Diesel engine denitration catalyst and preparation method thereof
By regulating the morphology of vanadium and introducing phosphomolybdenum heteropoly acid with a specific structure, the performance of the vanadium-based SCR catalyst is improved, which solves the problem of performance degradation of the vanadium-based catalyst in high temperature environments and achieves efficient denitration performance in a wide temperature range. Meets the National VI emission standards for diesel engines.
Patent Information
- Application Number
- CN202210762031.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-06-29
AI Technical Summary
The performance of existing vanadium-based SCR catalysts is greatly reduced in high-temperature environments and cannot meet the application requirements of the National VI emission standards for diesel engines.
A diesel engine SCR catalyst composed of vanadium pentoxide V2O5, phosphomolybdenum heteropoly acid H5Mo12O41P, tungsten trioxide WO3, phosphorus pentoxide P2O5, silicon dioxide SiO2 and titanium dioxide TiO2 is used to control the form of vanadium through a high-temperature treatment process, and use Phosphoric acid and phosphomolybdenum heteropoly acid with a specific structure are used as assistants to control the redox and acid-base properties of the catalyst.
It maintains excellent denitration performance in a wide temperature range, has high temperature resistance, and achieves efficient denitration under low vanadium loading, meeting the application requirements of the National VI diesel engine standards.
Smart Images

Figure CN114950557B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a technology in the field of SCR catalysts, in particular to a diesel engine denitration catalyst and a preparation method thereof. Background Art
[0002] SCR technology is the most widely used denitrification technology at present, and its core lies in the catalyst. The current mainstream SCR catalysts are vanadium-based and copper molecular sieves. Although vanadium-based catalysts are widely used in fixed source SCR denitrification due to their low cost and strong sulfur resistance, they cannot meet the application requirements of the National VI emission standards for diesel engines due to their low performance and applicable temperature window. Therefore, it is of great significance to improve the denitrification performance of vanadium-based catalysts to meet the existing National VI copper molecular sieve standards.
[0003] Heteropolyacids (salts) have many special properties: the components are relatively simple, the structure is determined, and they have the structural characteristics of both complexes and metal oxides. Heteropolyacids (salts) are multi-electron oxidants and strong proton acids. Their oxidizability can be changed by changing the composition, which is beneficial to catalyst design; solid heteropolyacids (salts) are thermally stable. These properties allow heteropolyacids (salts) to be used as homogeneous and heterogeneous oxidation catalysts and acid catalysts or bifunctional catalysts. However, there are few studies on the application of heteropolyacids in SCR catalysts. Summary of the invention
[0004] In view of the defects that the overall performance of existing vanadium-based SCR catalysts cannot meet the application requirements of the National VI standard for diesel engines and the performance will be greatly reduced under high temperature environment, the present invention proposes a diesel engine denitrification catalyst and a preparation method thereof, which has excellent denitrification performance in a wide temperature range, and has a simple preparation process and high economy.
[0005] The present invention is achieved through the following technical solutions:
[0006] The present invention relates to a diesel engine SCR catalyst, comprising a carrier and a coating, wherein the components and mass percentage contents of the coating are: vanadium pentoxide V2O5: 1-2%, phosphorus molybdenum heteropoly acid H5Mo 12 O 41 P: 1-2%, tungsten trioxide WO3: 5-10%, phosphorus pentoxide P2O5: 1-2%, silicon dioxide SiO2: 5% and titanium dioxide TiO2: 80-85%.
[0007] The carrier is made of, but not limited to, honeycomb cordierite.
[0008] The invention relates to a method for preparing the diesel engine SCR catalyst, which comprises the steps of adding phosphoric acid, vanadyl oxalate, ammonium metatungstate and titanium dioxide into deionized water in sequence, uniformly mixing the mixture and then drying and calcining the mixture to obtain an active powder, which is then further mixed with phosphomolybdic acid having a keggin structure, deionized water and liquid silica gel and coated on a carrier to obtain the active powder after final calcination.
[0009] The mass percentage ratio of the phosphoric acid, vanadyl oxalate, ammonium metatungstate, titanium dioxide and deionized water is: (1.9-4.1): (3.1-6.8): (6.1-13.5): 100: (100-110).
