A method for manufacturing environmentally friendly packaging bags using waste textiles
By cleaning and adding specific additives to waste PET textiles, environmentally friendly packaging bags are prepared, which solves the problem of performance degradation of waste textile packaging bags under external influence, and achieves the long-term stability of the material and environmentally friendly degradability.
Patent Information
- Application Number
- CN202210761183.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-06-30
AI Technical Summary
Packaging bags prepared from waste textiles may deteriorate under the influence of heat, ultraviolet light, oxygen, mechanical stress, high-energy radiation, electric fields, and microorganisms, resulting in a decline in material performance and affecting the normal use of plastic packaging bags.
By cleaning, sterilizing and breaking and loosening waste PET textiles, low-density polyethylene, photooxygen inhibitors, polylactic acid, trithyl phosphate and aminopropyl triethoxysilane are added to the extruder for melt extrusion. After granulation, cooling and drying, blow molding is made into a film to prepare an environmentally friendly packaging bag.
提高了包装袋的抗老化性能,保持了力学性能的良好状态,并通过生物降解材料保护环境。
Smart Images

Figure BDA0003724283940000031 
Figure BDA0003724283940000041 
Figure BDA0003724283940000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling waste textiles, and in particular to a method for manufacturing an environmentally friendly packaging bag by utilizing waste textiles. Background Art
[0002] Packaging bags are used to wrap the surface of products, forming a very light and protective appearance around the products, so as to achieve the purpose of dustproof, oilproof, moisture-proof, waterproof and sun-proof, and effectively protect the products. Plastic packaging bags are made of plastic as raw materials and are widely used in industrial production and daily life. Most plastics are light in weight and have stable chemical properties. They will not rust. Plastics usually have good impact resistance, wear resistance and transparency. Plastics have excellent insulation and low thermal conductivity.
[0003] Commonly used plastic packaging bags are mostly polyethylene plastic films or polypropylene plastic films, which are odorless and non-toxic. However, whether it is polyethylene plastic film or polypropylene plastic film, a large amount of polyethylene or polypropylene raw materials are required, which has high production costs. When packaging some products with low packaging requirements, a large amount of resources are wasted. Polyester fiber is the chemical fiber with the largest output, and the main variety of polyester fiber is polyethylene terephthalate (PET). At present, the recycling and regeneration technology of non-fiber polyester represented by polyester bottles at home and abroad is relatively mature, while the recycling technology of waste polyester textiles is still in its infancy. Therefore, using recycled waste polyester textiles to prepare packaging bags can not only reduce production costs and reduce resource waste, but also protect the environment and the process is simple. However, packaging bags prepared from waste textiles may deteriorate under the influence of heat, ultraviolet light, oxygen, mechanical stress, high-energy radiation, electric fields, and microorganisms, resulting in deterioration of material properties, such as yellowing, decreased relative molecular weight, cracking on the surface of the product, and loss of gloss. What is more serious is that it leads to a significant decrease in mechanical properties such as impact strength, flexural strength, tensile strength and elongation, thereby affecting the normal use of plastic packaging bags. Therefore, in order to enable plastic packaging bags to protect products for a long time, a method for manufacturing environmentally friendly packaging bags using waste textiles is urgently needed to solve the above problems. Summary of the invention
[0004] In order to overcome the above-mentioned technical problems, the purpose of the present invention is to provide a method for manufacturing environmentally friendly packaging bags using waste textiles: by cleaning and sterilizing waste PET textiles, then crushing and loosening them to obtain pretreated waste PET textiles, adding the pretreated waste PET textiles, low-density polyethylene, light-oxidation inhibitor, polylactic acid, tricresyl phosphate and aminopropyl triethoxysilane to an extruder for melt extrusion, granulating them with a granulator, and obtaining recycled plastic particles after cooling, drying the recycled plastic particles, and then blow-molding them into films, and obtaining environmentally friendly packaging bags after cutting and shaping, thereby solving the problem that the existing packaging bags made of waste textiles may deteriorate during use, resulting in deterioration of material properties, thereby affecting the normal use of plastic packaging bags.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for manufacturing an environmentally friendly packaging bag using waste textiles comprises the following steps:
[0007] Step 1: Weigh 70-90 parts of waste PET textiles, 50-60 parts of low-density polyethylene, 5-15 parts of light-oxidation inhibitor, 40-50 parts of polylactic acid, 3-7 parts of tricresyl phosphate and 6-12 parts of aminopropyltriethoxysilane according to weight;
[0008] Step 2: washing and sterilizing the waste PET textiles, and then crushing and loosening them to obtain pretreated waste PET textiles, adding the pretreated waste PET textiles, low-density polyethylene, light-oxidation inhibitor, polylactic acid, tricresyl phosphate and aminopropyl triethoxysilane into an extruder for melt extrusion, granulating them in a granulator, and obtaining recycled plastic pellets after cooling;
[0009] Step 3: Dry the recycled plastic pellets, blow them into film, cut and shape them to obtain environmentally friendly packaging bags.
