 2500 nm, 3000 nm, 3500 nm, 3800 nm, 4000 nm, 4500 nm, or 5000 nm), and the SiO x The median particle size is less than the median particle size of Si-M alloy. This preferred technical solution uses SiO with a median particle size of 150 to 400 nm. x , combined with Si-M alloy with smaller expansion, the average particle size is 400-5000nm, and the large and small particles are matched at the same time to improve the dispersibility of nano-silicon-based materials, reduce the agglomeration between particles, and achieve the best complementary effect and the best performance.
[0022] Preferably, the first active material is composed of SiOx and Si-M alloy in a mass ratio of 0.01 to 100, the median particle size of the Si-M alloy is 150 to 400 nm (e.g., 150 nm, 170 nm, 185 nm, 200 nm, 220 nm, 240 nm, 280 nm, 300 nm, 350 nm or 400 nm, etc.), SiO x The median particle size is 200 to 5000 nm (e.g., 200 nm, 250 nm, 400 nm, 600 nm, 800 nm, 1000 nm, 1250 nm, 1500 nm, 2000 nm, 2500 nm, 3000 nm, 3500 nm, 3800 nm, 4000 nm, 4500 nm or 5000 nm, etc.) and the median particle size of the Si-M alloy is less than SiO x This preferred technical solution uses Si-M alloy with a median particle size of 150-400nm, combined with SiO x The average particle size is between 400 and 5000 nm. By combining large and small particles, the dispersion of nano-silicon-based materials is improved, the agglomeration between particles is reduced, and the complementary effects are optimal, resulting in the best performance.
[0023] Preferably, the components of the second active material include any one of natural graphite and artificial graphite or a combination of two of them.
[0024] Preferably, the median particle size of the second active substance is 1 to 15 um, for example, 1 um, 2 um, 3 um, 4.5 um, 5 um, 6 um, 8 um, 10 um, 12 um, 13 um or 15 um.
[0025] Preferably, the median particle size of the second active material is larger than that of the first active material, with a difference of 2 μm to 12 μm. Within this preferred range, the dispersibility and bonding of the flaky silicon-based material between graphite sheets can be better improved, which is beneficial to improving the electrochemical performance.
[0026] Preferably, based on the total mass of the core-shell type composite negative electrode material as 100wt%, the mass percentage of the first active substance is 1-70wt%, for example, 1wt%, 3wt%, 5wt%, 8wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 37wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt% or 70wt%, etc.; the mass percentage of the second active substance is 5-60wt%. %, for example, 5wt%, 10wt%, 12wt%, 18wt%, 20wt%, 25wt%, 30wt%, 35wt%, 37wt%, 40wt%, 45wt%, 50wt%, 55wt% or 60wt% etc.; the mass percentage of the third active substance material is 5-50wt%, for example, 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 37wt%, 40wt%, 45wt% or 50wt% etc.
[0027] In a second aspect, the present invention provides a method for preparing the core-shell composite negative electrode material as described in the first aspect, the method comprising the following steps:
[0028] (1) mixing and granulating a first active material and a second active material to obtain a first precursor;
[0029] (2) performing carbon coating modification on the first precursor, and then sintering to obtain a core-shell composite negative electrode material;
[0030] Wherein, the first active material is a flaky silicon-based material, and the second active material is a flaky graphite material.
[0031] As a preferred technical solution of the method of the present invention, the particle aspect ratio of the flaky silicon-based material is 1.5 to 100 and does not include 1.5, and the particle aspect ratio is the ratio of the maximum linear dimension to the minimum linear dimension of the particle.
[0032] Preferably, the specific surface area of the flaky silicon-based material is 50 to 500 m 2 / g, for example 50m 2 / g, 65m 2 / g, 80m 2 / g、100m 2 / g, 125m 2 / g, 150m 2 / g, 200m 2 / g, 240m 2 / g, 270m 2 / g、300m 2 / g, 350m 2 / g, 400m2 / g, 450m 2 / g or 500m 2 / g, etc.
[0033] Preferably, the aspect ratio of the flaky graphite material is 2 to 120 and does not include 2.
[0034] Preferably, the first active material comprises Si, SiO x Or a combination of at least two of Si-M alloys, wherein 0.5≤x≤1.5, and M is any one of B, Fe, Cu, Sn, Ge, Ti, Mg, Ni or Ce, or a combination of at least two of them.
[0035] Preferably, in the first active substance, the absolute value of the difference in median particle diameters of different substances is 50 nm to 1500 nm.