[0010] The dry calcination means: drying at 120°C first and then calcining at a temperature of 650-700°C. The high-temperature pre-calcination obtains the required vanadium form, thereby improving the denitration performance.
[0011] The mass percentage ratio of the phosphomolybdic acid, deionized water, liquid silica gel and active powder is: (1.1-2.2): (100-110): 21.5: 100.
[0012] The coating is preferably carried out by vacuuming with feeding from below, with a slurry viscosity of 1000-2000 Pa·s, a solid content of 40-50%, and a loading of 150-250 g / L.
[0013] The final calcination temperature is 400-450°C.
[0014] Technical Effects
[0015] The present invention uses a high-temperature treatment process for active powders to regulate the morphology of vanadium, and uses phosphoric acid as an auxiliary agent to promote the generation of polymerized vanadium. The prepared catalyst has high temperature resistance and obtains excellent denitration performance at a low vanadium loading, thereby having a wide temperature range. In addition, a phosphorus molybdenum heteropoly acid with a specific structure is used as an auxiliary agent, and its addition time and post-treatment conditions are controlled to regulate the redox property of the catalyst and the acidity and alkalinity, further improving the performance of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a comparison diagram of the effects of the embodiments. DETAILED DESCRIPTION Example 1
[0017] This embodiment relates to a diesel engine SCR catalyst, and its preparation method includes:
[0018] Step 1: Dissolve 7.3 g of 85% phosphoric acid, 18.2 g of vanadyl oxalate pentahydrate, and 30.0 g of ammonium metatungstate in 400 ml of deionized water, and stir until completely dissolved to obtain active solution 1;
[0019] Step 2: Add 383g of titanium dioxide into the active solution 1, stir evenly, dry at 120°C, and then calcine at a maximum temperature of 650°C to obtain active powder 1;
[0020] Step 3: Mix 6.8 g of phosphomolybdic acid, 90 g of liquid silica gel, active powder 1 and 450 ml of deionized water to obtain active slurry 1;
[0021] Step 4: coating the active slurry on the cordierite carrier, the slurry viscosity during coating was 1320 Pa·s, the solid content was 46.5%, after drying at 120°C, calcining at a maximum temperature of 450°C to obtain the product, and the loading amount was 240 g / L; Example 2
[0022] This embodiment relates to a diesel engine SCR catalyst, which is different from the embodiment 1 in that the maximum calcination temperature of the active powder is 700°C. Comparative Example 1
[0023] This embodiment relates to a diesel engine SCR catalyst, which is different from the embodiment 1 in that the maximum calcination temperature of the active powder is 600°C. Comparative Example 2
[0024] This embodiment relates to a diesel engine SCR catalyst, which is different from the embodiment 1 in that the maximum calcination temperature of the active powder is 750°C. Comparative Example 3
[0025] This embodiment relates to a diesel engine SCR catalyst, which is different from Embodiment 1 in that the calcination temperature of the final product is 500°C. Comparative Example 4
[0026] This embodiment relates to a diesel engine SCR catalyst, which is different from Embodiment 1 in that ammonium heptamolybdate is used instead of phosphomolybdic acid. Comparative Example 5
[0027] This embodiment relates to a diesel engine SCR catalyst, which is different from Embodiment 1 in that phosphoric acid is not added during the preparation of the active solution, but is added to the final product by impregnation. Comparative Example 6
[0028] This embodiment relates to a diesel engine SCR catalyst, which differs from Embodiment 1 in that commercial National VI copper molecular sieve is used and samples of the same size are cut.
