A method for gradient reduction separation and recovery of iron and vanadium-titanium resources in vanadium-titanium magnetite

Through the gradient reduction and separation method, the problem of recovery of iron and vanadium titanium resources in vanadium titanium magnetite is solved, and the selective reduction and separation of vanadium titanium resources at low temperatures is realized, the energy consumption of electric furnaces and CO2 emissions are reduced, and the low-temperature chlorination is improved Efficiency and product purity enhance the environmental protection and economicality of the process.

CN115537548BActive Publication Date: 2024-11-15CHONGQING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211424324.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-14
Publication Date
2024-11-15
Estimated Expiration
2042-11-14

AI Technical Summary

Technical Problem

The prior art is difficult to effectively recover iron and vanadium titanium resources in vanadium titanium magnetite. In traditional methods, the reduction temperature is high and the time is long, and the impurity oxide is chlorinated during the low-temperature chlorination process, resulting in reactor clogging and product purity decrease. Low-temperature selective chlorination requires strict requirements on raw materials, and the carbon content and Fe content are difficult to control.

Method used

Gradient reduction separation methods are adopted, including low-temperature selective reduction, magnetic separation, reduction-carbon nitriding treatment and low-temperature chlorination. By regulating the components and temperature of the reduction gas, Ti(C with suitable O/(C+N) ratio is prepared. ,N,O) and V(C,N,O) raw materials avoid impurities chlorination and realize gradient selective reduction and separation and recovery of vanadium titanium resources.

Benefits of technology

The selective reduction of iron in vanadium-titanium magnetite and the separation of vanadium-titanium resources at lower temperatures, reduce the energy consumption of electric furnaces, reduce CO2 emissions, improve the efficiency of low-temperature chlorination and product purity, avoid impurities chlorination, and enhance the environmental protection of the process Sexual and economical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115537548B_ABST
    Figure CN115537548B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for gradient reduction separation and recovery of iron and vanadium-titanium resources in vanadium-titanium magnetite. The method uses one or more gases of CH4-H2 and CH4-H2-N2 as a reducing agent, selectively and controllably reduces the iron oxide in vanadium-titanium magnetite to Fe3C at low temperature, and separates Fe3C from vanadium-rich titanium material by magnetic separation process, and then uses CH4-H2-N2 mixed gas to reduce and carbonitride the vanadium-rich titanium material at a relatively low temperature, and the vanadium-rich titanium material after carbonitridation can be selectively chlorinated and separated by low-temperature chlorination of Ti (C, N, O) and V (C, N, O). The present invention can realize the gradient reduction and separation of iron and vanadium-titanium resources in vanadium-titanium magnetite at low temperature through a novel reduction method, and can accurately control the carbonitridation degree of vanadium-rich titanium material, effectively improve the subsequent low-temperature chlorination efficiency, realize the separation of vanadium-titanium components and impurities, and enrich scandium elements at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, and in particular to a method for recovering iron and vanadium and titanium from vanadium-titanium magnetite by gradient reduction and low-temperature chlorination separation. Background Art

[0002] Titanium is a very important structural metal. my country is a country with abundant titanium resources, but more than 90% of titanium resources exist in the Panxi area of ​​Sichuan in the form of vanadium-titanium magnetite. Panxi vanadium-titanium magnetite is a composite ore with cobalt, chromium, nickel, scandium, gallium, copper, selenium, tellurium, platinum and more than a dozen other rare and precious metals. It has a very high comprehensive utilization value, with a TiO2 grade of 7.82% to 15.78% and a V2O5 grade of 0.28% to 0.39%. Due to its complex mineral composition and element occurrence state, it is currently difficult to fully utilize all the valuable elements of Panxi vanadium-titanium magnetite, especially the simultaneous recycling of iron, vanadium and titanium resources.