[0036] Preferably, the first active material is composed of Si and SiO in a mass ratio of 0.01 to 100. x The median particle size of Si is 10-300 nm, and SiO x The median particle size of Si is 150-5000nm, and the median particle size of Si is less than that of SiO x Median particle size.
[0037] Preferably, the first active material is composed of Si and Si-M alloy in a mass ratio of 0.01-100, the median particle size of Si is 10-300 nm, the median particle size of Si-M alloy is 150-5000 nm, and the median particle size of Si is less than that of Si-M alloy.
[0038] Preferably, the first active material is composed of SiO x With Si-M alloy composition, SiO x The median particle size of Si-M alloy is 150-400nm, the median particle size of Si-M alloy is 200-5000nm and SiO x The median particle size is less than the median particle size of Si-M alloy.
[0039] Preferably, the first active material is composed of SiOx and Si-M alloy in a mass ratio of 0.01 to 100, the median particle size of the Si-M alloy is 150 to 400 nm, and the SiO x The median particle size is 200-5000nm and the median particle size of Si-M alloy is less than that of SiO x Median particle size.
[0040] Preferably, the first active material is Si, SiO x And Si-M alloy composition, Si and SiO xThe mass ratio of Si to Si-M alloy is 0.02-100, the median particle size of Si is 10-300 nm, and the mass ratio of Si to Si-M alloy is 0.02-100. x The median particle size of Si is 150-5000nm, the median particle size of Si-M alloy is 150-5000nm, and the median particle size of Si is less than that of SiO x Median particle size < median particle size of Si-M alloy;
[0041] Preferably, the first active material is Si, SiO x And Si-M alloy composition, Si and SiO x The mass ratio of Si to Si-M alloy is 0.02-100, the median particle size of Si is 10-300 nm, and the mass ratio of Si to Si-M alloy is 0.02-100. x The median particle size of Si is 150-5000nm, the median particle size of Si-M alloy is 150-5000nm, the median particle size of Si is less than that of Si-M alloy and less than that of SiO x Median particle size.
[0042] Preferably, the components of the second active material include any one of natural graphite and artificial graphite or a combination of two of them.
[0043] Preferably, the median particle size of the second active material is 1 to 15 um.
[0044] As a preferred technical solution of the method of the present invention, the mixing granulation method in step (1) is any one of spray drying, mixing heating or kneading molding.
[0045] Preferably, the carbon coating modification method in step (2) is any one of a liquid phase coating method, a solid phase coating method or a gas phase coating method.
[0046] Preferably, the process steps of the liquid phase coating method include: dispersing the first precursor and the carbon source in an organic solvent system, and drying to obtain the second precursor.
[0047] Preferably, the process steps of the solid phase coating method include: mixing the first precursor and the carbon source in a mixer to obtain the second precursor.
[0048] Preferably, in the liquid phase coating method and the solid phase coating method, the carbon source is independently any one of polyesters, sugars, organic acids or asphalt, or a combination of at least two of them.
[0049] Preferably, the polyesters include any one of phenolic resin, polyethylene terephthalate, polybutylene terephthalate or polyarylate, or a combination of at least two of them. Typical but non-limiting examples of the combination include a combination of phenolic resin and polyethylene terephthalate, a combination of polyethylene terephthalate and polyarylate, a combination of phenolic resin, polybutylene terephthalate and polyarylate, and the like.
[0050] Preferably, the process steps of the gas phase coating method include: in a reaction furnace, using an organic carbon source gas as a coating source, raising the temperature to 500° C. to 1200° C. under the condition of passing an inert gas, and carbon coating the first precursor to obtain the second precursor.
[0051] In the vapor coating method, the temperature is raised to, for example, 500°C, 600°C, 650°C, 700°C, 750°C, 800°C, 900°C, 1000°C, 1100°C, or 1200°C.
[0052] Preferably, in the gas phase coating method, the organic carbon source gas is any one of hydrocarbons or aromatic hydrocarbon derivatives with 1 to 3 benzene rings, or a combination of at least two of them.
[0053] The sintering in step (3) of the present invention is high-temperature sintering.
[0054] Preferably, the sintering in step (3) comprises: placing the second precursor in a reactor, heating it to 500° C. to 1200° C. under the protection of an inert gas, to obtain a core-shell composite negative electrode material.
[0055] During the sintering in step (3), the temperature is raised to, for example, 500°C, 600°C, 650°C, 700°C, 750°C, 800°C, 900°C, 1000°C, 1100°C or 1200°C.
