A method for pretreating fuel cell membrane electrode ionomer

By using alcohol solvents and pure water for stirring and high-speed shearing in the preparation of membrane electrodes, combined with ultrasonic dispersion technology, the problems of uneven dispersion and difficult morphology control of ionomers were solved, and the performance of the catalytic layer and membrane were significantly improved. electrode life.

CN114188582BActive Publication Date: 2024-10-22DONGFANG ELECTRIC (CHENGDU) HYDROGEN FUEL CELL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111507040.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-10
Publication Date
2024-10-22
Estimated Expiration
2041-12-10

AI Technical Summary

Technical Problem

Existing fuel cell membrane electrode preparation methods cannot efficiently disperse and regulate ionomer morphology, which affects the two-phase distribution of the catalytic layer, resulting in poor performance and lifespan.

Method used

The alcohol solvent is mixed with pure water and then cooled and sheared in a closed high-speed shearer, and then mixed with the catalyst under ultrasonic waves to form a catalyst slurry to achieve effective dispersion and morphological control of the ionomer.

Benefits of technology

It effectively opens the ionomer agglomerates to form a network structure, improves the uniformity of catalyst distribution and membrane electrode performance, shortens the dispersion time, and enhances the strength and life of the catalytic layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114188582B_ABST
    Figure CN114188582B_ABST
Patent Text Reader

Abstract

The invention discloses a fuel cell membrane electrode ionomer pretreatment method, which belongs to the field of fuel cell technology and comprises the following steps: S1. weighing 1 part of ionomer dispersion liquid and placing it in a beaker, weighing 10 parts of pure water and 2-4 parts of alcohol solvent, adding them into the ionomer dispersion liquid and stirring and mixing them evenly, wherein the alcohol solvent is an alcohol solvent with 2-3 carbon atoms; S2. placing the premixed ionomer dispersion liquid in a closed high-speed shearing machine, turning on the cooling system, and shearing, thereby completing the pretreatment of the ionomer; S3. then mixing the pretreated ionomer with a catalyst, water, and an alcohol solvent, and then dispersing the slurry using ultrasound, thereby obtaining the required catalyst slurry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fuel cells, and in particular relates to a fuel cell membrane electrode ionomer pretreatment method. Background Art

[0002] The catalyst layer of the membrane electrode is the core place where the electrochemical reaction of the fuel cell occurs, and it is also the key area that determines the power density of the membrane electrode. The catalyst layer is constructed by platinum catalysts and proton conductor ionomers, and has a microporous structure at the micro-nano scale. In the catalyst layer, only when the catalyst platinum particles and ionomers are in contact and exposed to the position where hydrogen and oxygen molecules can diffuse, such as the pore surface, to form a gas-liquid-solid three-phase reaction interface, can the hydrogen-oxygen electrochemical reaction be carried out efficiently.

[0003] The core functions of ionomers in the membrane electrode catalyst layer are mainly in three aspects: (1) conducting protons; (2) stabilizing the dispersion state of the catalyst; and (3) constructing the skeleton of the microporous structure. Therefore, the morphological structure of the ionomer is a key factor affecting the performance and durability of the catalyst layer. The agglomerated ionomers should be dispersed as much as possible so that they can effectively contact the dispersed catalyst. At the same time, their polymer chains should overlap with each other to form a network structure to play a skeleton support role.

[0004] Conventional membrane electrode preparation generally uses a dispersion of ionomers, that is, ionomers are dispersed in water or water-alcohol solvents in the form of nano-micron-sized aggregates, and the size of the aggregates is affected by the solvent system and the concentration of the ionomer. During preparation, the ionomer dispersion is usually directly mixed with the catalyst in a certain solvent, and the whole is dispersed by ultrasonic or ball milling to obtain a catalyst slurry. Ultrasonic waves can effectively disperse nanocatalysts, but the dispersion effect on ionomers with a large aspect ratio and in an aggregated state is poor, and it is impossible to effectively regulate their morphology; the shearing effect of ball milling is strong, and the morphological regulation effect of ionomers is obvious, but this dispersion method is inefficient and time-consuming, and the strong shearing of ball milling causes certain damage to the catalyst.

[0005] It can be seen that the above methods all have obvious defects. They are unable to efficiently disperse and regulate the morphology of the ionomers, which affects the two-phase distribution of the ionomers and the catalyst, and is not conducive to the construction and strength of the high-activity reaction interface of the catalytic layer, and ultimately affects the performance and life of the membrane electrode. This is also the main technical difficulty faced in the preparation of membrane electrode slurry. Summary of the invention

[0006] The purpose of the present invention is to provide a method for pretreatment of fuel cell membrane electrode ionomers to solve the technical problem that the existing design specifications cannot efficiently disperse and morphologically control the ionomers, which affects the two-phase distribution of the ionomer and the catalyst, and is not conducive to the construction and strength of the high-activity reaction interface of the catalytic layer, and ultimately affects the performance and life of the membrane electrode.