[0003] Panxi vanadium-titanium magnetite generally undergoes multiple beneficiation processes to obtain vanadium-titanium magnetite concentrate and titanium concentrate. About 54% of the TiO2 in the vanadium-titanium magnetite enters the vanadium-titanium magnetite concentrate. The iron and vanadium elements in the vanadium-titanium magnetite concentrate can be recovered through the "blast furnace ironmaking-converter steelmaking vanadium slag-sodium vanadium extraction" process, but the titanium element in the vanadium-titanium magnetite concentrate will enter the slag to form a titanium-containing blast furnace slag containing about 25% TiO2, which has not been effectively utilized and can only be piled up in large quantities in the slag yard. In addition, the vanadium-titanium magnetite can also be selectively reduced under solid-state conditions by the reduction-grinding method, fully reducing the iron oxides therein to metallic iron, while the vanadium-titanium oxides remain unchanged, and then through grinding, magnetic separation and other processes to separate into iron powder concentrate and vanadium-rich titanium materials, and then the vanadium-rich titanium materials are processed to extract vanadium-titanium resources. However, the reduction-grinding method has strict requirements on the metallization rate of the reduced pellets (≥90%), so the reduction temperature is high, the reduction time is long, the vanadium and titanium oxides in the ore will also be partially reduced, and the subsequent separation rate of metallic iron and vanadium-rich titanium materials is low. At the same time, the iron powder concentrate obtained by the reduction-grinding method has a high impurity content and needs to be smelted and purified in an electric furnace, and the added value of the product is low.

[0004] For the subsequent purification of titanium-rich materials or vanadium-rich titanium materials, the most ideal method at present is to selectively recover the vanadium and titanium resources therein through the chlorination method. Compared with the sulfuric acid leaching process, the chlorination method has the advantages of short process, continuous production, large scale, less "three wastes" emissions, and good product properties. However, the traditional boiling chlorination temperature is high (above 800°C), and the quality requirements of raw materials are also high. The vanadium-rich titanium materials obtained by smelting Panxi vanadium-titanium magnetite have high impurity contents such as CaO, SiO2, and MgO. During the high-temperature chlorination process, these impurity oxides are easily chlorinated to form low-melting point chlorides, resulting in reactor blockage, increased chlorine consumption, and reduced purity of chlorinated products. Although the molten salt chlorination method has relatively loose requirements on the impurity content of titanium-rich materials, the chlorination tailings cannot be treated, and the environmental pollution is large. At the same time, it has high requirements on equipment and complex operation, which is not suitable for large-scale industrial production.

[0005] The low-temperature chlorination process (400-600°C) proposed in recent years can avoid the chlorination of calcium and magnesium impurities and achieve the selective chlorination of vanadium and titanium elements, but its raw materials are vanadium titanium carbonitrides (Ti(C,N), V(C,N)), so the vanadium-rich titanium material needs to be reduced-carbonitrided first. The traditional reduction-carbonitriding process generally uses C as a reducing agent and a carbonizing agent. Some C will remain in the vanadium-rich titanium material after carbonitriding. Ti(C,N) and V(C,N) will also produce C during the low-temperature chlorination process. Excessive C in the chlorination process will promote the chlorination of impurities such as calcium and magnesium, which will significantly reduce the low-temperature chlorination rate and the purity of the prepared chlorinated product. The low-temperature chlorination process also has strict requirements on the Fe content in the raw materials. Metallic iron will also be chlorinated to form low-melting FeCl3 during the low-temperature chlorination process. Excessive FeCl3 will also affect the low-temperature chlorination process. At the same time, although the temperature of low-temperature selective chlorination is lower than the chlorination temperature of impurity oxides such as CaO and MgO, the chlorination process of pure Ti(C,N) and V(C,N) is a strongly exothermic process, which will cause the temperature of the local reaction zone to be too high during the chlorination process, causing impurities such as calcium and magnesium to be chlorinated. Therefore, in the process of preparing low-temperature chlorination raw materials, if the carbon content in the raw materials can be reduced, the chlorination of impurities such as calcium and magnesium can be avoided during the low-temperature chlorination process, which will effectively improve the low-temperature chlorination efficiency of vanadium and titanium resources and reduce process costs. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for recovering iron and vanadium and titanium from vanadium-titanium magnetite with high low-temperature chlorination efficiency and less chlorination impurities.

