Positive electrode active material for lithium secondary battery and lithium secondary battery containing the same
By designing the lithium ion diffusion path in the positive electrode active material of the lithium secondary battery to form a one-dimensional or two-dimensional channel structure along the center direction of the particles, the problem of poor thermal stability of the lithium secondary battery is solved, and the capacity, power and Lifespan characteristics.
Patent Information
- Application Number
- CN202110793065.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2015-01-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2035-01-21
AI Technical Summary
The positive electrode active materials of existing lithium secondary batteries have poor thermal stability during charging and discharging, resulting in unstable structure and affecting the safety and life of the battery.
Using a positive electrode active material with a layered structure, the lithium ion diffusion path in the primary particles is formed along the a-axis or b-axis towards the center of the secondary particles, forming a one-dimensional or two-dimensional pore structure to improve the conduction speed of lithium ions and Structural stability.
Through this structural design, lithium ions are easier to absorb and release when charged and discharged, improving the capacity, power and life characteristics of the battery and reducing the internal impedance of the battery.
Smart Images

Figure CN113540421B_ABST
Abstract
Description
[0001] The present application is a divisional application of an application filed on January 21, 2015, with application number 201580000969.1 and invention name “Positive electrode active material for lithium secondary battery and lithium secondary battery containing the same”.
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application claims the benefit of U.S. Provisional Patent Application No. 62 / 551,417, filed on August 29, 2017. Technical Field
[0004] The present invention relates to a positive electrode active material for a lithium secondary battery and a lithium secondary battery containing the same, and more particularly to a positive electrode active material for a lithium secondary battery characterized in that lithium ion diffusion paths within primary particles and secondary particles in a positive electrode active material having a layered structure are formed in a manner that has directionality toward a specific direction, and a lithium secondary battery containing the same. Background Art
[0005] Recently, there has been an increasing interest in energy storage technology. Batteries have been widely used as energy sources in the fields of mobile phones, cameras, laptop PCs, and electric vehicles, leading to intensive research and development of electrochemical devices. In this regard, electrochemical devices are one of the topics of great interest. In particular, the development of rechargeable secondary batteries has become a focus of attention.
[0006] Among the secondary batteries currently in use, the lithium secondary battery developed in the early 1990s is a compact, lightweight and large-capacity battery that has been widely used as a power source for portable devices since its appearance in 1991. Lithium secondary batteries have higher operating voltage and energy density than conventional batteries using aqueous electrolytes (such as Ni-MH batteries, Ni-Cd batteries and lead-sulfuric acid batteries), and have attracted much attention due to these advantages. In particular, recent research on power sources for electric vehicles that combine internal combustion engines and lithium secondary batteries has been actively progressing in the United States, Japan, Europe and other regions.
[0007] However, lithium-ion batteries are used as large batteries for electric vehicles in terms of energy density, but nickel-metal hydride batteries have been used until now for safety reasons, and the biggest issue at present is the high price and safety. In particular, the positive electrode active materials currently used commercially, such as LiCoO2 and LiNiO2, have the disadvantage that the crystal structure is not stable enough due to the detachment of lithium during charging, and the thermal properties are very poor. That is, if the overcharged battery is heated at 200-270°C, the structure changes rapidly, and the reaction of releasing oxygen in the lattice occurs due to this structural change.
[0008] In order to improve this situation, various methods are being tried, for example, by replacing a portion of nickel with a transition metal element to shift the temperature of heat generation to a slightly higher temperature or to prevent rapid heat generation. Materials that replace a portion of nickel with cobalt, for example, LiNi1-XCoxO2 (x = 0.1-0.3), although showing excellent charge / discharge characteristics and life characteristics, the problem of thermal stability has not been solved. In addition, Li-Ni-Mn composite oxides, in which Mn with excellent thermal stability replaces a portion of Ni, or Li-Ni-Mn-Co composite oxides, in which Mn and Co replace a portion of Ni, are also widely known in terms of composition and preparation-related technologies. Recently, Japanese Patent No. 2000-227858 discloses that the positive electrode active material is not prepared by partially substituting transition metals into LiNiO2 or LiMnO2 by this technology, but by a new technology to uniformly distribute Mn and Ni compounds at the atomic level to obtain a solid solution.