[0010] As a further solution of the present invention: the photo-oxidation inhibitor is prepared by the following steps:
[0011] S1: Add methyl acrylate and anhydrous methanol to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, introduce nitrogen protection, add the mixed solution dropwise while stirring at a temperature of -5-0°C and a stirring rate of 300-400r / min, and control the dropping rate to 1-2 drops / s. After the addition is completed, continue to stir and react for 30-50 minutes, then heat to 20-25°C and continue to stir and react for 20-30 hours. After the reaction is completed, the reaction product is rotary evaporated to remove the solvent and unreacted methyl acrylate, and then placed in a vacuum drying oven and dried at a temperature of 40-45°C for 20-30 hours to obtain intermediate 1;
[0012] The reaction principle is as follows:
[0013]
[0014] S2: Add ethylenediamine and anhydrous methanol to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, introduce nitrogen protection, add the intermediate 1 solution dropwise while stirring at a temperature of -5-0°C and a stirring rate of 300-400r / min, and control the dropping rate to 1-2 drops / s. After the addition is completed, continue to stir and react for 30-50 minutes, then heat to 20-25°C and continue to stir and react for 20-30 hours. After the reaction is completed, the reaction product is rotary evaporated to remove the solvent and unreacted ethylenediamine, and then placed in a vacuum drying oven and dried at a temperature of 40-45°C for 20-30 hours to obtain intermediate 2;
[0015] The reaction principle is as follows:
[0016]
[0017] S3: Add deionized water, 2,2,6,6-tetramethylpiperidinol and magnesium hydroxide to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, stir for 1-1.5h at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat to 80-85°C and add hydrogen peroxide solution dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the addition is completed, continue to stir and react for 8-10h. After the reaction is completed, cool the reaction product to room temperature, vacuum filter, add manganese dioxide to the filtrate, and then heat to 60-65°C and stir and react for 1-1.5h. After the reaction is completed, cool the reaction product to room temperature, vacuum filter, and remove the solvent by rotary evaporation of the filtrate. Then place it in a vacuum drying oven and dry it at 60-65°C for 5-6h to obtain intermediate 3;
[0018] The reaction principle is as follows:
[0019]
[0020] S4: Add intermediate 3, n-octane, molybdenum trioxide and tert-butyl hydroperoxide aqueous solution into a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and heat to reflux while stirring at a stirring rate of 300-400 r / min. The heating rate is controlled to be 2-3°C / min, and then the stirring reaction is continued for 3-4 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. Sodium sulfite solution is added to the filtrate, and then the temperature is raised to 60-65°C and stirred for 30-50 minutes. After the reaction is completed, the reaction product is cooled to room temperature, allowed to stand for stratification, and the organic phase is dried over anhydrous magnesium sulfate, and then filtered. The filtrate is rotary evaporated to remove the solvent to obtain intermediate 4;
[0021] The reaction principle is as follows:
[0022]
[0023] S5: Add intermediate 4, dimethyl sebacate and tetraisopropyl titanate into a three-necked flask equipped with a stirrer and a thermometer, stir and react for 6-8 hours at a temperature of 180-190°C and a stirring rate of 300-400 r / min. After the reaction is completed, cool the reaction product to room temperature, wash it with distilled water 2-3 times, and then stand to separate the layers. Dry the organic phase with anhydrous magnesium sulfate, filter it, and place it in a vacuum drying oven at a temperature of 60-65°C for 5-6 hours to obtain intermediate 5;
[0024] The reaction principle is as follows:
[0025]
[0026] S6: Add intermediate 5 and anhydrous ethanol to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, introduce nitrogen protection, stir and react for 20-30 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then add sodium hydroxide solution dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the addition is completed, heat the temperature to 50-55°C and continue stirring and reacting for 4-5 hours. After the reaction is completed, cool the reaction product to room temperature, adjust the pH to 1-2 with concentrated hydrochloric acid, and then stand to precipitate, then vacuum filter, place the filter cake in a vacuum drying oven, and dry it at a temperature of 50-60°C for 20-30 hours to obtain intermediate 6;
[0027] The reaction principle is as follows:
[0028]
[0029] S7: Add intermediate 6 and chloroform to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, add thionyl chloride dropwise while stirring at a temperature of 45-50°C and a stirring rate of 300-400 r / min, and control the dropping rate to be 1-2 drops / s. After the addition is completed, continue stirring and reacting for 6-8 hours. After the reaction is completed, cool the reaction product to room temperature, and then remove the solvent and unreacted thionyl chloride by rotary evaporation to obtain intermediate 7;
[0030] The reaction principle is as follows:
[0031]
[0032] S8: Add intermediate 2, potassium carbonate and deionized water to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, stir for 25-35 minutes at a temperature of -5-0°C and a stirring rate of 300-400r / min, then add intermediate 7 solution dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the addition is completed, heat the temperature to 25-30°C and continue stirring to react for 20-30 hours. After the reaction is completed, vacuum filter the reaction product, wash the filter cake with distilled water 2-3 times, and then place it in a vacuum drying oven and dry it at a temperature of 50-55°C for 6-8 hours to obtain a photo-oxidation inhibitor.