[0056] Preferably, the reactor comprises any one of a vacuum furnace, a box furnace, a rotary kiln, a roller kiln, a pusher kiln or a tubular furnace.
[0057] In a third aspect, the present invention provides a negative electrode, which comprises the core-shell type negative electrode material described in the first aspect.
[0058] In a fourth aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the core-shell composite negative electrode material described in the first aspect.
[0059] It should be noted that the particle aspect ratio described in the present invention is a characteristic of a single particle, which is a different concept from the median particle size. The median particle size is a statistical analysis of the overall particle size distribution. Particles with different aspect ratios can all have their median particle sizes measured using a particle size analyzer. The present invention uses a Malvern particle size analyzer to test the median particle size.
[0060] Compared with the prior art, the present invention has the following beneficial effects:
[0061] (1) In the core-shell composite negative electrode material provided by the present invention, since the flaky silicon-based material particles have a large specific surface area and irregular morphology, the bonding force and bonding tightness between the silicon-based material particles can be effectively improved, and the composite effect between the silicon-based material particles and the flaky graphite material can be improved; the flaky silicon-based material and the flaky graphite material have good bonding performance, and the flaky silicon-based material can be dispersed between multiple graphite sheets. The flaky graphite material forms a good conductive network inside the particles, thereby improving the internal conductivity of the material and buffering the expansion of the nano-silicon-based material. A dense conductive carbon layer is coated on the outside of the inner core formed by the two, which can improve the conductivity of the material, further reduce the gaps inside and outside the particles, effectively inhibit the expansion of the material and reduce the side reactions between the material and the electrolyte.
[0062] (2) The present invention can improve the bonding strength, bonding tightness, conductivity and expansion inhibition of the formed network structure by optimizing the aspect ratio and other parameters of the flaky silicon-based material and the flaky graphite material, so that the core-shell composite negative electrode material can obtain excellent reversible capacity, first efficiency and cycle stability.
[0063] (3) The present invention optimizes the types of flaky silicon-based materials, combines particle size control and type selection, and better utilizes the complementary advantages between materials to improve the electrochemical properties of the materials.
[0064] (4) The core-shell composite negative electrode material of the present invention is used for the negative electrode of lithium ion batteries, and has high specific capacity (capacity>400mAh / g), first efficiency and excellent cycle life. The process of the present invention is simple and easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] Figure 1 This is a schematic diagram of the structure of the composite negative electrode material provided by the present invention, wherein 1 is a first active material, 2 is a second active material, and 3 is a third active material.
[0066] Figure 2 The following are the test results of the negative electrode material X-ray diffractometer of Example 1.
[0067] Figure 3 The following is a cycle curve obtained by testing a battery made of the negative electrode material of Example 1. DETAILED DESCRIPTION
[0068] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0069] The negative electrode materials of each embodiment and comparative example were tested using the following method:
[0070] ① Use X′Pert Pro X-ray diffractometer and PANalytical to test the structure of the material.
[0071] ② Use the following method to test the initial charge and discharge performance:
[0072] The negative electrode materials, acetylene black, CMC and SBR of each embodiment and comparative example were dispersed in pure water in a mass ratio of 90:5:2.5:2.5 and mixed. The obtained mixed slurry was coated on a copper foil current collector and vacuum dried to obtain a negative electrode sheet. Then, 1 mol / L LiPF6 / EC+DMC+EMC (v / v=1:1:1) electrolyte, SK (12 μm) separator and casing were assembled into CR2016 button batteries by conventional processes, and the electrochemical properties were tested at a current density of 0.1C.
[0073] ③ Use the following method to test the cycle performance:
[0074] The negative electrode material, acetylene black, CMC, and SBR were dispersed in pure water at a mass ratio of 95:2:1.5:1.5, mixed, coated on a copper foil current collector, and vacuum dried to obtain a negative electrode plate; then the ternary positive electrode plate (NCM811) prepared by the traditional mature process, 1mol / L LiPF6 / EC+DMC+EMC (v / v=1:1:1) electrolyte, SK (12μm) diaphragm, and shell were assembled using conventional production processes to assemble 18650 cylindrical single cells. The charge and discharge test of the cylindrical battery was carried out on the LAND battery test system of Wuhan Jinnuo Electronics Co., Ltd., at room temperature, constant current charge and discharge at a rate of 1C, and the charge and discharge voltage was limited to 2.75-4.2V. The test results are shown in Table 1.