[0009] According to European Patent No. 0918041 or U.S. Patent No. 6040090 on the composition of Li-Ni-Mn-Co composite oxides, in which Mn and Co replace a portion of Ni, LiNi1-xCoxMnyO2 (0<y≤0.3) has improved thermal stability compared to existing materials containing only Ni and Co. However, the thermal stability of Ni-based compounds has not yet been resolved.
[0010] In order to solve this problem, Korean Patent Application No. 10-2005-7007548 discloses a lithium transition metal oxide with a metal concentration gradient. However, this method can make the inner layer and the outer layer have different metal compositions during synthesis, but the metal composition does not change gradually and continuously in the synthesized positive electrode active material. Through a heat treatment process, a gradual concentration gradient of the metal composition can be obtained. However, the interface resistance generated between the inner layer and the outer layer acts as a resistance to the diffusion of lithium in the particles, which may lead to a decrease in life characteristics. In addition, since the material is an NCM-based composite with an inner layer composed of LCO, Co rich NCM and a nickel content of less than 60%, and the overall nickel content is also low, it is difficult to reflect a high capacity.
[0011] Furthermore, the powder synthesized by this invention has a low tapped density because the powder does not use ammonia as a chelating agent, and is therefore insufficient for use as a positive electrode active material for lithium secondary batteries requiring high thermal energy density. Summary of the invention
[0012] Technical issues
[0013] In order to solve the above technical problems, an object of the present invention is to provide a positive electrode active material for a lithium secondary battery with a novel structure, in which the lithium ion diffusion paths within the primary particles and the secondary particles in the positive electrode active material have a layered structure and exhibit specific directionality.
[0014] Another object of the present invention is to provide a lithium secondary battery comprising the positive electrode active material for a lithium secondary battery according to the present invention.
[0015] Technical Solution
[0016] In order to solve the above technical problems, the present invention provides a positive electrode active material for a lithium secondary battery, characterized in that the positive electrode active material is a spherical secondary particle formed by aggregation of primary particles, and the lithium ion diffusion path within the primary particle is formed along the a-axis or b-axis on the layered structure toward the center of the secondary particle.
[0017] Figure 6 and Figure 7 The structural model diagram of the primary particles and secondary particles of the positive electrode active material for lithium secondary batteries according to the present invention is shown. Figure 7 As shown, according to the positive electrode active material for lithium secondary batteries of the present invention, the lithium ion diffusion path in the primary particle is formed side by side along the a-axis or b-axis on the layered structure and exhibits directionality toward the center of the secondary particle.
[0018] According to the positive electrode active material for lithium secondary batteries of the present invention, it is characterized in that the aspect ratio of the primary particles is greater than 1, and the lithium ion diffusion path in the primary particles is formed along the long axis direction of the particles. That is, in the positive electrode active material for lithium secondary batteries of the present invention, since the lithium ion diffusion path is formed along the long axis direction, when lithium ions move into the primary particles in the positive electrode active material during charge and discharge, they move into the primary particles along the horizontal axis direction with a relatively narrow area. Therefore, as charge and discharge continue, the area where the crystal structure collapses is relatively reduced, and finally the structural stability is reflected.
[0019] The positive electrode active material for lithium secondary batteries according to the present invention is characterized in that the aspect ratio is greater than 1, and the area of primary particles formed by the lithium ion diffusion path in the particles along the long axis direction of the particles is greater than 20% of the total area.
[0020] According to the positive electrode active material for lithium secondary batteries of the present invention, when the particles are square in shape as shown in FIG. 6 , the aspect ratio is defined as L / W (L is the major axis and W is the minor axis); when the horizontal axis lengths are W1 and W2, the aspect ratio is defined as L / (W1+W2) / 2.