[0033] The reaction principle is as follows:
[0034]
[0035] As a further solution of the present invention: the usage ratio of the methyl acrylate, anhydrous methanol and the mixed liquid in step S1 is 0.4 mol:40-50 mL:40-50 mL, and the mixed liquid is a mixture formed by dissolving ethylenediamine in anhydrous methanol at a ratio of 0.05 mol:20-25 mL.
[0036] As a further solution of the present invention: the usage ratio of the ethylenediamine, anhydrous methanol and intermediate 1 in step S2 is 0.4 mol:50-60 mL:30-35 mL, and the intermediate 1 solution is a solution formed by dissolving the intermediate 1 in anhydrous methanol at a ratio of 0.1 mol:30 mL.
[0037] As a further solution of the present invention: the usage ratio of the deionized water, 2,2,6,6-tetramethylpiperidinol, magnesium hydroxide, hydrogen peroxide solution and manganese dioxide in step S3 is 25-30 mL: 0.1 mol: 0.8-1.0 g: 25-30 g: 0.1-0.15 g, and the mass fraction of the hydrogen peroxide solution is 30%.
[0038] As a further scheme of the present invention: the dosage ratio of the intermediate 3, n-octane, molybdenum trioxide, tert-butyl hydroperoxide aqueous solution and sodium sulfite solution in step S4 is 0.05 mol: 55-60 g: 0.12-0.15 g: 25-30 g: 100-150 mL, the mass fraction of the tert-butyl hydroperoxide aqueous solution is 70%, and the mass fraction of the sodium sulfite solution is 20%.
[0039] As a further solution of the present invention: the usage ratio of the intermediate 4, dimethyl sebacate and tetraisopropyl titanate in step S5 is 0.1 mol: 0.1 mol: 0.15-0.25 g.
[0040] As a further solution of the present invention: the usage ratio of the intermediate 5, anhydrous ethanol and sodium hydroxide solution in step S6 is 0.2 mol: 100-120 mL: 80-100 g, the mass fraction of the sodium hydroxide solution is 15%, and the mass fraction of the concentrated hydrochloric acid is 36-38%.
[0041] As a further solution of the present invention: the intermediate 2 in step S7, chloroform and 0.2 mol of dichlorothionyl: 100-120 mL: 30-40 mL.
[0042] As a further scheme of the present invention: the usage ratio of the intermediate 2, potassium carbonate, deionized water and intermediate 7 solution in step S8 is 5mmol:0.055-0.060g:40-50mL:20-30mL, and the intermediate 7 solution is a solution formed by dissolving the intermediate 7 in chloroform at a ratio of 0.02mol:10-12mL.
[0043] Beneficial effects of the present invention:
[0044] The invention discloses a method for manufacturing an environmentally friendly packaging bag using waste textiles. The method comprises the following steps: washing and sterilizing waste PET textiles, and then crushing and loosening them to obtain pretreated waste PET textiles; adding the pretreated waste PET textiles, low-density polyethylene, a light-oxidation inhibitor, polylactic acid, tricresyl phosphate and aminopropyl triethoxysilane into an extruder for melt extrusion; granulating the pretreated waste PET textiles with a granulator; cooling the pretreated waste PET textiles to obtain recycled plastic pellets; drying the recycled plastic pellets; and then blowing the recycled plastic pellets into films; and cutting and shaping the pretreated waste PET textiles to obtain environmentally friendly packaging bags. In the method, the waste PET textiles are firstly processed, and the packaging bags are prepared with the waste PET textiles as the main raw materials, thereby reducing environmental pollution, saving production costs, and achieving the purpose of resource recycling and reuse. The light-oxidation inhibitor is added thereto to inhibit the light-oxidation of the packaging bags, thereby improving the anti-aging performance of the packaging bags, and maintaining good mechanical properties for a long time. The polylactic acid is added thereto to enable the waste packaging bags to be quickly biodegraded, thereby protecting the environment.