[0075] Example 1
[0076] This embodiment provides a core-shell composite negative electrode material and a preparation method thereof, the method comprising the following steps:
[0077] (1) The flaky silicon with a median particle size of 80 nm and an aspect ratio of 8 and the flaky SiO with a median particle size of 400 nm and an aspect ratio of 3 were 0.98 and flake natural graphite with a median particle size of 5 μm and an aspect ratio of 10 in a mass ratio of 30:30:40 to obtain a precursor A;
[0078] (2) Precursor A and glucose are dispersed in ethanol at a mass ratio of 70:30, and dried to obtain precursor B;
[0079] (3) Precursor B was placed in a box furnace, nitrogen was introduced, and the temperature was raised to 800° C. to obtain a core-shell composite negative electrode material with a carbon coating layer thickness of 0.5 μm.
[0080] The core-shell composite negative electrode material obtained in this embodiment includes: a core formed by a first active material and a second active material, and a carbon coating layer shell, wherein the first active material is a silicon-based material, specifically flaky silicon and flaky SiO 0.98 The second active material is flaky natural graphite, and the third active material is a dense carbon coating shell obtained by converting glucose.
[0081] Figure 2 This is the test result of the negative electrode material X-ray diffractometer of Example 1. The characteristic peaks of silicon, silicon dioxide and graphite can be seen from the figure.
[0082] Figure 3 The cycle curve of the battery made of the negative electrode material of Example 1 and tested is obtained. As can be seen from the figure, it can be seen that the material has excellent cycle performance and the capacity retention rate after 600 cycles is 90.2%.
[0083] Example 2
[0084] This embodiment provides a core-shell composite negative electrode material and a preparation method thereof, the method comprising the following steps:
[0085] (1) flake silicon with a median particle size of 200 nm and an aspect ratio of 25, flake Si-Fe alloy with a median particle size of 900 nm and an aspect ratio of 7.0, and flake artificial graphite with a median particle size of 8 μm and an aspect ratio of 3 are mixed and heated in a mass ratio of 45:5:50 to obtain a precursor A;
[0086] (2) Precursor A and asphalt are mixed in a mixer at a mass ratio of 80:20 to obtain precursor B;
[0087] (3) Precursor B is placed in a tube furnace, argon gas is introduced, and the temperature is raised to 900° C. to obtain a core-shell composite negative electrode material with a carbon coating layer thickness of 0.3 μm.
[0088] Example 3
[0089] This embodiment provides a core-shell composite negative electrode material and a preparation method thereof, the method comprising the following steps:
[0090] (1) SiO2 with a median particle size of 200 nm and an aspect ratio of 4 1.05 , a flake Si-Cu alloy with a median particle size of 600 nm and an aspect ratio of 10 and a flake natural graphite with a median particle size of 10 μm and an aspect ratio of 21 were spray dried in a mass ratio of 30:35:35 to obtain a precursor A;
[0091] (2) Precursor A is placed in a rotary furnace, acetylene gas is introduced, and the precursor B is obtained by deposition at 800°C for 2 h;
[0092] (3) Precursor B was placed in a roller kiln, nitrogen was introduced, and the temperature was raised to 700° C. to obtain a core-shell composite negative electrode material with a carbon coating layer thickness of 0.1 μm.
[0093] Example 4
[0094] This embodiment provides a core-shell composite negative electrode material and a preparation method thereof, the method comprising the following steps:
[0095] (1) Si-Ni alloy flakes with a median particle size of 250 nm and an aspect ratio of 12, SiO flakes with a median particle size of 300 nm and an aspect ratio of 6 1.0 and flake artificial graphite with a median particle size of 3 μm and an aspect ratio of 15 in a mass ratio of 35:15:60 to obtain a precursor A;
[0096] (2) Precursor A and phenolic resin are mixed in a mixer at a mass ratio of 85:15 to obtain precursor B;
[0097] (3) Precursor B was placed in a vacuum furnace, nitrogen was introduced, and the temperature was raised to 980° C. to obtain a core-shell composite negative electrode material with a carbon coating layer thickness of 0.3 μm.