[0007] The present invention discloses a fuel cell membrane electrode ionomer pretreatment method, comprising the following steps:

[0008] S1. Weigh 1 part of the ionomer dispersion into a beaker, weigh 10 parts of pure water and 2-4 parts of an alcohol solvent, add the ionomer dispersion and stir to mix evenly, wherein the alcohol solvent is an alcohol solvent with 2-3 carbon atoms;

[0009] S2. The premixed ionomer dispersion is placed in a closed high-speed shearing machine, the cooling system is turned on, and shearing is performed, thereby completing the pretreatment of the ionomer;

[0010] S3. Then the pretreated ionomer is mixed with a catalyst, water, and an alcohol solvent, and the slurry is dispersed by ultrasonic wave to obtain the desired catalyst slurry.

[0011] Furthermore, the alcohol solvent in step S1 is ethanol or n-propanol.

[0012] Furthermore, 2 parts of ethanol are added in step S1.

[0013] Furthermore, in step S2, the cooling system maintains the slurry temperature at 25°C, the shear line speed at 20-30 m / s, and the shearing time at 2-8 min.

[0014] Furthermore, in step S2, the cooling system maintains the slurry temperature at 25°C, the shear line speed at 20 m / s, and the shearing time at 2 min.

[0015] Furthermore, in step S2, the cooling system maintains the slurry temperature at 25°C, the shear line speed at 20 m / s, and the shearing time at 5 min.

[0016] Furthermore, in step S2, the cooling system maintains the slurry temperature at 25°C, the shear line speed at 30 m / s, and the shearing time at 5 min.

[0017] Furthermore, in step S2, the cooling system maintains the slurry temperature at 25°C, the shear line speed at 30 m / s, and the shearing time at 8 min.

[0018] Furthermore, in step S3, the mass ratio of the ionomer to the catalyst, water and alcohol solvent is: 1 part of catalyst, 10 parts of water, 10 parts of alcohol solvent and 4 parts of ionomer.

[0019] Furthermore, in step S3, the ultrasonic dispersion treatment time is 20 min, the ultrasonic power is 500 W, and the slurry temperature is controlled to be 25°C.

[0020] The beneficial effects of the present invention are:

[0021] 1. It can effectively open the ionomer agglomerates and reduce the aggregation scale of the ionomer, which is conducive to the effective combination with the catalyst and uniform distribution in the slurry;

[0022] 2. It can effectively regulate the morphological structure of the ionomer, so that the polymer chains with large aspect ratios can be entangled and overlapped with each other to form a network structure and construct the skeleton structure of the catalyst layer;

[0023] 3. The dispersion of ionomer agglomerates takes less time and is more efficient;

[0024] 4. During the shearing process, the container should be sealed to prevent air from mixing in and avoid the generation of bubbles. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 This is a particle size distribution diagram of the catalyst slurry of Example 1 of the present invention;

[0027] Figure 2 This is a particle size distribution diagram of the catalyst slurry of Example 2 of the present invention;

[0028] Figure 3 This is a particle size distribution diagram of the catalyst slurry of Example 3 of the present invention;

[0029] Figure 4 This is a particle size distribution diagram of the catalyst slurry of Example 4 of the present invention;

[0030] Figure 5 This is a particle size distribution diagram of the catalyst slurry of Comparative Example 1 of the present invention;

[0031] Figure 6 This is a particle size distribution diagram of the catalyst slurry of Comparative Example 2 of the present invention;

[0032] Figure 7 This is a particle size distribution diagram of the catalyst slurry of Comparative Example 3 of the present invention;

[0033] Figure 8 This is a diagram showing the size of aggregates on the surface of the catalyst layer of Example 1 of the present invention;

[0034] Fig. 9 This is a diagram showing the size of aggregates on the surface of the catalyst layer of Example 2 of the present invention;

[0035] Fig.10 This is a diagram of the size of aggregates on the surface of the catalyst layer of Example 3 of the present invention;

[0036] Fig.11 This is a diagram showing the size of aggregates on the surface of the catalyst layer of Example 4 of the present invention;

[0037] Fig.12 This is a diagram showing the size of aggregates on the surface of the catalyst layer of Comparative Example 1 of the present invention;

[0038] Fig.13 This is a diagram showing the size of aggregates on the surface of the catalyst layer of Comparative Example 2 of the present invention;

[0039] Fig.14 This is a diagram showing the size of the aggregates on the surface of the catalyst layer of Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0040] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0041] Example 1

[0042] A fuel cell membrane electrode ionomer pretreatment method comprises the following steps:

[0043] (1) Weigh 1 part of ionomer dispersion into a beaker, weigh 10 parts of pure water and 3 parts of ethanol, add them to the ionomer dispersion and stir to mix evenly;

[0044] (2) The premixed ionomer dispersion is placed in a closed high-speed shearing machine, the cooling system is turned on, the slurry temperature is maintained at 25°C, the shearing line speed is 20m / s, and the shearing time is 5min, thus completing the pretreatment of the ionomer.