[0045] In the process of preparing the environmentally friendly packaging bag, a photo-oxidation inhibitor is also prepared. First, the alkenyl group on methyl acrylate is reacted with the amino group on ethylenediamine to introduce a large number of ester groups into ethylenediamine to obtain intermediate 1. Then, intermediate 1 reacts with ethylenediamine again to form an amide bond, and a large number of amino groups are introduced to obtain intermediate 2. 2,2,6,6-tetramethylpiperidinol is treated with hydrogen peroxide to connect oxygen free radicals to obtain intermediate 3. Then, the oxygen free radical on intermediate 3 reacts with n-octane to introduce alkyl groups thereto to enhance its lipophilicity and stability to obtain intermediate 4. Then, the hydroxyl group on intermediate 4 undergoes an ester exchange reaction with dimethyl sebacate to introduce ester groups to obtain intermediate 5. Then, the ester group on intermediate 5 is hydrolyzed under alkaline conditions, and then acidified to form carboxyl groups to obtain intermediate 6. Then, intermediate 6 reacts with dithionyl chloride to convert the carboxyl groups into hydroxyl groups. The intermediate 7 is converted into an acyl chloride group, and then the amino group on the intermediate 2 reacts with the acyl chloride group on the intermediate 7 to undergo a nucleophilic substitution reaction, thereby introducing a large number of hindered amine groups into the intermediate 2 to obtain a photo-oxidation inhibitor; the large number of hindered amine groups on the photo-oxidation inhibitor can be converted into corresponding nitroxide free radicals under oxidative conditions such as heat and light, which can effectively capture the alkyl free radicals and alkoxy free radicals in the high molecular polymer, making them inactive, and generating corresponding esters and peroxy esters, which will continue to react with the alkyl free radicals, alkoxy free radicals and peroxy free radicals in the polymer, and will regenerate nitroxide free radicals while generating corresponding compounds, and the generated nitroxide free radicals can recapture the free radicals generated by light induction in the high molecular polymer, thereby inhibiting the degradation of the high molecular material, and the regeneration ability can maintain the excellent properties of the high molecular material for a long time. DETAILED DESCRIPTION
[0046] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] Embodiment 1:
[0048] This embodiment is a method for preparing a photo-oxidation inhibitor, comprising the following steps:
[0049] S1: 0.4 mol of methyl acrylate and 40 mL of anhydrous methanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, and nitrogen was introduced for protection. At a temperature of -5°C and a stirring rate of 300 r / min, a mixed solution of 40 mL of ethylenediamine dissolved in anhydrous methanol at a ratio of 0.05 mol:20 mL was added dropwise while stirring. The dropping rate was controlled to be 1 drop / s. After the addition was completed, the reaction was continued to stir for 30 minutes, and then the temperature was raised to 20°C and the reaction was continued to stir for 20 hours. After the reaction was completed, the reaction product was rotary evaporated to remove the solvent and unreacted methyl acrylate, and then placed in a vacuum drying oven and dried at a temperature of 40°C for 20 hours to obtain intermediate 1;
[0050] S2: 0.4 mol of ethylenediamine and 50 mL of anhydrous methanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, and nitrogen was introduced for protection. Under the conditions of -5°C and a stirring rate of 300 r / min, 30 mL of the intermediate 1 solution formed by dissolving 0.1 mol:30 mL of the intermediate 1 in anhydrous methanol was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the stirring reaction was continued for 30 minutes, and then the temperature was raised to 20°C and the stirring reaction was continued for 20 hours. After the reaction was completed, the reaction product was rotary evaporated to remove the solvent and unreacted ethylenediamine, and then placed in a vacuum drying oven and dried at 40°C for 20 hours to obtain intermediate 2;
[0051] S3: 25 mL of deionized water, 0.1 mol of 2,2,6,6-tetramethylpiperidinol and 0.8 g of magnesium hydroxide were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and stirred at 25°C and a stirring rate of 300 r / min for 1 h. Then, 25 g of a 30% hydrogen peroxide solution was added dropwise while heating to 80°C, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the reaction was continued to stir for 8 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. 0.1 g of manganese dioxide was added to the filtrate, and then the temperature was raised to 60°C and stirred for 1 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filtrate was rotary evaporated to remove the solvent, and then placed in a vacuum drying oven and dried at 60°C for 5 h to obtain intermediate 3.