[0007] In order to solve the above technical problems, the present invention adopts the following technical solution: a method for gradient reduction separation and recovery of iron and vanadium-titanium resources in vanadium-titanium magnetite, comprising the following steps:

[0008] S1: Grind the vanadium-titanium magnetite concentrate to obtain a powder raw material with a particle size of 0.1-0.15 mm, and then perform low-temperature selective reduction on the powder raw material under a reducing atmosphere, the reduction temperature is 570-700° C., the reduction time is 2-3 hours, the reducing atmosphere is CH4-H2-N2, and the volume proportion of each gas in the reducing atmosphere is: CH4 is 4-10%, H2 is 72-96%, and N2 is 0-20%;

[0009] S2: ball-milling the reduction-carbonitridation product obtained in S1 to a size below 0.074 mm, and magnetically separating the ball-milled material to obtain a magnetic material and a vanadium-rich titanium material;

[0010] S3: subjecting the vanadium-rich titanium material obtained in S2 to reduction-carbonitriding treatment, the reduction temperature is 1000-1100° C., the reduction time is 3-4 hours, and the reduction atmosphere is a CH4-H2-N2 mixed gas;

[0011] S4: The reduction-carbonitridation product obtained in S3 is crushed to less than 1 mm, and low-temperature chlorination is performed. The chlorination temperature is 280-450° C. and the chlorination time is 1-2 hours. After chlorination, a chlorinated product and chlorinated tailings are obtained.

[0012] As an improvement, the powder raw material obtained after grinding in S1 is first dried at a temperature of 100-200° C. and a heat preservation time of 4 hours.

[0013] As an improvement, the vanadium-titanium-rich material in S2 is a non-magnetic material, and the separation rate of Fe3C in the magnetic separation process is ≥95%.

[0014] As an improvement, the volume proportion of each gas in CH4-H2-N2 in S3 is: CH4 is 4-10%, N2 is 12-16%, and H2 is 74-80%.

[0015] As an improvement, the reduction-carbonitridation product in S4, i.e., the titanium-containing phase and the vanadium-containing phase in the low-temperature chlorination raw material, are Ti(C, N, O) and V(C, N, O), and O / (C+N) in the phase is ≥2, and the product does not contain deposited carbon.

[0016] Compared with the prior art, the present invention has at least the following advantages:

[0017] 1. In the traditional reduction-grinding method, the carbon thermal reduction reaction temperature is high, the reduction time is long, the carbon emission is high, and the vanadium titanium oxide in the ore is partially reduced, and the gradient selective reduction of iron and vanadium titanium resources in vanadium titanium magnetite cannot be achieved; the carbides of vanadium and titanium are all weakly magnetic, resulting in a low magnetic separation rate of the subsequent iron phase component. At the same time, the separated vanadium-rich titanium material has more impurity phases, containing a certain amount of metallic iron and solid carbon, and is difficult to be directly used in high-temperature boiling chlorination or low-temperature selective chlorination processes to recover vanadium titanium resources. The method of the present invention can selectively and controllably reduce the iron oxide in vanadium titanium magnetite to Fe3C at a relatively low temperature, while the vanadium titanium oxide in the ore remains unchanged. Compared with the iron powder concentrate obtained by the reduction-grinding method, the Fe3C product has high added value and can significantly reduce the energy consumption of the electric furnace when used for electric furnace smelting. The entire low-temperature selective reduction process is environmentally friendly and clean, with no CO2 emissions, and the tail gas can be recycled. In addition, Fe3C can be better separated from vanadium-rich titanium materials by magnetic separation. At the same time, the separated vanadium-rich titanium materials can be reduced-carbonitrided at a lower temperature (compared with traditional carbon thermal reduction), and then used in the subsequent low-temperature selective chlorination process to recover the vanadium and titanium resources therein, thereby realizing the gradient reduction and separation recovery of iron and vanadium and titanium resources in vanadium-titanium magnetite.