[0098] Example 5
[0099] This embodiment provides a core-shell composite negative electrode material and a preparation method thereof, the method comprising the following steps:
[0100] (1) Si flakes with a median particle size of 200 nm and an aspect ratio of 8 and SiO flakes with a median particle size of 3 μm and an aspect ratio of 5 were prepared. 1.25 and flake artificial graphite with a median particle size of 10 μm and an aspect ratio of 5 were spray-dried at a mass ratio of 15:25:60 to obtain precursor A;
[0101] (2) Precursor A and sucrose are dispersed in ethanol at a mass ratio of 80:20, and dried to obtain precursor B;
[0102] (3) Precursor B was placed in a tube furnace, nitrogen was introduced, and the temperature was raised to 1000° C. to obtain a core-shell composite negative electrode material with a carbon coating layer thickness of 0.4 μm.
[0103] Example 6
[0104] This embodiment provides a core-shell composite negative electrode material and a preparation method thereof, the method comprising the following steps:
[0105] (1) Si flakes with a median particle size of 50 nm and an aspect ratio of 35 and SiO flakes with a median particle size of 400 nm and an aspect ratio of 6 0.9, a flake Si-Ti alloy with a median particle size of 700 nm and an aspect ratio of 18 and a flake natural graphite with a median particle size of 8 μm and an aspect ratio of 40 were spray dried in a mass ratio of 25:10:15:50 to obtain a precursor A;
[0106] (2) Precursor A and asphalt are mixed in a mixer at a mass ratio of 65:35 to obtain precursor B;
[0107] (3) Precursor B was placed in a roller kiln, nitrogen was introduced, and the temperature was raised to 650° C. to obtain a core-shell composite negative electrode material with a carbon coating layer thickness of 0.8 μm.
[0108] Example 7
[0109] This embodiment provides a core-shell composite negative electrode material and a preparation method thereof, the method comprising the following steps:
[0110] (1) Si flakes with a median particle size of 150 nm and an aspect ratio of 15, Si-Fe alloy flakes with a median particle size of 300 nm and an aspect ratio of 12, SiO flakes with a median particle size of 800 nm and an aspect ratio of 20, 0.85 and flake artificial graphite with a median particle size of 5 μm and an aspect ratio of 10 were spray-dried at a mass ratio of 15:35:15:45 to obtain precursor A;
[0111] (2) Precursor A and sucrose are dispersed in ethanol at a mass ratio of 85:15, and dried to obtain precursor B;
[0112] (3) Precursor B was placed in a tube furnace, nitrogen was introduced, and the temperature was raised to 850° C. to obtain a core-shell composite negative electrode material with a carbon coating layer thickness of 0.3 μm.
[0113] Example 8
[0114] This embodiment provides a core-shell composite negative electrode material and a preparation method thereof, which is different from Embodiment 1 in that:
[0115] The flaky natural graphite with a median particle size of 5 μm and an aspect ratio of 10 was replaced by the flaky natural graphite with a median particle size of 1.5 μm and an aspect ratio of 10, and the rest was the same as in Example 1.
[0116] Example 9
[0117] This embodiment provides a core-shell composite negative electrode material and a preparation method thereof, which is different from Embodiment 1 in that:
[0118] The flaky natural graphite with a median particle size of 5 μm and an aspect ratio of 10 was replaced by the flaky natural graphite with a median particle size of 14 μm and an aspect ratio of 10, and the rest was the same as in Example 1.
[0119] Example 10
[0120] A high-capacity composite negative electrode material was prepared in a method substantially the same as that in Example 1, except that nano-silicon and SiO 0.98 The median particle size is 400 nm. The battery is manufactured in the same manner as in Example 1.
[0121] Embodiment 11
[0122] A high-capacity composite negative electrode material was prepared in a method substantially the same as in Example 1, the difference from Example 1 being that the silicon-based material was flaky silicon with a median particle size of 80 nm and an aspect ratio of 8; and a battery was manufactured in a method substantially the same as in Example 1.
[0123] Comparative Example 1
[0124] A high-capacity composite negative electrode material was prepared in a method substantially the same as that in Example 1, except that the silicon-based material was non-flaky nano-silicon and non-flaky SiO 0.98 , nano-silicon and SiO 0.98 The aspect ratio is 1.1; the battery is manufactured in the same manner as in Example 1.
[0125] Comparative Example 2
[0126] A high-capacity composite negative electrode material was prepared in a method substantially the same as in Example 1, except that natural graphite was non-flaky graphite with an aspect ratio of 1.2. A battery was manufactured in a method substantially the same as in Example 1.
[0127] Table 1
[0128]
[0129]
[0130] The negative electrode materials of various embodiments of the present invention have high specific capacity, high efficiency and excellent cycle life.