[0052] S4: 0.05 mol of intermediate 3, 55 g of n-octane, 0.12 g of molybdenum trioxide and 25 g of 70% aqueous tert-butyl hydroperoxide solution were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and the mixture was heated to reflux while stirring at a stirring rate of 300 r / min. The heating rate was controlled to be 2°C / min, and the stirring reaction was continued for 3 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. 100 mL of 20% sodium sulfite solution was added to the filtrate, and then the temperature was raised to 60°C and stirred for 30 min. After the reaction was completed, the reaction product was cooled to room temperature, allowed to stand for stratification, and the organic phase was dried over anhydrous magnesium sulfate, and then filtered. The filtrate was rotary evaporated to remove the solvent to obtain intermediate 4;
[0053] S5: 0.1 mol of intermediate 4, 0.1 mol of dimethyl sebacate and 0.15 g of tetraisopropyl titanate were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for 6 h at a temperature of 180°C and a stirring rate of 300 r / min. After the reaction, the reaction product was cooled to room temperature, washed with distilled water twice, and then allowed to stand for stratification. The organic phase was dried with anhydrous magnesium sulfate, filtered, and placed in a vacuum drying oven and dried at 60°C for 5 h to obtain intermediate 5;
[0054] S6: 0.2 mol of intermediate 5 and 100 mL of anhydrous ethanol were added to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, and nitrogen was introduced for protection. The mixture was stirred at 25°C and a stirring rate of 300 r / min for 20 min, and then 80 g of a 15% sodium hydroxide solution was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the temperature was raised to 50°C and the stirring reaction was continued for 4 h. After the reaction was completed, the reaction product was cooled to room temperature, and the pH was adjusted to 1 with 36% concentrated hydrochloric acid. The mixture was then allowed to stand to precipitate, and then vacuum filtered. The filter cake was placed in a vacuum drying oven and dried at 50°C for 20 h to obtain intermediate 6;
[0055] S7: 0.2 mol of intermediate 6 and 100 mL of chloroform were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and 30 mL of thionyl chloride was added dropwise while stirring at a temperature of 45°C and a stirring rate of 300 r / min. The dropping rate was controlled to be 1 drop / s. After the addition was completed, the stirring reaction was continued for 6 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent and unreacted thionyl chloride were removed by rotary evaporation to obtain intermediate 7;
[0056] S8: Add 5mmol of intermediate 2, 0.055g of potassium carbonate and 40mL of deionized water into a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, stir for 25-35min at a temperature of -5°C and a stirring rate of 300-400r / min, then add dropwise 20mL of intermediate 7 dissolved in chloroform at a ratio of 0.02mol:10mL while stirring, and control the dropping rate to 1 drop / s. After the addition is completed, heat the temperature to 25°C and continue stirring for 20h. After the reaction is completed, vacuum filter the reaction product, wash the filter cake twice with distilled water, and then place it in a vacuum drying oven and dry it at 50°C for 6h to obtain a photo-oxidation inhibitor.
[0057] Embodiment 2:
[0058] This embodiment is a method for preparing a photo-oxidation inhibitor, comprising the following steps:
[0059] S1: 0.4 mol of methyl acrylate and 50 mL of anhydrous methanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, and nitrogen was introduced for protection. At a temperature of 0°C and a stirring rate of 400 r / min, a mixed solution of 50 mL of ethylenediamine dissolved in anhydrous methanol at a ratio of 0.05 mol:25 mL was added dropwise while stirring. The dropping rate was controlled to be 2 drops / s. After the addition was completed, the reaction was continued to stir for 50 minutes, and then the temperature was raised to 25°C and the reaction was continued to stir for 30 hours. After the reaction was completed, the reaction product was rotary evaporated to remove the solvent and unreacted methyl acrylate, and then placed in a vacuum drying oven and dried at a temperature of 45°C for 30 hours to obtain intermediate 1;
[0060] S2: 0.4 mol of ethylenediamine and 60 mL of anhydrous methanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, and nitrogen was introduced for protection. At a temperature of 0°C and a stirring rate of 400 r / min, 35 mL of the intermediate 1 solution formed by dissolving 0.1 mol:30 mL of the intermediate 1 in anhydrous methanol was added dropwise while stirring, and the dropping rate was controlled to be 2 drops / s. After the addition was completed, the stirring reaction was continued for 50 minutes, and then the temperature was raised to 25°C and the stirring reaction was continued for 30 hours. After the reaction was completed, the reaction product was rotary evaporated to remove the solvent and unreacted ethylenediamine, and then placed in a vacuum drying oven and dried at a temperature of 45°C for 30 hours to obtain intermediate 2;
[0061] S3: 30 mL of deionized water, 0.1 mol of 2,2,6,6-tetramethylpiperidinol and 1.0 g of magnesium hydroxide were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and stirred for 1.5 h at a temperature of 30°C and a stirring rate of 400 r / min. Then, 30 g of a 30% hydrogen peroxide solution was added dropwise while heating to 85°C, and the dropping rate was controlled to be 2 drops / s. After the addition was completed, the stirring reaction was continued for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. 0.15 g of manganese dioxide was added to the filtrate, and then the temperature was raised to 65°C and stirred for 1.5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. The filtrate was rotary evaporated to remove the solvent, and then placed in a vacuum drying oven and dried at 65°C for 6 h to obtain intermediate 3;