[0021] According to the positive electrode active material for lithium secondary batteries of the present invention, it is characterized in that the area occupied by the primary particles in which the lithium ion diffusion path is toward the center direction of the secondary particles is more than 40% of the area of the entire particles. According to the positive electrode active material for lithium secondary batteries of the present invention, it is characterized in that the lithium ion diffusion path in the primary particles is inclined within ±45° from the center direction of the secondary particles. That is, according to the positive electrode active material for lithium secondary batteries of the present invention, it is characterized in that the lithium ion diffusion path in the primary particles is toward the center of the secondary particles, but this is not mechanically arranged toward the exact center direction of the secondary particles, but is freely arranged within ±45° from the center direction of the secondary particles.
[0022] According to the positive electrode active material for lithium secondary batteries of the present invention, it is characterized in that the primary particles are formed in a directional manner toward the center direction of the entire particle, and the lithium ion diffusion path within the primary particles is formed along the center direction of the entire particle, so that the lithium ion diffusion path has a one-dimensional or two-dimensional pore structure from the surface to the center of the secondary particle.
[0023] Thus, the primary particles having different aspect ratios may be in the shape of needles, plates, cuboids, oblong cuboids or cylinders.
[0024] Based on this lithium ion diffusion path, lithium ions have a faster conduction speed and show higher lithium ion conductivity. Even with repeated charge and discharge, the crystal structure will not easily disintegrate, thereby improving the cycle characteristics.
[0025] In addition, according to the positive electrode active material for lithium secondary batteries of the present invention, based on the lithium ion diffusion path formed by the one-dimensional pore structure as a linear path or the two-dimensional pore structure as a surface path, the charge transfer resistance, diffusion, migration and convection between the active material particles and the lithium ions or the electrolyte are low, thereby significantly reducing the internal impedance of the battery.
[0026] The positive electrode active material for lithium secondary battery according to the present invention is characterized in that the secondary particles include:
[0027] A core layer, represented by the following chemical formula 1, and having a constant concentration of transition metal;
[0028] a concentration gradient layer formed on the outer surface of the core layer, wherein the concentration of one or more transition metals changes continuously to form a concentration gradient; and
[0029] The shell layer is represented by the following Chemical Formula 2 and is formed on the outer surface of the concentration gradient layer, and the concentration of the transition metal is constant.
[0030] <Chemical formula 1> Li x Ni 1-a-b-c Co a Mn b Me c O 2-y X y
[0031] (In the chemical formula 1, 0.9≤x≤1.15, 0≤a≤0.20, 0≤b≤0.20, 0≤c≤0.1, 0≤y≤0.1; Me is at least one element selected from the group consisting of Al, Mg, B, P, Ti, Si, Zr, Ba and a combination thereof; X is at least one element and molecule selected from the group consisting of anions of F, BO3, and PO4.)
[0032] <Chemical formula 2> Li x Ni 1-a-b-c Co a Mn b Me c O 2-y X y
[0033] (In the chemical formula 2, 0.9≤x≤1.15, 0≤a≤0.50, 0≤b≤0.6, 0≤c≤0.2, 0≤y≤0.1; Me is at least one element selected from the group consisting of Al, Mg, B, P, Ti, Si, Zr, Ba and a combination thereof; X is at least one element and molecule selected from the group consisting of anions of F, BO3, and PO4.)
[0034] The positive electrode active material for a lithium secondary battery according to the present invention is characterized in that the thickness of the shell layer is 0.05 to 2.0 μm.
[0035] According to the positive electrode active material for a lithium secondary battery of the present invention, it is characterized in that in the primary particles of the concentration gradient layer, a lithium ion diffusion path is directed toward the center of the secondary particles.
[0036] The present invention also provides a lithium secondary battery, which includes the positive electrode active material for a lithium secondary battery according to the present invention.
[0037] Technical Effects
[0038] According to the positive electrode active material for lithium secondary batteries of the present invention, since the lithium ion diffusion path in the primary particles is formed in a directional manner toward the center of the particles, it is easier to store and release lithium ions in the primary particles, thereby greatly improving the capacity, power and life characteristics of the battery including the positive electrode active material for lithium secondary batteries of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 SEM images of positive electrode active material particles prepared in Examples 1 to 5 of the present invention and Comparative Example 1 are shown.
[0040] Figure 2 The results of measuring the SEM images of the fracture surfaces of the positive electrode active material particles prepared in Examples 1 to 5 of the present invention and Comparative Example 1 are shown.
