Titanium-based metallic glass powder rich in double-strong Fenton active elements and preparation method thereof

Titanium-based metal glass powder prepared by ball milling solves the problems of stability and resource waste of existing metal glass catalytic materials, realizes the synergistic effect of Cu and Fe, improves Fenton activity and stability, and can be acidic and neutral Efficiently degrade dyes in the environment.

CN114433849BActive Publication Date: 2024-11-22NANJING INST OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202111481050.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-06
Publication Date
2024-11-22
Estimated Expiration
2041-12-06

AI Technical Summary

Technical Problem

During the Fenton process, the existing metal glass catalytic materials have problems such as easy oxidation of Fe elements, insufficient stability, narrow Fenton active pH range and waste of resources. It is difficult to simultaneously contain Cu and Fe and do not contain no catalytic active elements. Difficult to make.

Method used

Three metal powders: Ti, Cu and Fe were prepared by ball milling method to prepare titanium-based metal glass powder rich in Cu and Fe, and the percentage of Ti element atoms was controlled to be between 40 and 60%, and the ratio between Cu and Fe was 1:0.25 and 1: 4. Use stearic acid as the process control agent, ball mill and cool and sieve to obtain pure titanium-based metallic glass powder.

Benefits of technology

The stable metal glass formation is achieved, the use of invalid elements is avoided, and the Fenton activity and stability of the catalyst is improved. Titanium-based metal glass powder shows efficient catalytic performance in both acidic and neutral environments, and can quickly degrade dyes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114433849B_ABST
    Figure CN114433849B_ABST
Patent Text Reader

Abstract

The present invention relates to a titanium-based metallic glass powder rich in double strong Fenton active elements and a preparation method thereof. The atomic percentage of Ti element in the metallic glass powder is 40-60%, and the atomic ratio of Cu to Fe is 1:0.25-1:4. The preparation steps are as follows: (1) Select three metal powder raw materials of Ti, Cu and Fe, mix them, and seal them together with process control agents and grinding balls in a ball mill; (2) Provide a protective atmosphere for the mixed powder in the sealed ball mill, then install the ball mill on a ball mill, and start the equipment for ball milling. The preparation method is simple and efficient, and can be completed in only one step. It also avoids the design and selection of elements that only promote the formation of metallic glass but have no direct contribution to dye degradation, thereby saving resources and costs. In addition, the obtained material has obvious advantages in photo-Fenton catalytic performance, among which Ti 50 Cu 40 Fe 10 The degradation rate of rhodamine B was as high as 87% within 4 minutes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photocatalytic material preparation, and specifically relates to a titanium-based metallic glass powder rich in double-strong Fenton active elements and a preparation method thereof. Background Art

[0002] With the continuous development of the printing and dyeing industry, the discharge of highly toxic organic waste liquid is increasing, which poses a great threat to the ecological environment and human health. Faced with the severe situation brought by industrial wastewater, Fenton technology (Fe 2+ / Fe 3+ +H2O2) is widely used due to its significant advantages. This is because the Fenton process produces non-selective, highly active hydroxyl radicals (·OH), which can quickly degrade almost all types of dyes. In contrast, other methods have certain limitations, such as the zero-valent reduction method, which is only sensitive to azo dyes. However, in the traditional Fenton process, the Fe element exists entirely in the form of ions, which is not only difficult to separate and recycle, but also limited by the working environment of strong acids. For this reason, experts and scholars have proposed using Fe-based metallic glass (Fe 0 ) replaces Fe 2+ The heterogeneous Fenton-like method for starting the reaction. This not only solves the problem of catalyst recovery, but also takes advantage of the advantages of metallic glass, namely, the structure is completely uniform and has no grain boundaries, so it is stable as a catalyst and not easy to deactivate. In addition, metallic glass is thermodynamically metastable and has a high Gibbs free energy, which can promote its own Fenton catalytic efficiency. However, it is worth noting that although the metallic glass structure is conducive to the increase of catalyst stability, Fe-based metallic glass will still be affected by Fe 0The problem of easy oxidation and insufficient stability, and the narrow pH range of Fenton activity involved in Fe element has not been solved. In addition, most of the selected components belong to the Fe-Si-B system, in which the component element B is expensive, which increases the cost of wastewater treatment. Considering that Cu, like Fe, is a strong Fenton active element, and Cu element is more stable and has more significant Fenton activity in a neutral environment, people began to explore the Fenton-like activity of Cu-based metallic glass. However, its absolute Fenton activity in a strong acid environment is not as good as that of Fe-based metallic glass. More regrettably, the Cu-based metallic glass reported so far, like Fe-based metallic glass, involves a large number of elements that only promote the formation of metallic glass but have no direct contribution to dye degradation (such as Zr, Al and Gd in Cu-Zr-Al-Gd, C and P in Fe-CP, Si and P in Fe-Si-B), which makes the value of each element not be reflected to the greatest extent, resulting in a waste of resources. Therefore, it is very meaningful to develop a metallic glass material that is rich in two strong Fenton active elements, Cu and Fe, and does not contain catalytically inactive elements. At present, most of the reported metallic glass-type Fenton catalytic materials are alloy strips obtained by the spin quenching method, which has two main problems: first, the dispersion effect of the alloy strips during the degradation process is far inferior to that of the powder material; second, the spin quenching method has very strict requirements on the alloy composition required to form metallic glass, and it is difficult to produce metallic glass materials that are rich in Cu and Fe and do not contain too many amorphous formation promoting elements. Summary of the invention