[0062] S4: 0.05 mol of intermediate 3, 60 g of n-octane, 0.15 g of molybdenum trioxide and 30 g of 70% by mass aqueous solution of tert-butyl hydroperoxide were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and the mixture was heated to reflux while stirring at a stirring rate of 400 r / min. The heating rate was controlled to be 3°C / min, and the stirring reaction was continued for 4 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered. 150 mL of 20% by mass sodium sulfite solution was added to the filtrate, and then the temperature was raised to 65°C and stirred for 50 minutes. After the reaction was completed, the reaction product was cooled to room temperature, allowed to stand for stratification, and the organic phase was dried over anhydrous magnesium sulfate, and then filtered. The filtrate was rotary evaporated to remove the solvent to obtain intermediate 4;
[0063] S5: 0.1 mol of intermediate 4, 0.1 mol of dimethyl sebacate and 0.25 g of tetraisopropyl titanate were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for 8 h at a temperature of 190°C and a stirring rate of 400 r / min. After the reaction, the reaction product was cooled to room temperature, washed with distilled water for 3 times, and then allowed to stand for stratification. The organic phase was dried with anhydrous magnesium sulfate, filtered, and placed in a vacuum drying oven and dried at a temperature of 65°C for 6 h to obtain intermediate 5;
[0064] S6: 0.2 mol of intermediate 5 and 120 mL of anhydrous ethanol were added to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, and nitrogen was introduced for protection. The mixture was stirred for 30 min at a temperature of 30°C and a stirring rate of 400 r / min. Then, 100 g of a 15% sodium hydroxide solution was added dropwise while stirring, and the dropping rate was controlled to be 2 drops / s. After the addition was completed, the temperature was raised to 55°C and the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and the pH was adjusted to 2 with 38% concentrated hydrochloric acid. Then, the mixture was allowed to stand to precipitate, and then vacuum filtered. The filter cake was placed in a vacuum drying oven and dried at 60°C for 30 h to obtain intermediate 6;
[0065] S7: 0.2 mol of intermediate 6 and 120 mL of chloroform were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel. 40 mL of thionyl chloride was added dropwise while stirring at a temperature of 50°C and a stirring rate of 400 r / min. The dropping rate was controlled to be 2 drops / s. After the addition was completed, the stirring reaction was continued for 8 hours. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent and unreacted thionyl chloride were removed by rotary evaporation to obtain intermediate 7;
[0066] S8: Add 5 mmol of intermediate 2, 0.060 g of potassium carbonate and 50 mL of deionized water into a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, stir for 35 min at a temperature of 0°C and a stirring rate of 400 r / min, then add dropwise 30 mL of intermediate 7 dissolved in chloroform at a ratio of 0.02 mol:12 mL while stirring, and control the dropping rate to 2 drops / s. After the addition is completed, heat the temperature to 30°C and continue stirring for 30 h. After the reaction is completed, vacuum filter the reaction product, wash the filter cake with distilled water 3 times, and then place it in a vacuum drying oven and dry it at 55°C for 8 h to obtain a photo-oxidation inhibitor.
[0067] Embodiment 3:
[0068] This embodiment is a method for manufacturing an environmentally friendly packaging bag using waste textiles, comprising the following steps:
[0069] Step 1: Weigh 70 parts of waste PET textiles, 50 parts of low-density polyethylene, 5 parts of the photo-oxidation inhibitor from Example 1, 40 parts of polylactic acid, 3 parts of tricresyl phosphate and 6 parts of aminopropyltriethoxysilane according to weight;
[0070] Step 2: washing and sterilizing the waste PET textiles, and then crushing and loosening them to obtain pretreated waste PET textiles, adding the pretreated waste PET textiles, low-density polyethylene, light-oxidation inhibitor, polylactic acid, tricresyl phosphate and aminopropyl triethoxysilane into an extruder for melt extrusion, granulating them in a granulator, and obtaining recycled plastic pellets after cooling;
[0071] Step 3: Dry the recycled plastic pellets, blow them into film, cut and shape them to obtain environmentally friendly packaging bags.
[0072] Embodiment 4:
[0073] This embodiment is a method for manufacturing an environmentally friendly packaging bag using waste textiles, comprising the following steps:
[0074] Step 1: Weigh 90 parts of waste PET textiles, 60 parts of low-density polyethylene, 15 parts of the photo-oxidation inhibitor from Example 2, 50 parts of polylactic acid, 7 parts of tricresyl phosphate and 12 parts of aminopropyltriethoxysilane according to weight;
[0075] Step 2: washing and sterilizing the waste PET textiles, and then crushing and loosening them to obtain pretreated waste PET textiles, adding the pretreated waste PET textiles, low-density polyethylene, light-oxidation inhibitor, polylactic acid, tricresyl phosphate and aminopropyl triethoxysilane into an extruder for melt extrusion, granulating them in a granulator, and obtaining recycled plastic pellets after cooling;
[0076] Step 3: Dry the recycled plastic pellets, blow them into film, cut and shape them to obtain environmentally friendly packaging bags.
[0077] Comparative Example 1:
[0078] The difference between Comparative Example 1 and Example 4 is that no photo-oxidation inhibitor is added.
[0079] Comparative Example 2:
[0080] The difference between Comparative Example 2 and Example 4 is that an ultraviolet absorber UV-O is used instead of the photo-oxidation inhibitor.