[0041] Figure 3 and Figure 4 The results of measuring the shapes and structures of primary particles in the particles of Example 3 of the present invention and Comparative Example 1 using TEM are shown.
[0042] Figure 5 The results of measuring the composition inside the particles prepared in Example 3 of the present invention using EDX are shown.
[0043] 6 shows a layered structure of a positive electrode active material for a lithium secondary battery according to the present invention (a), and is a schematic diagram showing the shape of a particle cross section and a lithium ion diffusion path of a primary particle.
[0044] Figure 7 A schematic cross-sectional view of the primary particle according to the present invention is shown. DETAILED DESCRIPTION
[0045] Hereinafter, the present invention will be described in more detail based on examples. However, the present invention is not limited to the following examples.
[0046] <Example 1>
[0047] In step 1, 20L of distilled water and 1000g of ammonia as a chelating agent are added to a co-precipitation reactor (internal volume: 100L, rotary motor power: more than 80%), and stirred at a motor speed of 300-1000rpm while maintaining the temperature in the reactor at 40-50°C.
[0048] In step 2, nickel sulfate, cobalt sulfate and manganese sulfate are mixed in a molar ratio of 80:20:0 to prepare a 2.5M concentration of the first precursor aqueous solution at 2.2 L / hour, and a 28% concentration of ammonia aqueous solution is continuously supplied to the reactor at 0.15 L / hour. In addition, in order to adjust the pH value, a 25% concentration of sodium hydroxide aqueous solution is supplied to maintain the pH value at 11.3 to 11.4. The impeller speed is adjusted to 300 to 1000 rpm. The first precursor aqueous solution, the ammonia aqueous solution and the sodium hydroxide aqueous solution are continuously supplied to the reactor, and the total amount is 38 L.
[0049] In step 3, nickel sulfate, cobalt sulfate and manganese sulfate are mixed in a molar ratio of 35:20:45 to prepare a 2.5M aqueous solution for forming a concentration gradient layer, 10L of a first precursor aqueous solution prepared by mixing nickel sulfate, cobalt sulfate and manganese sulfate in a molar ratio of 80:20:0 to prepare a 2.5M concentration is placed in another agitator other than the above reactor, and the aqueous solution for forming a concentration gradient layer is supplied at a rate of 2.2L / hour while stirring to prepare a second precursor aqueous solution, and the second precursor aqueous solution is introduced into the above reactor. The aqueous solution for forming a concentration gradient layer is mixed and introduced into the reactor until the molar ratio of nickel sulfate, cobalt sulfate and manganese sulfate in the second precursor aqueous solution becomes 40:20:40, i.e., the shell concentration, and a 28% concentration ammonia aqueous solution is supplied to the reactor at a rate of 0.08L / hour, and a sodium hydroxide solution is used to maintain the pH value at 11.3-11.4. At this time, the total amount of the second precursor aqueous solution, the ammonia aqueous solution and the sodium hydroxide aqueous solution supplied was 24L.
[0050] In step 4, a third precursor aqueous solution prepared by mixing nickel sulfate, cobalt sulfate and manganese sulfate in a molar ratio of 40:20:40 is supplied to a reactor until the volume occupied is 8 L. After the reaction is completed, a spherical nickel-manganese-cobalt composite hydroxide precipitate is obtained from the reactor.
[0051] The precipitated composite metal hydroxide was filtered, washed with pure water, and dried in a hot air dryer at 100°C for 12 hours to obtain a precursor powder in the form of a metal composite oxide, the inner core layer of which was (Ni 0.8 Co0.20 )(OH)2, the outer shell is from (Ni 0.80 Co 0.20 )(OH)2 to (Ni 0.4 Co 0.2 Mn 0.4 )(OH)2 has a continuous concentration gradient.