[0003] The purpose of the present invention is to provide a titanium-based metallic glass powder rich in double strong Fenton active elements and a preparation method thereof in view of the above problems. The method is simple and efficient, and the obtained material has obvious advantages in photo-Fenton catalytic performance.

[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0005] (1) selecting three metal powder raw materials of Ti, Cu and Fe, mixing them together with a process control agent and grinding balls, placing them in a sealed ball mill, wherein the atomic percentage of Ti element in the mixed metal powder is 40 to 60%, and the atomic ratio of Cu to Fe is 1:0.25 to 1:4;

[0006] (2) providing a protective atmosphere for the mixed powder in the sealed ball mill, then installing the ball mill on a ball mill, starting the equipment for ball milling, and after a period of time, obtaining a titanium-based metallic glass catalytic material rich in two strong Fenton-active elements, Cu and Fe.

[0007] After the ball milling process in step (2) is completed, the ball mill jar needs to be cooled for 3 hours under natural conditions, and then the jar is slowly opened, sieved, and the material is taken out, thereby obtaining pure titanium-based metallic glass powder.

[0008] Furthermore, the impurity content in the metal powder raw material does not exceed 1wt%.

[0009] Furthermore, the atomic percentage of Ti in the mixed metal powder is 45-55%. The atomic percentage of Ti should not be too high or too low: if the atomic percentage of Ti is too low, the metallic glass-forming ability of the mixed powder is limited, which is not conducive to obtaining a completely metallic glass with a stable structure; if the atomic percentage of Ti is too high, the content of strong Fenton-active elements in the prepared metallic glass is insufficient, resulting in the metallic glass having an unclear advantage in Fenton catalytic activity. As a preferred embodiment of the present invention, the purity of the metal powder raw material is 99.9wt%, and the atomic percentage of Ti in the mixed metal powder is 50%.

[0010] Preferably, the process control agent used in step (1) is stearic acid, and the addition amount is 1.0-4.0% of the total mass of the metal raw material. The grinding balls and the ball mill are made of stainless steel, wherein the particle size of the grinding balls ranges from 5 to 10 mm, the capacity of the ball mill is 100 mL, and the ball-to-material ratio is 15:1-30:1.

[0011] The protective atmosphere in step (2) is argon gas with a purity of 99.9%, and vacuum needs to be drawn before filling the argon gas. The ball mill speed is 825-900 r / min, and it stops for 5 minutes every 30 minutes of operation. After each stop, the system automatically changes the rotation direction of the main disk. The total ball milling time is 50 hours.

[0012] More preferably, in step (1), the amount of stearic acid added is 1.7-2.6% of the total mass of the metal raw material, the grinding balls are composed of three particle sizes of 5, 8 and 10 mm, and the ball-to-material ratio is 20:1-26:1.