[0045] (3) Then the pretreated ionomer is mixed with a catalyst, water, and ethanol, and the mass ratio of each component is: 1 part of catalyst, 10 parts of water, 10 parts of ethanol, and 4 parts of ionomer; the slurry is then dispersed by ultrasonic treatment for 20 minutes, the ultrasonic power is 500W, and the slurry temperature is controlled at 25°C. The desired catalyst slurry is thus obtained.

[0046] Example 2

[0047] A fuel cell membrane electrode ionomer pretreatment method comprises the following steps:

[0048] (1) Weigh 1 part of ionomer dispersion into a beaker, weigh 10 parts of pure water and 3 parts of n-propanol, add them into the ionomer dispersion and stir to mix evenly;

[0049] (2) The premixed ionomer dispersion is placed in a closed high-speed shearing machine, the cooling system is turned on, the slurry temperature is maintained at 25°C, the shearing line speed is 20 m / s, and the shearing time is 2 min, thus completing the pretreatment of the ionomer.

[0050] (3) Then the pretreated ionomer is mixed with the catalyst, water and n-propanol, and the mass ratio of each component and the slurry dispersion process are consistent with Example 1. That is, the desired catalyst slurry is obtained.

[0051] Example 3

[0052] A fuel cell membrane electrode ionomer pretreatment method comprises the following steps:

[0053] (1) Weigh 1 part of ionomer dispersion into a beaker, weigh 10 parts of pure water and 2 parts of ethanol, add them into the ionomer dispersion and stir to mix evenly;

[0054] (2) The premixed ionomer dispersion is placed in a closed high-speed shearing machine, the cooling system is turned on, the slurry temperature is maintained at 25°C, the shearing line speed is 30m / s, and the shearing time is 5min, thus completing the pretreatment of the ionomer.

[0055] (3) The pretreated ionomer is then mixed with the catalyst, water and ethanol, and the mass ratio of each component and the slurry dispersion process are consistent with Example 1. That is, the desired catalyst slurry is obtained.

[0056] Example 4

[0057] A fuel cell membrane electrode ionomer pretreatment method comprises the following steps:

[0058] (1) Weigh 1 part of ionomer dispersion into a beaker, weigh 10 parts of pure water and 4 parts of ethanol, add them to the ionomer dispersion and stir to mix evenly;

[0059] (2) The premixed ionomer dispersion is placed in a closed high-speed shearing machine, the cooling system is turned on, the slurry temperature is maintained at 25°C, the shearing line speed is 30m / s, and the shearing time is 8min, thus completing the pretreatment of the ionomer.

[0060] (3) The pretreated ionomer is then mixed with the catalyst, water and ethanol, and the mass ratio of each component and the slurry dispersion process are consistent with Example 1. That is, the desired catalyst slurry is obtained.

[0061] Comparative Example 1

[0062] A method for preparing a fuel cell membrane electrode slurry comprises the following steps:

[0063] (1) Mixing the unpretreated ionomer with a catalyst, water, and ethanol, wherein the mass ratio of the components is: 1 part of catalyst, 10 parts of water, 10 parts of ethanol, and 4 parts of ionomer;

[0064] (2) The above slurry was subjected to ultrasonic dispersion treatment for 20 minutes, the ultrasonic power was 500 W, and the slurry temperature was controlled at 25° C. Thus, the desired catalyst slurry was obtained.

[0065] Comparative Example 2

[0066] A method for preparing a fuel cell membrane electrode slurry comprises the following steps:

[0067] (1) Weigh 1 part of ionomer dispersion into a beaker, weigh 12 parts of pure water, add it to the ionomer dispersion and stir to mix evenly;

[0068] (2) The premixed ionomer dispersion is placed in a closed high-speed shearing machine, the cooling system is turned on, the slurry temperature is maintained at 25°C, the shearing line speed is 30m / s, and the shearing time is 8min, thus completing the pretreatment of the ionomer.

[0069] (3) The pretreated ionomer is then mixed with the catalyst, water and ethanol, and the mass ratio of each component and the slurry dispersion process are consistent with Example 1. That is, the desired catalyst slurry is obtained.