[0052] The metal composite hydroxide precursor and lithium hydroxide (LiOH·H2O) are mixed in a molar ratio of 1:1.00-1.10, and heated to 550°C at a heating rate of 2°C / min. After heat treatment for 10 hours, the mixture is calcined at 750°C for 20 hours to obtain a positive electrode active material powder, the inner core layer of which is Li(Ni 0.80 Co 0.20 )O2, the outer shell is from Li(Ni 0.80 Co 0.20 )O2 to Li(Ni 0.4 Co 0.2 Mn 0.4 )O2 has a continuous concentration gradient.
[0053] <Example 2>
[0054] The positive electrode was prepared in the same manner as in Example 1, except that the composition of the inner core layer was Li(Ni 0.70 Co 0.30 )O2, the composition of the outer shell changes from Li(Ni 0.70 Co 0.30 )O2 to Li(Ni 0.4 Co 0.2 Mn 0.4 )O2 has a continuous and constant concentration gradient.
[0055] <Example 3>
[0056] The positive electrode was prepared in the same manner as in Example 1, except that the composition of the inner core layer was Li(Ni 0.80 Co 0.20 )O2, the composition of the outer shell changes from Li(Ni 0.80 Co 0.20 )O2 to Li(Ni 0.35 Co 0.35 Mn 0.30 )O2 has a continuous and constant concentration gradient.
[0057] <Example 4>
[0058] The positive electrode was prepared in the same manner as in Example 1, except that the composition of the inner core layer was Li(Ni 0.90 Co 0.10)O2, the composition of the outer shell changes from Li(Ni 0.90 Co 0.10 )O2 to Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 has a continuous and constant concentration gradient.
[0059] <Example 5>
[0060] The positive electrode was prepared in the same manner as in Example 1, except that the composition of the inner core layer was Li(Ni 0.97 Co 0.03 )O2, the composition of the outer shell changes from Li(Ni 0.97 Co 0.03 )O2 to Li(Ni 0.5 Co 0.2 Mn 0.3 )O2 has a continuous and constant concentration gradient.
[0061] Comparative Example 1
[0062] 60L of distilled water and 1000g of ammonia as a chelating agent were added to a coprecipitation reactor (capacity: 70L), and stirred at a motor speed of 6000rpm while maintaining the temperature in the reactor at 40-50°C. In addition, nitrogen was continuously supplied to the reactor at a flow rate of 3L / min. Then, nickel sulfate, cobalt sulfate and manganese sulfate were mixed in a molar ratio of 8:1:1 to prepare a 1M concentration of precursor aqueous solution at 6.5L / hour, and a 28% concentration of ammonia aqueous solution was continuously supplied to the reactor at 0.6L / hour. In addition, in order to adjust the pH value, a 25% concentration of sodium hydroxide aqueous solution was continuously supplied to the liquid surface in the reaction tank at a rate of 1.5-2.0L / hour, maintaining the pH value at 11-12. The temperature of the reaction solution was controlled at 50±2°C. After 30 hours, when the temperature in the reactor reached normal, the hydroxide particles discharged from the overflow pipe were continuously extracted, washed with water, and dried in a hot air dryer at 100°C for 12 hours to obtain (Ni 0.8 Co 0.1 Mn 0.1 Precursor powder in the form of a metal composite hydroxide composed of )(OH)2.
[0063] The metal composite hydroxide and lithium hydroxide (LiOH·H2O) were mixed in a molar ratio of 1:1.00-1.10, and heated to 550°C at a heating rate of 2°C / min. After heat treatment for 10 hours, the mixture was calcined at 750°C for 20 hours to obtain a positive electrode active material powder.
[0064] <Test example: SEM image measurement>
[0065] The positive electrode active material particles prepared in Examples 1 to 5 and Comparative Example 1 and the SEM images of the particle fracture surfaces were measured, and the results are shown in Figure 1 and Figure 2 .
[0066] from Figure 1 It can be seen that the positive electrode active material particles prepared in Examples 1 to 5 of the present invention and Comparative Example 1 are spherical secondary particles formed by aggregation of primary particles.
[0067] Figure 2 It is an SEM image of the broken surface of the particle. It can be seen from the figure that in the particles prepared in Examples 1 to 5 of the present invention, the aspect ratio of the primary particle is greater than 1, and it grows along the long axis of the primary particle, that is, the long side direction and has a directionality toward the center of the particle, so that a lithium conduction path is formed from the particle surface to the particle center by a one-dimensional or two-dimensional pore structure. On the contrary, in the comparative example, the aspect ratio of the primary particle is much smaller than the value shown in the embodiments, and it is an irregular morphology, and no directionality of the primary particle is observed in the secondary particle.