[0131] By comparing Example 1 with Example 8, it can be seen that the difference in median particle size between graphite and silicon-based material in Example 8 is less than 2 μm, the dispersion effect of silicon-based material and graphite material deteriorates, the agglomeration of silicon-based particles increases, the buffering effect of graphite weakens, and the cycle performance deteriorates.
[0132] By comparing Example 1 with Example 9, it can be seen that the difference in median particle size between graphite and silicon-based material in Example 9 is greater than 12 μm, the particle granulation effect deteriorates, the dispersion effect of silicon-based material and graphite material deteriorates, the agglomeration of silicon-based particles increases, the graphite conductive network inside the particles weakens, and the cycle performance deteriorates.
[0133] Comparison between Example 1 and Example 10 shows that in Example 10, silicon with a diameter greater than 300 nm is used, resulting in greater material expansion, and the Si and SiO0.98 The median particle size is the same, and the agglomeration is more serious, resulting in poor internal dispersion of the particles, increased local expansion, and ultimately a sharp decline in cycle performance.
[0134] By comparing Example 1 with Example 11, it can be seen that only a single silicon is used in Example 11. Although the capacity efficiency is improved, the material expands greatly, agglomerates more seriously, and the internal dispersion of the particles is poor, which ultimately leads to a sharp decline in cycle performance.
[0135] In Comparative Example 1, a non-flaky silicon-based material with an aspect ratio of less than 1.5 is used as the first active material, which results in loose bonding inside the particles and poor composite effect with graphite, thereby increasing the specific surface area and reducing the first efficiency. During the cycle, the electrolyte penetrates into the particles, reacts with the internal materials, continuously consumes the electrolyte and active materials, and ultimately causes poor cycle performance.
[0136] In Comparative Example 2, non-flaky graphite with an aspect ratio of less than 2 is used as a carrier, and the dispersibility of the silicon-based material is significantly deteriorated, resulting in serious agglomeration of the silicon-based material, poor internal conductivity, and a significant reduction in the buffering effect of the graphite material, which ultimately leads to increased material expansion and poor circulation.
[0137] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A core-shell composite negative electrode material, It is characterized in that The core-shell composite negative electrode material comprises: a core formed by a first active material and a second active material, and a carbon coating layer shell as a third active material, the first active material is a flaky silicon-based material, the second active material is a flaky graphite material; the flaky silicon-based material is dispersed between a plurality of flaky graphite material sheets; The particle aspect ratio of the flaky silicon-based material is 1.5 to 100 and does not include 1.5; The particle aspect ratio of the flaky graphite material is 2 to 120 and does not include 2; the particle aspect ratio is the ratio of the maximum linear dimension to the minimum linear dimension of the particle, the maximum linear dimension of the flaky material is the maximum length of the two-dimensional plane of the flaky material, and the minimum linear dimension is the thickness of the flaky material.
2. The core-shell composite negative electrode material according to claim 1, It is characterized in that The particle aspect ratio of the flaky silicon-based material is 2-40.
3. The core-shell composite negative electrode material according to claim 1, It is characterized in that The aspect ratio of the flaky graphite material is 3-50.
4. The core-shell composite negative electrode material according to claim 1, It is characterized in that The carbon coating layer is converted from an organic carbon source through sintering.
5. The core-shell composite negative electrode material according to claim 1, It is characterized in that The thickness of the carbon coating layer is 0.05-3 um.
6. The core-shell composite negative electrode material according to claim 1, It is characterized in that The first active material comprises Si, SiO x Or a combination of at least two of Si-M alloys, wherein 0.5≤x≤1.5, and M is any one of B, Fe, Cu, Sn, Ge, Ti, Mg, Ni or Ce, or a combination of at least two of them.
7. The core-shell composite negative electrode material according to claim 1, It is characterized in that In the first active material, the absolute value of the difference in median particle diameters of different materials is 50 nm to 1500 nm.
8. The core-shell composite negative electrode material according to claim 1, It is characterized in that The first active material is composed of Si and SiO in a mass ratio of 0.01 to 100. x The median particle size of Si is 10-300 nm, and SiO x The median particle size of Si is 150-5000nm, and the median particle size of Si is less than that of SiO x Median particle size.
9. The core-shell composite negative electrode material according to claim 1, It is characterized in that The first active material is composed of Si and Si-M alloy in a mass ratio of 0.01-100, the median particle size of Si is 10-300nm, the median particle size of Si-M alloy is 150-5000nm, and the median particle size of Si is less than the median particle size of Si-M alloy.