[0013] The present invention has the following significant advantages:

[0014] (1) Not only is the preparation method conducive to the formation of metallic glass, but the selected Ti element also has a very strong ability to form metallic glass. Therefore, in the present invention, the Ti element can form metallic glass with Cu and Fe elements without relying on any other elements. It is worth noting that Ti 0 The oxide film (such as TiO2) formed on the surface can utilize ultraviolet resources and has a very significant semiconductor photocatalytic effect, thereby completely avoiding the design and selection of elements that only promote the formation of metallic glass but have no direct contribution to dye degradation, saving resources and costs.

[0015] (2) Fe and Cu are two strong Fenton-active elements, both of which are rich in structurally stable titanium-based metallic glasses. They can work together to greatly improve the catalytic efficiency of the alloy material. The Fe element ensures the absolute Fenton activity of the catalyst under acidic conditions, and the Cu element ensures the Fenton efficiency of the alloy material under neutral conditions and the overall catalytic stability.

[0016] (3) The surface of titanium-based metallic glass powder has a dual-effect mechanism of heterogeneous photo-Fenton and semiconductor photocatalysis promoting each other: on the one hand, the photogenerated electrons (e - ) will be Cu 2+ / Fe 3+ capture, thereby reducing the recombination rate of photogenerated carriers and increasing the photocatalytic activity of semiconductors; on the other hand, Cu 2+ / Fe 3+ Get e - It will then immediately transform into the active ion Cu + / Fe 2+ , thereby improving the photo-Fenton efficiency.

[0017] (4) The preparation method is simple and efficient. It only takes one step to produce metallic glass powder with high specific surface area, and a large amount of energy is stored inside the alloy, thereby increasing the reactivity of the alloy powder. When the powder comes into contact with the dye, the energy is quickly released, causing the dye to degrade rapidly. For example, the prepared Ti 50 Cu 40 Fe 10 Metallic glass powder can degrade nearly 90% of Rhodamine B dye in just 4 minutes. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Ti involved in the method of the present invention 50 Cu 40 Fe 10 X-ray diffraction (XRD) pattern of the metallic glass powder (Example 1);

[0019] Figure 2 Ti involved in the present invention 50 Cu 40 Fe 10 Surface morphology (SEM) photo of metallic glass powder;

[0020] Figure 3 Ti involved in the present invention 50 Cu 40 Fe 10 Particle size distribution of metallic glass powder;

[0021] Figure 4 Ti involved in the present invention 50 Cu 40 Fe 10 Degradation curve of Rhodamine B dye by metallic glass powder and blank control group under ultraviolet light. DETAILED DESCRIPTION

[0022] For ease of understanding, the present invention is further described below in conjunction with specific embodiments, but this is not intended to be an improper limitation to the present invention.

[0023] Example 1

[0024] Step 1: Select Ti, Cu, and Fe powder raw materials with a purity of 99.9wt%, weigh them according to the atomic percentage of Ti: 50%, Cu: 40%, and Fe: 10%, and weigh 1.7% of the total mass of stearic acid as a process control agent;

[0025] Step 2: Place the raw materials prepared in step 1, stearic acid, and stainless steel grinding balls with particle sizes of 5, 8, and 10 mm in a 100 mL stainless steel ball mill jar, and then seal it. The ball-to-material ratio is 20:1.

[0026] Step 3: Evacuate the ball mill sealed in step 2, and after a few minutes, fill the ball mill with argon gas with a purity of 99.9% as a protective atmosphere, and then fix the ball mill on the main plate of the ball mill;

[0027] Step 4: When the conditions in step 3 are met, start the equipment for ball milling at a speed of 825 r / min, run for 30 minutes and stop for 5 minutes, and the system automatically changes the main disk rotation direction after each stop. The total ball milling time is 50 hours;

[0028] Step 5: After the equipment has completed the operation according to step 4, unload the ball mill from the main plate of the ball mill, let it cool in a natural environment for 3 hours, then slowly open the can, sieve, and take the material to finally obtain Ti 50 Cu 40 Fe 10 Metallic glass powder.