[0068] <Test example: TEM image measurement>
[0069] The shape and structure of the primary particles in the particles prepared in Example 5 and Comparative Example 1 were measured by TEM, and the results are shown in FIG. Figure 3 and Figure 4 .
[0070] from Figure 3 It is found that in the particles prepared in Example 5 of the present invention, the primary particles are formed to have directionality toward the center, and the lithium ion conduction paths in the primary particles are formed in parallel toward the center of the secondary particles.
[0071] On the contrary, in the particles prepared in Comparative Example 1 of the present invention, Figure 4 It is found that the lithium ion conduction paths in the primary particles have no directionality and are formed irregularly.
[0072] <Test example: EDX image measurement>
[0073] The composition of the particles prepared in Example 3 was measured using EDX, and the results are shown in FIG. Figure 5 .
[0074] from Figure 5 It can be seen that in the particles prepared according to the embodiment of the present invention, nickel, cobalt and manganese present a concentration gradient from the core to the surface.
[0075] <Test example: Particle characteristics measurement>
[0076] The composition and particle size distribution of the lithium metal composite oxides prepared in Examples 1 to 5 and Comparative Example 1 were measured using a particle size analyzer, and the results are shown in Table 1 below.
[0077] In order to analyze its composition, a certain amount (about 2 g) of the lithium metal composite oxide prepared above was accurately (accuracy unit: 0.1 mg) weighed, transferred to a glass beaker, added with aqua regia (HCl:HNO3=3:1), and placed in a magnetic stirring heater (Hot Plate) to completely dissolve.
[0078] Using an induced coupled plasma atomic emission analyzer (ICP-AES, Perkin-Elmer 7300), the intensity (Intensity) of the modulated standard solution (3 types) was measured using a standard solution (Inorganic Venture, 1000 mg / kg) within the intrinsic wavelength of each element Li / Ni / Co / Mn, and a calibration curve (Calibration Curve) was prepared. Then, the pretreated sample solution and the base sample were poured into the analyzer, and the actual intensity was calculated by measuring each intensity. The concentration of each component compared with the prepared calibration curve was calculated, and normalized (Normalization) so that the overall sum became a theoretical value, thereby analyzing the composition of the prepared lithium metal composite oxide.
[0079] [Table 1]
[0080]
[0081] <Preparation Example: Preparation of Battery>
[0082] The positive electrode active materials prepared in Examples 1 to 6 and Comparative Example 1, super P as a conductive material, and polyvinylidene fluoride (PVdF) as a binder were mixed in a weight ratio of 92:5:3 to prepare a slurry. The slurry was uniformly coated on an aluminum foil with a thickness of 15 μm and dried under vacuum at 135°C to prepare a positive electrode for a lithium secondary battery.
[0083] The positive electrode and lithium foil are set as relative electrodes, a porous polyethylene film (Celgard LLC., Celgard2300, thickness: 25 μm) is set as a separation membrane, and a coin shell is prepared through a conventional preparation process using a liquid electrolyte with a concentration of 1.15 M LiPF6 dissolved in a mixed solvent of acetic acid ester and ethyl methyl carbonate in a volume ratio of 3:7.
[0084] <Test example: Battery characteristics measurement>
[0085] The initial capacity, initial efficiency, rate characteristics and life characteristics of the batteries including the active materials prepared in Examples 1 to 5 and Comparative Example were measured, and the results are shown in Table 3 below.
[0086] As can be seen from Table 3 below, the battery characteristics of the battery including the active material prepared in the example of the present invention are greatly improved compared with the comparative example.
[0087] [Table 2]
[0088]
[0089] Industrial Applicability
[0090] As described above, according to the positive electrode active material for lithium secondary batteries of the present invention, since the lithium ion diffusion path in the primary particles is formed in a directional manner toward the center of the particles, it is easier to store and release lithium ions in the primary particles, thereby greatly improving the capacity, power and life characteristics of the battery including the positive electrode active material for lithium secondary batteries of the present invention, which can be said to be very useful in this regard.