[0018] 2. The traditional chlorination process is high-temperature boiling chlorination with carbon addition. During the chlorination process, impurity oxides such as CaO and MgO will also be chlorinated to form low-melting chlorides, which will cause the adhesion of the chlorinated raw materials and affect the low-temperature chlorination process. At the same time, the low-temperature selective chlorination process has strict requirements on the carbon content and Fe content in the chlorinated raw materials. Pure Ti (C, N) and V (C, N) will produce excessive carbon during the low-temperature chlorination process, which will promote the chlorination reaction of impurities such as calcium and magnesium at low temperatures. Metallic iron will also be chlorinated during the low-temperature chlorination process to form low-melting FeCl3. Excessive FeCl3 will also affect the low-temperature chlorination process. The low-temperature chlorination raw materials prepared by the traditional carbon thermal reduction method have too much carbon content and residual Fe content, and the carbonization degree of Ti and V is difficult to control, which will seriously affect the subsequent low-temperature chlorination process. The method of the present invention selectively reduces and separates the iron and vanadium-titanium resources in the vanadium-titanium magnetite in a gradient manner, so that the low-temperature chlorination raw material prepared does not contain free carbon and has a low residual Fe content. At the same time, the carbonitriding degree of the vanadium-rich titanium material can be accurately controlled by regulating the reducing gas composition, the reducing temperature and the time, so as to control the O / (C+N) ratio of Ti(C,N,O) and V(C,N,O) to be ≥2, and the chlorination of impurities can be completely avoided in the subsequent low-temperature selective chlorination process, thereby ensuring the smooth progress of the low-temperature chlorination process.

[0019] 3. Although the temperature of low-temperature selective chlorination is lower than the chlorination temperature of impurity oxides such as CaO and MgO, the chlorination process of Ti(C,N) and V(C,N) is a strongly exothermic process, which will cause the temperature of the local reaction zone to be too high during the chlorination process, causing the impurity oxides such as CaO and MgO to be chlorinated. Ti(C,N,O) and V(C,N,O) with a suitable O / (C+N) ratio prepared by the method of the present invention can be selectively chlorinated at a lower temperature, and less heat is released during the chlorination process, which can effectively prevent impurities such as calcium and magnesium from being chlorinated due to excessively high local reaction temperatures, thereby ensuring the low-temperature selective chlorination rate and product purity.

[0020] 4. The present invention realizes the separation and recovery of iron and vanadium-titanium resources in vanadium-titanium magnetite concentrate and the enrichment of scandium. At the same time, due to the separation of TiO2 in the chlorinated tailings, oxides such as CaO are not chlorinated and can be further recycled. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The process flow diagram of the method of the present invention is shown in FIG. DETAILED DESCRIPTION

[0022] A method for separating and recovering iron and vanadium-titanium resources in vanadium-titanium magnetite by gradient reduction comprises the following steps:

[0023] S1: Grind the vanadium-titanium magnetite concentrate to obtain a powder raw material with a particle size of 0.1-0.15 mm, and then perform low-temperature selective reduction on the powder raw material under a reducing atmosphere, the reduction temperature is 570-700°C, the reduction time is 2-3h, the reducing atmosphere is aCH4-bH2-cN2, and the volume proportion of each gas in the reducing atmosphere is: CH4 is 4-10%, H2 is 72-96%, and N2 is 0-20%; the low-temperature selective reduction process in S1 can only reduce the iron oxide in the vanadium-titanium magnetite, and the reduction temperature of the vanadium-titanium oxide is higher than this temperature, and the reduction product of the iron oxide is Fe3C (magnetic substance).

[0024] S2: ball-milling the vanadium-titanium magnetite powder obtained in S1 after low-temperature selective reduction to a size below 0.074 mm, and magnetically separating the ball-milled material to obtain a magnetic material and a vanadium-rich titanium material;

[0025] S3: subjecting the vanadium-rich titanium material obtained in S2 to reduction-carbonitriding treatment, the reduction temperature is 1000-1100° C., the reduction time is 3-4 hours, and the reduction atmosphere is a CH4-H2-N2 mixed gas;

[0026] S4: The reduction-carbonitridation product obtained in S3 is crushed to less than 1 mm, and low-temperature chlorination is performed. The chlorination temperature is 280-450° C. and the chlorination time is 1-2 hours. After chlorination, a chlorinated product and chlorinated tailings are obtained.

[0027] Specifically, the powder raw material obtained after grinding in S1 is first dried at a temperature of 100-200° C. for 4 hours to remove moisture or volatile substances that may be contained in the raw material to avoid affecting the subsequent gas-based reduction process.

[0028] Specifically, the low-temperature selective reduction process in S1 can only reduce the iron oxide in the vanadium-titanium magnetite. The reduction temperature of the vanadium-titanium oxide is higher than this temperature, and the reduction product of the iron oxide is Fe3C (magnetic substance).