10. The core-shell composite negative electrode material according to claim 1, It is characterized in that The first active material is composed of SiO x With Si-M alloy composition, SiO x The median particle size of Si-M alloy is 150-400nm, the median particle size of Si-M alloy is 200-5000nm and SiO x The median particle size is less than the median particle size of Si-M alloy.
11. The core-shell composite negative electrode material according to claim 1, It is characterized in that The first active material is composed of SiOx and Si-M alloy in a mass ratio of 0.01 to 100, the median particle size of the Si-M alloy is 150 to 400 nm, and the SiO x The median particle size is 200-5000nm and the median particle size of Si-M alloy is less than that of SiO x Median particle size.
12. The core-shell composite negative electrode material according to claim 1, It is characterized in that The first active material is composed of Si, SiO x And Si-M alloy composition, Si and SiO x The mass ratio of Si to Si-M alloy is 0.02-100, the median particle size of Si is 10-300 nm, and the mass ratio of Si to Si-M alloy is 0.02-100. x The median particle size of Si is 150-5000nm, the median particle size of Si-M alloy is 150-5000nm, and the median particle size of Si is less than that of SiO x The median particle size is less than the median particle size of Si-M alloy.
13. The core-shell composite negative electrode material according to claim 1, It is characterized in that The first active material is composed of Si, SiO x And Si-M alloy composition, Si and SiO x The mass ratio of Si to Si-M alloy is 0.02-100, the median particle size of Si is 10-300 nm, and the mass ratio of Si to Si-M alloy is 0.02-100. x The median particle size of Si is 150-5000nm, the median particle size of Si-M alloy is 150-5000nm, the median particle size of Si is less than that of Si-M alloy and less than that of SiO x Median particle size.
14. The core-shell composite negative electrode material according to claim 1, It is characterized in that The components of the second active material include any one of natural graphite and artificial graphite or a combination of two of them.
15. The core-shell composite negative electrode material according to claim 1, It is characterized in that The median particle size of the second active material is 1 to 15 um.
16. The core-shell composite negative electrode material according to claim 1, It is characterized in that The median particle size of the second active material is larger than that of the first active material, and the difference is 2 μm to 12 μm.
17. The core-shell composite negative electrode material according to claim 1, It is characterized in that Taking the total mass of the core-shell composite negative electrode material as 100wt%, the mass percentage of the first active substance is 1-70wt%, the mass percentage of the second active substance is 5-60wt%, and the mass percentage of the third active substance is 5-50wt%.
18. A method for preparing a core-shell composite negative electrode material according to any one of claims 1 to 17, It is characterized in that The method comprises the following steps: (1) mixing and granulating a first active material and a second active material to obtain a first precursor; (2) performing carbon coating modification on the first precursor, and then sintering to obtain a core-shell composite negative electrode material; Among them, the first active substance is a flaky silicon-based material, the second active substance is a flaky graphite material, the particle aspect ratio of the flaky silicon-based material is 1.5 to 100 and does not include 1.5, the particle aspect ratio is the ratio of the maximum linear dimension to the minimum linear dimension of the particle, and the aspect ratio of the flaky graphite material is 2 to 50 and does not include 2.
19. The method according to claim 18, It is characterized in that The specific surface area of the flaky silicon-based material is 50 to 500 m 2 / g.
20. The method according to claim 18, It is characterized in that The first active material comprises Si, SiO x Or a combination of at least two of Si-M alloys, wherein 0.5≤x≤1.5, and M is any one of B, Fe, Cu, Sn, Ge, Ti, Mg, Ni or Ce, or a combination of at least two of them.
21. The method according to claim 18, It is characterized in that In the first active material, the absolute value of the difference in median particle diameters of different materials is 50 nm to 1500 nm.
22. The method according to claim 18, It is characterized in that The first active material is composed of Si and SiO in a mass ratio of 0.01 to 100. x The median particle size of Si is 10-300 nm, and SiO x The median particle size of Si is 150-5000nm, and the median particle size of Si is less than that of SiO x Median particle size.
23. The method according to claim 18, It is characterized in that The first active material is composed of Si and Si-M alloy in a mass ratio of 0.01-100, the median particle size of Si is 10-300nm, the median particle size of Si-M alloy is 150-5000nm, and the median particle size of Si is less than the median particle size of Si-M alloy.