[0029] The above eight products were prepared at a space velocity of 50000h -1, 200-400℃, H2O: 5%, O2: 5%, NO: 300ppm, NH3: 330ppm, heating rate 20℃ / min, denitration performance test was carried out under the initial stable temperature of 130℃. The specific test content is as follows (the test method is: using a blank carrier, adjusting the parameters of each flow meter according to the above flue gas conditions and reaching the required value, recording the NO concentration at the reactor outlet after stabilization at 130℃ (as the calculated value of the NO concentration at the inlet of the test sample), replacing the blank carrier with the test sample, setting the heating rate after stabilization at 130℃, using a Fourier infrared flue gas analyzer to monitor the outlet flue gas parameters online, calculating the denitration efficiency based on these two values, and obtaining the temperature and efficiency relationship curve):
[0030] Test results such as Figure 1 As shown, it can be seen from the figure that the main reason for the low performance of comparative example 1 is that the calcination temperature of the active powder is insufficient, resulting in the failure to generate polymeric vanadium; the main reason for the low performance of comparative example 2 is that the calcination temperature of the active powder is too high, resulting in the production of rutile phase in part of the titanium dioxide (if only tungsten is added, the rutile phase temperature is about 620°C, if tungsten is not added, the rutile phase temperature is about 580°C, and the simultaneous addition of phosphorus and tungsten helps to improve its anti-sintering performance, thereby providing conditions for the production of polymeric vanadium); the main reason for the low performance of comparative example 3 is that phosphomolybdic acid is unstable at high temperatures and loses the required keggin structure; the main reason for the low performance of comparative example 4 is similar to that of comparative example 3, which is a heteropolyacid without a keggin structure, so the two sets of data are close; the main reason for the low performance of comparative example 5 is that the final product is impregnated with phosphoric acid, which will cause phosphorus to combine with the active component, thereby reducing the catalytic activity, and when phosphoric acid is added in the preparation of the active powder, phosphoric acid will combine with and fix titanium and tungsten, and at the same time occupy the position of vanadium on the carrier, promoting the formation of polymeric vanadium. In contrast, the performance of Examples 1 and 2 has been greatly improved, reaching or even exceeding the commercial National VI copper molecular sieve catalyst. The reasons are: ① Compared with dispersed vanadium, polymerized vanadium has stronger denitrification activity, but polymerized vanadium can generally be obtained at a high vanadium loading, and the high-vanadium catalyst has poor high-temperature performance. The polymerized vanadium is obtained at a low vanadium loading by means of phosphoric acid and high-temperature calcination. At the same time, the addition of phosphorus and tungsten improves the thermal stability of titanium dioxide and prevents it from rutile at this calcination temperature. ② The introduction of a specific structure of phosphomolybdic heteropoly acid optimizes the redox and acidity and alkalinity of the catalyst, while controlling the preparation conditions to ensure the integrity of its characteristic structure.
[0031] In summary, the present invention significantly improves the performance of the vanadium-based SCR catalyst by regulating the morphology of vanadium and introducing phosphomolybdic heteropoly acid, so that it can meet the application requirements of the National VI standard for diesel engines.
[0032] The above-mentioned specific implementation can be partially adjusted in different ways by those skilled in the art without departing from the principle and purpose of the present invention. The protection scope of the present invention shall be based on the claims and shall not be limited by the above-mentioned specific implementation. Each implementation scheme within its scope shall be subject to the constraints of the present invention.
Claims
1. A method for preparing a diesel engine SCR catalyst, characterized in that: The active powder is obtained by sequentially adding phosphoric acid, vanadyl oxalate, ammonium metatungstate and titanium dioxide into deionized water, uniformly mixing, drying and calcining, and then further mixing with phosphomolybdic acid having a keggin structure, deionized water and liquid silica gel, coating the mixture on a carrier, and finally calcining to obtain the active powder; The diesel engine SCR catalyst comprises a carrier and a coating, the components and mass percentage of the coating are: vanadium pentoxide V2O5: 1-2%, phosphorus molybdenum heteropoly acid H5Mo 12 O 41 P: 1-2%, tungsten trioxide WO3: 5-10%, phosphorus pentoxide P2O5: 1-2%, silicon dioxide SiO2: 5% and titanium dioxide TiO2: 80-85%; The carrier is made of honeycomb cordierite; The mass ratio of the phosphoric acid, vanadyl oxalate, ammonium metatungstate, titanium dioxide and deionized water is: (1.9-4.1): (3.1-6.8): (6.1-13.5): 100: (100-110); The mass ratio of the phosphomolybdic acid, deionized water, liquid silica gel and active powder is: (1.1-2.2): (100-110): 21.5: 100; The drying and calcining means: drying at 120°C first and then calcining at a temperature of 650-700°C. The high-temperature pre-calcination obtains the required vanadium form, thereby improving the denitration performance; The final calcination temperature is 400-450°C.
2. The preparation method according to claim 1, characterized in that: The coating is carried out by vacuuming with feeding from below, the slurry has a viscosity of 1000-2000 Pa·s, a solid content of 40-50%, and a loading capacity of 150-250 g / L.