[0029] Specifically, the vanadium-rich titanium material in S2 is a non-magnetic material, and the separation rate of Fe3C in the magnetic separation process is ≥95%.

[0030] Specifically, the volume proportion of each gas in CH4-H2-N2 in S3 is: CH4 is 4-10%, N2 is 12-16%, and H2 is 74-80%. CH4 is mainly used as a reducing agent and a carbonizing agent, H2 is a reducing agent, and N2 is a nitriding agent. The gas products in the reduction-carbonitridation process are H2, N2, CO, and a trace amount of H2O.

[0031] The reduction-carbonitridation product in S4, i.e., the titanium-containing phase and the vanadium-containing phase in the low-temperature chlorination raw material are Ti(C, N, O) and V(C, N, O), and O / (C+N) in the phase is ≥2, and the product does not contain deposited carbon.

[0032] The low-temperature chlorination reaction type in S4 is boiling chlorination, and the collected chlorination products are TiCl4 and VOCl3, both of which have boiling points lower than the low-temperature chlorination temperature and purity ≥98.5%.

[0033] During the low-temperature chlorination process in S4, the chlorination volatilization rate of Ti is ≥95%, and the chlorination volatilization rate of V is ≥98%. All Sc2O3 in the chlorinated tailings is chlorinated, and the chlorination rates of CaO and MgO impurity oxides are both <2%.

[0034] The present invention is further described in detail below with reference to the accompanying drawings and specific examples.

[0035] Taking Panzhihua vanadium-titanium magnetite as raw material, its main chemical composition is shown in Table 1.

[0036] Table 1 Main chemical components of Panzhihua vanadium-titanium magnetite

[0037] TFe <![CDATA[TiO2]]> <![CDATA[V2O5]]> NiO CoO S P 39.80 13.26 0.39 0.024 0.021 0.61 0.013

[0038] Example 1: A method for separating and recovering iron and vanadium-titanium resources from vanadium-titanium magnetite by gradient reduction, the specific steps are as follows:

[0039] S1: After grinding and screening the Panzhihua vanadium-titanium magnetite, a vanadium-titanium magnetite powder raw material with a particle size of 0.1-0.15 mm was obtained. 10.0 g of the sample was weighed and placed in a high-temperature tubular furnace for heating. During the heating process, N2 was introduced to remove the air in the furnace tube. After the temperature reached the reduction temperature, CH4-H2 gas was introduced for selective reduction of iron oxides. After the reduction was completed, the mixture was cooled in a nitrogen atmosphere. The reduction temperature was 500°C, the reduction time was 3 hours, and the volume fraction ratio of CH4 to H2 was 10:90.

[0040] S2: After the high-temperature tubular reactor is cooled to room temperature, the reduced vanadium-titanium magnetite powder is taken out, and then crushed and ball-milled to less than 0.074 mm, and Fe / Fe3C powder and vanadium-rich titanium material are obtained through magnetic separation. The reduction rate of iron oxide in the vanadium-titanium magnetite is 98.3%, and the separation rate of Fe3C powder in the magnetic separation process is 95.1%.

[0041] S3: The vanadium-rich titanium material is placed in a high-temperature tubular furnace for reduction-carbonitriding. During the heating process, N2 is introduced to remove the air in the furnace tube. After the temperature is raised to the reduction temperature, a CH4-H2-N2 mixed gas is introduced to carry out reduction-carbonitriding of the vanadium-rich titanium material. The reduction temperature is 1000°C, the reduction time is 4 hours, and the volume fraction ratio of CH4, H2 and N2 is 10:74:16. After carbonitriding, the O / (C+N) of Ti(C,N,O) in the vanadium-rich titanium material is ≈2.15, and the O / (C+N) of V(C,N,O) is ≈2.12.

[0042] S4: After the high-temperature tubular reactor is cooled to room temperature, take out the vanadium-rich titanium material (chlorination raw material) after carbonitridation, grind and crush it, and place it in the chlorination reactor for low-temperature chlorination. During the heating process, N2 is introduced as a protective gas. After reaching the low-temperature chlorination temperature, chlorine is introduced for chlorination. The chlorination temperature is 450°C and the chlorination time is 1 hour. After the chlorination is completed, nitrogen is introduced for cooling.