24. The method according to claim 18, It is characterized in that The first active material is composed of SiO x With Si-M alloy composition, SiO x The median particle size of Si-M alloy is 150-400nm, the median particle size of Si-M alloy is 200-5000nm and SiO x The median particle size is less than the median particle size of Si-M alloy.
25. The method according to claim 18, It is characterized in that The first active material is composed of SiOx and Si-M alloy in a mass ratio of 0.01 to 100, the median particle size of the Si-M alloy is 150 to 400 nm, and the SiO x The median particle size is 200-5000nm and the median particle size of Si-M alloy is less than that of SiO x Median particle size.
26. The method according to claim 18, It is characterized in that The first active material is composed of Si, SiO x And Si-M alloy composition, Si and SiO x The mass ratio of Si to Si-M alloy is 0.02-100, the median particle size of Si is 10-300 nm, and the mass ratio of Si to Si-M alloy is 0.02-100. x The median particle size of Si is 150-5000nm, the median particle size of Si-M alloy is 150-5000nm, and the median particle size of Si is less than that of SiO x The median particle size is less than the median particle size of Si-M alloy.
27. The method according to claim 18, It is characterized in that The first active material is composed of Si, SiO x And Si-M alloy composition, Si and SiO x The mass ratio of Si to Si-M alloy is 0.02-100, the median particle size of Si is 10-300 nm, and the mass ratio of Si to Si-M alloy is 0.02-100. x The median particle size of Si is 150-5000nm, the median particle size of Si-M alloy is 150-5000nm, the median particle size of Si is less than that of Si-M alloy and less than that of SiO x Median particle size.
28. The method according to claim 18, It is characterized in that The components of the second active material include any one of natural graphite and artificial graphite or a combination of two of them.
29. The method according to claim 18, It is characterized in that The median particle size of the second active material is 1 to 15 um.
30. The method according to claim 18, It is characterized in that The mixing granulation method in step (1) is any one of spray drying, mixing heating or kneading molding.
31. The method according to claim 18, It is characterized in that The carbon coating modification method in step (2) is any one of a liquid phase coating method, a solid phase coating method or a gas phase coating method.
32. The method according to claim 31, It is characterized in that The process steps of the liquid phase coating method include: dispersing a first precursor and a carbon source in an organic solvent system, and drying to obtain a second precursor.
33. The method according to claim 31, It is characterized in that The process steps of the solid phase coating method include: placing a first precursor and a carbon source in a mixer and mixing them to obtain a second precursor.
34. The method according to claim 31, It is characterized in that In the liquid phase coating method and the solid phase coating method, the carbon source is independently any one of polyesters, sugars, organic acids or asphalt, or a combination of at least two of them.
35. The method according to claim 34, It is characterized in that The polyesters include any one or a combination of at least two of phenolic resin, polyethylene terephthalate, polybutylene terephthalate or polyarylate.
36. The method according to claim 31, It is characterized in that The process steps of the gas phase coating method include: in a reaction furnace, using organic carbon source gas as a coating source, heating to 500° C. to 1200° C. under the condition of inert gas, and carbon coating the first precursor to obtain the second precursor.
37. The method according to claim 36, It is characterized in that In the gas phase coating method, the organic carbon source gas is any one of hydrocarbons or aromatic hydrocarbon derivatives with 1 to 3 benzene rings, or a combination of at least two of them.
38. The method according to claim 18, It is characterized in that The sintering in step (2) comprises: placing the second precursor in a reactor, heating it to 500° C. to 1200° C. under the protection of an inert gas, and obtaining a core-shell composite negative electrode material.
39. The method according to claim 38, It is characterized in that The reactor comprises any one of a vacuum furnace, a box furnace, a rotary kiln, a roller kiln, a pusher kiln or a tube furnace.
40. A negative electrode, It is characterized in that The negative electrode comprises the core-shell composite negative electrode material according to any one of claims 1 to 17.
41. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the core-shell composite negative electrode material according to any one of claims 1 to 17.
Citation Information
Patent Citations
Carbon-coated silicon / graphite composite material preparation method
CN109273692A
Negative electrode active material for rechargeable lithium battery, negative electrode including the same and method of preparing the same, and rechargeable lithium battery including the same
CN102956877A
Lithium-ion battery silicon-carbon anode material and preparation method thereof
CN103199252A
Silicon monoxide composite negative electrode material for lithium ion battery, preparation method and lithium ion battery
CN103474631A
Silicon-carbon composite anode material, preparation method thereof and lithium ion battery
CN104103807A