[0081] Comparative Example 3:
[0082] The difference between Comparative Example 3 and Example 4 is that light stabilizer 744 is used instead of the photo-oxidation inhibitor.
[0083] The performance of the environmentally friendly packaging bags of Examples 3-4 and Comparative Examples 1-3 was tested, and the test results are shown in the following table:
[0084]
[0085] Referring to the data in the above table, according to the comparison between Example 4 and Comparative Examples 1-3, it can be known that the addition of ultraviolet absorber UV-O, light stabilizer 744 and photo-oxidation inhibitor can significantly improve the ultraviolet resistance of the environmentally friendly packaging bag without substantially affecting the degradation performance of the environmentally friendly packaging bag, and improve its anti-aging performance, among which the photo-oxidation inhibitor has the best enhancement effect.
[0086] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0087] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for manufacturing environmentally friendly packaging bags using waste textiles, characterized in that: The following steps are involved: Step 1: Weigh 70-90 parts of waste PET textiles, 50-60 parts of low-density polyethylene, 5-15 parts of light-oxidation inhibitor, 40-50 parts of polylactic acid, 3-7 parts of tricresyl phosphate and 6-12 parts of aminopropyltriethoxysilane according to weight; Step 2: washing and sterilizing the waste PET textiles, and then crushing and loosening them to obtain pretreated waste PET textiles, adding the pretreated waste PET textiles, low-density polyethylene, light-oxidation inhibitor, polylactic acid, tricresyl phosphate and aminopropyl triethoxysilane into an extruder for melt extrusion, granulating them in a granulator, and obtaining recycled plastic pellets after cooling; Step 3: Dry the recycled plastic pellets, blow them into films, cut and shape them, and obtain environmentally friendly packaging bags; The photo-oxidation inhibitor is prepared by the following steps: S1: Add methyl acrylate and anhydrous methanol to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, introduce nitrogen protection, add the mixed solution dropwise while stirring at a temperature of -5-0°C and a stirring rate of 300-400r / min, and control the dropping rate to 1-2 drops / s. After the addition is completed, continue to stir and react for 30-50 minutes, then heat to 20-25°C and continue to stir and react for 20-30 hours. After the reaction is completed, the reaction product is rotary evaporated to remove the solvent and unreacted methyl acrylate, and then placed in a vacuum drying oven and dried at a temperature of 40-45°C for 20-30 hours to obtain intermediate 1; S2: Add ethylenediamine and anhydrous methanol to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a constant pressure dropping funnel, introduce nitrogen protection, add the intermediate 1 solution dropwise while stirring at a temperature of -5-0°C and a stirring rate of 300-400r / min, and control the dropping rate to 1-2 drops / s. After the addition is completed, continue to stir and react for 30-50 minutes, then heat to 20-25°C and continue to stir and react for 20-30 hours. After the reaction is completed, the reaction product is rotary evaporated to remove the solvent and unreacted ethylenediamine, and then placed in a vacuum drying oven and dried at a temperature of 40-45°C for 20-30 hours to obtain intermediate 2; S3: Add deionized water, 2,2,6,6-tetramethylpiperidinol and magnesium hydroxide to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, stir for 1-1.5h at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat to 80-85°C and add hydrogen peroxide solution dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the addition is completed, continue to stir and react for 8-10h. After the reaction is completed, cool the reaction product to room temperature, vacuum filter, add manganese dioxide to the filtrate, and then heat to 60-65°C and stir and react for 1-1.5h. After the reaction is completed, cool the reaction product to room temperature, vacuum filter, and remove the solvent by rotary evaporation of the filtrate. Then place it in a vacuum drying oven and dry it at 60-65°C for 5-6h to obtain intermediate 3; S4: Add intermediate 3, n-octane, molybdenum trioxide and tert-butyl hydroperoxide aqueous solution into a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and heat to reflux while stirring at a stirring rate of 300-400 r / min. The heating rate is controlled to be 2-3°C / min, and then the stirring reaction is continued for 3-4 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered. Sodium sulfite solution is added to the filtrate, and then the temperature is raised to 60-65°C and stirred for 30-50 minutes. After the reaction is completed, the reaction product is cooled to room temperature, allowed to stand for stratification, and the organic phase is dried over anhydrous magnesium sulfate, and then filtered. The filtrate is rotary evaporated to remove the solvent to obtain intermediate 4; S5: Add intermediate 4, dimethyl sebacate and tetraisopropyl titanate into a three-necked flask equipped with a stirrer and a thermometer, stir and react for 6-8 hours at a temperature of 180-190°C and a stirring rate of 300-400 