[0029] Example 2

[0030] Step 1: Select Ti, Cu, and Fe powder raw materials with a purity of 99.9wt%, weigh them according to the atomic percentage of Ti: 50%, Cu: 30%, and Fe: 20%, and weigh 2.0% of the total mass of stearic acid as a process control agent;

[0031] Step 2: Place the raw materials prepared in step 1, stearic acid, and stainless steel grinding balls with particle sizes of 5, 8, and 10 mm in a 100 mL stainless steel ball mill jar, and then seal it. The ball-to-material ratio is 22:1;

[0032] Step 3: Evacuate the ball mill sealed in step 2, and after a few minutes, fill the ball mill with argon gas with a purity of 99.9% as a protective atmosphere, and then fix the ball mill on the main plate of the ball mill;

[0033] Step 4: When the conditions in step 3 are met, start the equipment for ball milling at a speed of 850 r / min, and stop for 5 minutes every 30 minutes. After each stop, the system automatically changes the rotation direction of the main disk. The total ball milling time is 50 hours.

[0034] Step 5: After the equipment has completed the operation according to step 4, unload the ball mill from the main plate of the ball mill, let it cool in a natural environment for 3 hours, then slowly open the can, sieve, and take the material to finally obtain Ti 50 Cu 30 Fe 20 Metallic glass powder.

[0035] Example 3

[0036] Step 1: Select Ti, Cu, and Fe powder raw materials with a purity of 99.9wt%, weigh them according to the atomic percentage of Ti: 50%, Cu: 20%, and Fe: 30%, and weigh 2.3% of the total mass of stearic acid as a process control agent;

[0037] Step 2: Place the raw materials prepared in step 1, stearic acid, and stainless steel grinding balls with particle sizes of 5, 8, and 10 mm in a 100 mL stainless steel ball mill jar, and then seal it, wherein the ball-to-material ratio is 24:1;

[0038] Step 3: Evacuate the ball mill sealed in step 2, and after a few minutes, fill the ball mill with argon gas with a purity of 99.9% as a protective atmosphere, and then fix the ball mill on the main plate of the ball mill;

[0039] Step 4: When the conditions in step 3 are met, start the equipment for ball milling at a speed of 875 r / min, stop for 5 minutes after every 30 minutes of operation, and the system automatically changes the main disk rotation direction after each stop. The total ball milling time is 50 hours;

[0040] Step 5: After the equipment has completed the operation according to step 4, unload the ball mill from the main plate of the ball mill, let it cool in a natural environment for 3 hours, then slowly open the can, sieve, and take the material to finally obtain Ti 50 Cu 20 Fe 30 Metallic glass powder.

[0041] Example 4

[0042] Step 1: Select Ti, Cu, and Fe powder raw materials with a purity of 99.9wt%, weigh them according to the atomic percentage of Ti: 50%, Cu: 10%, and Fe: 40%, and weigh 2.6% of the total mass of stearic acid as a process control agent;

[0043] Step 2: Place the raw materials prepared in step 1, stearic acid, and stainless steel grinding balls with particle sizes of 5, 8, and 10 mm in a 100 mL stainless steel ball mill jar, and then seal it. The ball-to-material ratio is 26:1;

[0044] Step 3: Evacuate the ball mill sealed in step 2, and after a few minutes, fill the ball mill with argon gas with a purity of 99.9% as a protective atmosphere, and then fix the ball mill on the main plate of the ball mill;

[0045] Step 4: When the conditions in step 3 are met, start the equipment for ball milling at a speed of 900 r / min, stop for 5 minutes after every 30 minutes of operation, and the system automatically changes the main disk rotation direction after each stop. The total ball milling time is 50 hours;

[0046] Step 5: After the equipment has completed the operation according to step 4, unload the ball mill from the main plate of the ball mill, let it cool in a natural environment for 3 hours, then slowly open the can, sieve, and take the material to finally obtain Ti 50 Cu 10 Fe 40 Metallic glass powder.