Claims
1. A positive electrode active material for a lithium secondary battery, wherein the positive electrode active material is a secondary particle formed by aggregation of primary particles, wherein the lithium ion diffusion path within the primary particle is formed toward the center of the secondary particle, The secondary particles include: A core layer, represented by the following chemical formula 1, and having a constant concentration of transition metal; a concentration gradient layer formed on the outer surface of the core layer, wherein the concentration of one or more transition metals changes continuously to form a concentration gradient; and A shell layer represented by the following chemical formula 2 and formed on the outer surface of the concentration gradient layer, and the concentration of the transition metal is constant, <Chemical formula 1> Li x1 Ni 1-a1-b1-c1 Co a1 Mn b1 Me c1 O 2-y1 X y1 In the chemical formula 1, 0.9≤x1≤1.15, 0.10≤a1≤0.20, b1=0, 0≤c1≤0.1, 0≤y1≤0.1; Me is at least one element selected from the group consisting of Al, Mg, B, P, Ti, Si, Zr, Ba and a combination thereof; X is at least one element and molecule selected from the group consisting of anions of F, BO3, and PO4, <Chemical formula 2> Li x2 Ni 1-a2-b2-c2 Co a2 Mn b2 Me c2 O 2-y2 X y2 In the chemical formula 2, 0.9≤x2≤1.15, 0.33≤a2≤0.35, 0.30≤b2≤0.40, 0≤c2≤0.2, 0≤y2≤0.1; Me is at least one element selected from the group consisting of Al, Mg, B, P, Ti, Si, Zr, Ba and combinations thereof; X is at least one element and molecule selected from the group consisting of anions of F, BO3, and PO4.
2. The positive electrode active material for lithium secondary battery according to claim 1, characterized in that: The aspect ratio of the primary particle is 1 or more, and a lithium ion diffusion path in the primary particle is formed along the long axis direction of the particle.
3. The positive electrode active material for lithium secondary battery according to claim 2, characterized in that: The aspect ratio is 1 or more, and the area of the primary particles formed along the long axis direction of the particles by the lithium ion diffusion paths in the particles is 20% or more of the total area.
4. The positive electrode active material for lithium secondary battery according to claim 1, characterized in that: The lithium ion diffusion path in the primary particle is inclined within ±45° from the center direction of the secondary particle.
5. The positive electrode active material for lithium secondary battery according to claim 1, characterized in that: The area of the primary particles in the direction of the lithium ion diffusion path toward the center of the secondary particles is 40% or more of the area of the entire particles.
6. The positive electrode active material for lithium secondary battery according to claim 1, characterized in that: The primary particle is formed in a directional manner toward the center of the entire particle, and the lithium ion diffusion path within the primary particle is formed along the center of the entire particle, so that the lithium ion diffusion path has a one-dimensional or two-dimensional pore structure from the surface to the center of the secondary particle.
7. The positive electrode active material for lithium secondary battery according to claim 6, characterized in that: The thickness of the shell layer is 0.05 to 2.0 μm.
8. The positive electrode active material for lithium secondary battery according to claim 6, characterized in that: In the primary particles of the concentration gradient layer, the lithium ion diffusion path is directed toward the center of the secondary particles.
9. The positive electrode active material for lithium secondary battery according to claim 1, characterized in that: The primary particles are in the shape of needles, plates, cuboids, oblong cuboids or cylinders. 10 . A lithium secondary battery comprising the positive electrode active material for a lithium secondary battery according to claim 1 .
Citation Information
Patent Citations
Lithium / nickel / cobalt composite oxide, process for preparing the same, and cathode active material for rechargeable battery
EP0918041A1
Processor and instruction processing method therefor
JP2000227858A
Positive electrode material for use in non-aqueous electrolyte battery, process for preparing the same, and non-aqueous electrolyte battery
US6040090A
Anode active material precursor for lithium secondary battery, anode active material manufactured using same, and lithium secondary battery comprising same