[0043] After testing the chlorination tailings and chlorination products, it was found that the chlorination volatilization rate of vanadium in the chlorination raw materials was about 99.1%, the chlorination volatilization rate of titanium was about 97.1%, and the chlorination products were TiCl4 and VOCl3, with a purity of about 99.2%. The chlorination rates of impurity oxides such as CaO and MgO in the chlorination raw materials were less than 1%, while all Sc2O3 was chlorinated.

[0044] Examples 2-8 adopt the same preparation method as Example 1, the only difference is the amount ratio of ingredients and the selection of process parameters, see Table 1 for details:

[0045] Table 1

[0046]

[0047] The results of testing the chlorinated tailings and chlorinated products obtained in Examples 1 to 8 are shown in Table 2:

[0048] Table 2

[0049]

[0050] It can be found from Table 2 that: based on different process parameter settings, although the experimental results of the eight groups of embodiments are slightly different, both iron and vanadium-titanium resources have been highly recovered. The results of the eight groups of embodiments show that within the relevant process parameter range, the method of the present invention can selectively reduce the iron oxides in the vanadium-titanium magnetite well in the early stage, and separate them from the vanadium-titanium-rich material in the vanadium-titanium magnetite by magnetic separation. At the same time, the carbonitridation degree of the vanadium-rich titanium material can be accurately controlled by regulating the reducing gas composition, reduction temperature and time, thereby improving the subsequent low-temperature selective chlorination efficiency and product purity, and finally realizing the gradient reduction and separation recovery of iron and vanadium-titanium resources in the vanadium-titanium magnetite.

[0051] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the technical requirements of the present invention.

Claims

1. A method for separating and recovering iron and vanadium-titanium resources from vanadium-titanium magnetite by gradient reduction, characterized in that: The steps include: S1: Grind the vanadium-titanium magnetite concentrate to obtain a powder raw material with a particle size of 0.1-0.15 mm, and then perform low-temperature selective reduction on the powder raw material under a reducing atmosphere, the reduction temperature is 570-700°C, the reduction time is 2-3h, the reducing atmosphere is CH4-H2-N2, and the volume proportion of each gas in the reducing atmosphere is: CH4 is 4-10%, H2 is 72-96%, and N2 is 0-20%; S2: ball-milling the reduction-carbonitridation product obtained in S1 to a size below 0.074 mm, and magnetically separating the ball-milled material to obtain a magnetic material and a vanadium-rich titanium material; S3: subjecting the vanadium-rich titanium material obtained in S2 to reduction-carbonitriding treatment, the reduction temperature is 1000-1100°C, the reduction time is 3-4h, the reduction atmosphere is a CH4-H2-N2 mixed gas, and the volume proportion of each gas in the CH4-H2-N2 mixed gas is: CH4 is 4-10%, N2 is 12-16%, and H2 is 74-80%; S4: The reduction-carbonitridation product obtained in S3 is crushed to less than 1 mm, and low-temperature chlorination is performed. The chlorination temperature is 280~450℃, and the chlorination time is 1~2h. After chlorination, chlorination products and chlorination tailings are obtained.

2. A method for separating and recovering iron and vanadium-titanium resources from vanadium-titanium magnetite by gradient reduction as claimed in claim 1, characterized in that: The powder raw material obtained after grinding in S1 is first dried at a temperature of 100-200° C. for 4 hours.

3. A method for separating and recovering iron and vanadium-titanium resources from vanadium-titanium magnetite by gradient reduction as claimed in claim 1 or 2, characterized in that: The vanadium-rich titanium material in S2 is a non-magnetic material, and the separation rate of Fe3C in the magnetic separation process is ≥95%.

4. A method for separating and recovering iron and vanadium-titanium resources from vanadium-titanium magnetite by gradient reduction as claimed in claim 3, characterized in that: The reduction-carbonitridation product in S4, i.e., the titanium-containing phase and the vanadium-containing phase in the low-temperature chlorination raw material, are Ti(C, N, O) and V(C, N, O), and O / (C+N) in the phase is ≥2, and the product does not contain deposited carbon.