[0047] Test example

[0048] Figure 1 The XRD pattern of the alloy powder prepared in Example 1 shows that only the amorphous diffuse scattering peak appears, indicating that Ti 50 Cu 40 Fe 10 It exists in the form of complete metallic glass, thus ensuring the catalytic stability of the alloy powder in a Fenton-like process. Figure 2 This is a SEM picture of the metallic glass powder prepared in Example 1. It can be seen from the picture that the prepared powder is granular and has a rough surface, and should have a good adsorption effect on dyes. Figure 3 This is a particle size distribution diagram of the metallic glass powder prepared in Example 1. The diagram shows that the particle size range of the metallic glass powder is 8.7 to 52.5 μm, and the average particle size is 25.2 μm. Figure 4 The degradation curve of the metallic glass powder prepared in Example 1 and the blank control group under ultraviolet light for Rhodamine B dye. The initial concentration of Rhodamine B dye is 20 mg / L, the amount of catalyst added is 1 g / L, the amount of hydrogen peroxide (mass concentration 30%) added is 1 mL, and the light source is a mercury lamp with a rated power of 100 W. The results show that the Ti prepared in Example 1 50 Cu 40 Fe 10 The metallic glass powder has a very high photo-Fenton activity, with a degradation rate of up to 87% for rhodamine B within 4 minutes. In contrast, the 4-minute degradation rate of the blank control group (only hydrogen peroxide) was only 36%.

Claims

1. A method for preparing titanium-based metallic glass powder rich in double-strong Fenton active elements, Features The steps include: (1) selecting three metal powder raw materials of Ti, Cu and Fe, mixing them together with a process control agent and grinding balls, placing them in a sealed ball mill, wherein the atomic percentage of Ti element in the mixed metal powder is 40 to 60%, and the atomic ratio of Cu to Fe is 1:0.25 to 1:4; (2) providing a protective atmosphere for the mixed powder in the sealed ball milling jar, then installing the ball milling jar on a ball mill, starting the equipment for ball milling, and after a period of time, obtaining a titanium-based metallic glass catalytic material rich in two strong Fenton-active elements, Cu and Fe; Among them, the process control agent used in step (1) is stearic acid, and the addition amount is 1.0-4.0% of the total mass of the metal raw material; the materials of the grinding balls and the ball mill are both stainless steel, wherein the particle size range of the grinding balls is 5-10 mm, the capacity of the ball mill is 100 mL, and the ball-to-material ratio is 15:1-30:

1.

2. A method for preparing a titanium-based metallic glass powder rich in double-strong Fenton active elements according to claim 1, Features: After the ball milling process in step (2) is completed, the ball mill jar needs to be cooled for 3 hours under natural conditions, and then the jar is slowly opened, sieved, and the material is taken out, thereby obtaining pure titanium-based metallic glass powder.

3. The method for preparing a titanium-based metallic glass powder rich in double-strong Fenton active elements according to claim 1, Features: The impurity content in the metal powder raw material does not exceed 1wt%.

4. The method for preparing a titanium-based metallic glass powder rich in double-strong Fenton active elements according to claim 1, Features: The atomic percentage of Ti element in the mixed metal powder is 45-55%.

5. The method for preparing a titanium-based metallic glass powder rich in double-strong Fenton active elements according to claim 3, Features: The metal powder raw material has a purity of 99.9 wt %.

6. The method for preparing a titanium-based metallic glass powder rich in double-strong Fenton active elements according to claim 4, Features: The atomic percentage of Ti element in the mixed metal powder is 50%.

7. The method for preparing a titanium-based metallic glass powder rich in double-strong Fenton active elements according to claim 1, Features: The protective atmosphere in step (2) is argon with a purity of 99.9%, and vacuum needs to be drawn before filling with argon; the ball mill speed is 825-900 r / min, and it stops for 5 minutes after every 30 minutes of operation, and the system automatically changes the main disk rotation direction after each stop. The total ball milling time is 50 hours.

8. The method for preparing a titanium-based metallic glass powder rich in double-strong Fenton active elements according to claim 1, Features: In the step (1), the amount of stearic acid added is 1.7-2.6% of the total mass of the metal raw material, the grinding balls are composed of three particle sizes of 5, 8 and 10 mm, and the ball-to-material ratio is 20:1-26:

1.

9. The metallic glass powder obtained according to the method for preparing a titanium-based metallic glass powder rich in double-strong Fenton active elements according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Manufacture method of superfine laminar zinc powder and zinc pulp

    CN101391305A

  • Ti-based bulk metallic glass

    CN102108475A

  • Metallic glass composite material and preparation method thereof

    CN106636985A

  • Application of copper-based amorphous alloy as catalytic functional material in wastewater treatment