[0070] Comparative Example 3

[0071] A method for preparing a fuel cell membrane electrode slurry comprises the following steps:

[0072] (1) Weigh 1 part of ionomer dispersion into a beaker, weigh 10 parts of ethanol, add it to the ionomer dispersion and stir to mix evenly;

[0073] (2) The premixed ionomer dispersion is placed in a closed high-speed shearing machine, the cooling system is turned on, the slurry temperature is maintained at 25°C, the shearing line speed is 30m / s, and the shearing time is 8min, thus completing the pretreatment of the ionomer.

[0074] (3) The pretreated ionomer is then mixed with the catalyst, water and ethanol, and the mass ratio of each component and the slurry dispersion process are consistent with Example 1. That is, the desired catalyst slurry is obtained.

[0075] The samples were tested according to the test standard: GB / T20042.5-2009 "Proton exchange membrane fuel cell part 5: membrane electrode test method".

[0076] Table 1 Membrane electrode performance test table

[0077] Serial number sample Performance (V@2.0A / cm2) 1 Example 1 0.635 2 Example 2 0.630 3 Example 3 0.638 4 Example 4 0.640 5 Comparative Example 1 0.610 6 Comparative Example 2 0.605 7 Comparative Example 3 0.615

[0078] In Examples 1, 2, 3, and 4, the catalyst slurry was prepared by using pretreated ionomers. The ionomer used in Comparative Example 1 was not pretreated. In Comparative Examples 2 and 3, the ionomers were pretreated, but only water or alcohol was added during the pretreatment process, and the water-to-alcohol ratio exceeded the protection scope of the present invention. The particle size distribution of the prepared catalyst slurry was tested by a laser particle size analyzer, and the agglomerate distribution of the prepared catalyst layer was observed by a SEM electron microscope. The results showed that compared with the comparative example, the membrane electrode slurry prepared by the present invention had a small particle size distribution, and most of the particle sizes were nanometers; the prepared catalyst layer agglomerates were small in size and small in number, and agglomerates above 10 microns almost disappeared; the performance of the prepared membrane electrode was improved by 20mV at 2.0A / cm2, about 3.25%.

Claims

1. A method for pretreating a fuel cell membrane electrode ionomer, characterized in that: The following steps are involved: S1. Weigh 1 part of the ionomer dispersion into a beaker, weigh 10 parts of pure water and 2-4 parts of an alcohol solvent, add the ionomer dispersion and stir to mix evenly, wherein the alcohol solvent is an alcohol solvent having 2-3 carbon atoms; S2. The premixed ionomer dispersion is placed in a closed high-speed shearing machine, the cooling system is turned on, and shearing is performed to complete the pretreatment of the ionomer; S3. The pretreated ionomer is then mixed with a catalyst, water, and an alcohol solvent, and the slurry is then dispersed using ultrasonic treatment to obtain the desired catalyst slurry; In step S3, the mass ratio of the ionomer to the catalyst, water and alcohol solvent is: 1 part of catalyst, 10 parts of water, 10 parts of alcohol solvent and 4 parts of ionomer.

2. A fuel cell membrane electrode ionomer pretreatment method according to claim 1, characterized in that: The alcohol solvent in step S1 is ethanol or n-propanol.

3. A fuel cell membrane electrode ionomer pretreatment method according to claim 2, characterized in that: In step S1, 2 parts of ethanol are added.

4. A fuel cell membrane electrode ionomer pretreatment method according to claim 1, characterized in that: In step S2, the cooling system maintains the slurry temperature at 25°C, the shear line speed at 20-30 m / s, and the shearing time at 2-8 min.

5. A fuel cell membrane electrode ionomer pretreatment method according to claim 4, characterized in that: In step S2, the cooling system maintains the slurry temperature at 25°C, the shear line speed at 20 m / s, and the shearing time at 2 min.

6. A fuel cell membrane electrode ionomer pretreatment method according to claim 4, characterized in that: In step S2, the cooling system maintains the slurry temperature at 25°C, the shear line speed at 20 m / s, and the shearing time at 5 min.

7. A fuel cell membrane electrode ionomer pretreatment method according to claim 4, characterized in that: In step S2, the cooling system maintains the slurry temperature at 25°C, the shear line speed at 30 m / s, and the shearing time at 5 min.

8. A fuel cell membrane electrode ionomer pretreatment method according to claim 4, characterized in that: In step S2, the cooling system maintains the slurry temperature at 25°C, the shear line speed at 30 m / s, and the shearing time at 8 min.

9. A fuel cell membrane electrode ionomer pretreatment method according to claim 1, characterized in that: In step S3, the ultrasonic dispersion treatment time is 20 minutes, the ultrasonic power is 500W, and the slurry temperature is controlled at 25°C.