r / min. After the reaction is completed, cool the reaction product to room temperature, wash it with distilled water 2-3 times, and then stand to separate the layers. Dry the organic phase with anhydrous magnesium sulfate, filter it, and place it in a vacuum drying oven at a temperature of 60-65°C for 5-6 hours to obtain intermediate 5; S6: Add intermediate 5 and anhydrous ethanol to a four-necked flask equipped with a stirrer, a thermometer, an air guide tube, a reflux condenser and a constant pressure dropping funnel, introduce nitrogen protection, stir and react for 20-30 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then add sodium hydroxide solution dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the addition is completed, heat the temperature to 50-55°C and continue stirring and reacting for 4-5 hours. After the reaction is completed, cool the reaction product to room temperature, adjust the pH to 1-2 with concentrated hydrochloric acid, and then stand to precipitate, then vacuum filter, place the filter cake in a vacuum drying oven, and dry it at a temperature of 50-60°C for 20-30 hours to obtain intermediate 6; S7: Add intermediate 6 and chloroform to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, add thionyl chloride dropwise while stirring at a temperature of 45-50°C and a stirring rate of 300-400 r / min, and control the dropping rate to be 1-2 drops / s. After the addition is completed, continue stirring and reacting for 6-8 hours. After the reaction is completed, cool the reaction product to room temperature, and then remove the solvent and unreacted thionyl chloride by rotary evaporation to obtain intermediate 7; S8: Add intermediate 2, potassium carbonate and deionized water to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, stir for 25-35 minutes at a temperature of -5-0°C and a stirring rate of 300-400r / min, then add intermediate 7 solution dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the addition is completed, heat the temperature to 25-30°C and continue stirring to react for 20-30 hours. After the reaction is completed, vacuum filter the reaction product, wash the filter cake with distilled water 2-3 times, and then place it in a vacuum drying oven and dry it at a temperature of 50-55°C for 6-8 hours to obtain a photo-oxidation inhibitor.
2. The method for manufacturing environmentally friendly packaging bags using waste textiles according to claim 1, characterized in that: The usage ratio of the methyl acrylate, anhydrous methanol and the mixed solution in step S1 is 0.4 mol:40-50 mL:40-50 mL, and the mixed solution is a mixture formed by dissolving ethylenediamine in anhydrous methanol at a ratio of 0.05 mol:20-25 mL.
3. The method for manufacturing environmentally friendly packaging bags using waste textiles according to claim 1, characterized in that: The usage ratio of the ethylenediamine, anhydrous methanol and intermediate 1 in step S2 is 0.4 mol:50-60 mL:30-35 mL, and the intermediate 1 solution is a solution formed by dissolving the intermediate 1 in anhydrous methanol at a ratio of 0.1 mol:30 mL.
4. The method for manufacturing environmentally friendly packaging bags using waste textiles according to claim 1, characterized in that: The usage ratio of the deionized water, 2,2,6,6-tetramethylpiperidinol, magnesium hydroxide, hydrogen peroxide solution and manganese dioxide in step S3 is 25-30 mL: 0.1 mol: 0.8-1.0 g: 25-30 g: 0.1-0.15 g, and the mass fraction of the hydrogen peroxide solution is 30%.
5. The method for manufacturing environmentally friendly packaging bags using waste textiles according to claim 1, characterized in that: The amount ratio of the intermediate 3, n-octane, molybdenum trioxide, tert-butyl hydroperoxide aqueous solution and sodium sulfite solution in step S4 is 0.05 mol: 55-60 g: 0.12-0.15 g: 25-30 g: 100-150 mL, the mass fraction of the tert-butyl hydroperoxide aqueous solution is 70%, and the mass fraction of the sodium sulfite solution is 20%.
6. The method for manufacturing environmentally friendly packaging bags using waste textiles according to claim 1, characterized in that: The usage ratio of the intermediate 4, dimethyl sebacate and tetraisopropyl titanate in step S5 is 0.1 mol: 0.1 mol: 0.15-0.25 g.
7. The method for manufacturing environmentally friendly packaging bags using waste textiles according to claim 2, characterized in that: The usage ratio of the intermediate 5, anhydrous ethanol and sodium hydroxide solution in step S6 is 0.2 mol: 100-120 mL: 80-100 g, the mass fraction of the sodium hydroxide solution is 15%, and the mass fraction of the concentrated hydrochloric acid is 36-38%.
8. The method for manufacturing environmentally friendly packaging bags using waste textiles according to claim 1, characterized in that: The intermediate 2 in step S7, chloroform and 0.2 mol of thionyl chloride: 100-120 mL: 30-40 mL.
9. The method for manufacturing environmentally friendly packaging bags using waste textiles according to claim 1, characterized in that: The usage ratio of the intermediate 2, potassium carbonate, deionized water and intermediate 7 solution in step S8 is 5 mmol: 0.055-0.060 g: 40-50 mL: 20-30 mL, and the intermediate 7 solution is a solution formed by dissolving the intermediate 7 in chloroform at a ratio of 0.02 mol: 10-12 mL.