A method for extracting carbides from carbon-containing tantalum-niobium alloy

The carbides in the carbon-tantalum niobium alloy are separated in the form of anode precipitates by electrolytic method, which solves the problem of inaccurate carbide extraction in the prior art, realizes the precise regulation of alloy composition and mechanical properties, and improves the analysis accuracy .

CN115786927BActive Publication Date: 2024-11-22NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211523504.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-11-22
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

The prior art is difficult to accurately extract carbides in carbon-containing tantalum niobium alloys, resulting in difficulty in regulating alloy composition and mechanical properties.

Method used

The carbides in the carbon-tantalum niobium alloy are separated in the form of anode precipitates by electrolyzing, and the current density and time are controlled by electrolysis of bromine-tartaric acid-methanol solution to ensure that the carbides are precipitated without damage and deposited separately on the anode. In the object.

Benefits of technology

The accurate morphology, size and content of carbides are detected, the C element analysis error is avoided, the precise regulation of alloy composition and mechanical properties is improved, and the accuracy of structural analysis of carbon-containing tantalum niobium alloys is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115786927B_ABST
    Figure CN115786927B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for extracting carbides from a carbon-containing tantalum-niobium alloy, comprising the following steps: 1. Using the carbon-containing tantalum-niobium alloy as an electrolytic anode and tantalum as an electrolytic cathode, and then performing electrolytic treatment in an electrolyte; 2. Filtering the electrolyte after the electrolytic treatment to obtain an anode precipitate; 3. Washing and drying the anode precipitate and weighing it to obtain the carbides in the carbon-containing tantalum-niobium alloy. The present invention uses an electrolytic method to separate all the carbides in the carbon-containing tantalum-niobium alloy in the form of an anode precipitate, thereby extracting carbides from the carbon-containing tantalum-niobium alloy. Since the electrolytic method can ensure that all carbides in the carbon-containing tantalum-niobium alloy are precipitated without damage and deposited separately in the anode precipitate, the accurate morphology, size, and content of the carbides are obtained, further avoiding the analysis error of the C element, which is conducive to the precise regulation of the alloy composition, organizational structure, and mechanical properties of the carbon-containing tantalum-niobium alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of extracting carbides from metal materials, and in particular relates to a method for extracting carbides from a carbon-containing tantalum-niobium alloy. Background Art

[0002] Among the refractory metals (tungsten, molybdenum, tantalum, niobium), niobium has the smallest density and the best compatibility with other elements. Its solid solubility in most alloying elements is greater than that of the other three metals. This provides a lot of room for the regulation of the composition and performance of niobium alloys. Currently, there are six major types of niobium alloys with more than 100 grades, namely medium, high and low strength niobium alloys, functional precision niobium alloys, high strength oxidation-resistant niobium alloys and plastic oxidation-resistant niobium alloys. Most niobium alloys have the advantages of high strength, good cold plasticity, good coating compatibility and good weldability, and have been widely used in aerospace engines and thermal structural parts; among them, high and medium strength niobium alloys are mainly strengthened by adding more W, Mo, Ta, V, Ti, Hf and other elements for solid solution strengthening, and at the same time, a small amount of active elements such as Ti, Zr, Hf and more C elements are added to form a carbide second phase for strengthening. The C element can produce a composite strengthening effect of solid solution strengthening + second phase strengthening with the active elements. The distribution rule of strengthening effect is: the higher the content of solid solution strengthening elements, the higher the alloy strength; the higher the carbide content, the smaller the size, and the more uniform the distribution, the higher the alloy strength. Limited by solid solubility, each element has an extreme content. If the carbon content is too high, the carbide particles will be too large and unevenly distributed. Such unevenly distributed and coarse carbides make the alloy embrittled, which in turn leads to a decrease in processing and application performance. Therefore, it is extremely important to obtain reasonable element composition and suitable structural organization through accurate detection to obtain matching alloy properties for the preparation of niobium alloy materials as soon as possible.

[0003] The preparation technology of carbide composite strengthened tantalum-niobium alloy is to first alloy carbon powder and niobium powder to make niobium carbide powder with a particle size of ≤15μm, then mix it evenly with the appropriate amount of alloy element powder to be added, and then press it into shape, sinter it, and melt, process and heat treat it after the composition inspection is qualified. When adding niobium carbide powder with a size greater than 15μm, the carbides in the prepared niobium alloy are usually needle-shaped, mostly distributed on the grain boundaries, and large in size; when the C content is high, the carbides are larger in size, coarse dendrites in the crystal, and generally distributed in a grid-like manner on the grain boundaries. In order to prepare refined and stabilized carbide particles, and accurately analyze the quality, composition, and morphology of carbides in niobium alloys, in order to accurately control the alloy composition and mechanical properties.

[0004] Therefore, it is necessary to provide a method for extracting carbides from carbon-containing tantalum-niobium alloys by electrolysis to solve the problem that carbides cannot be accurately quantified during the preparation of carbon-containing tantalum-niobium alloys. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for extracting carbides from a carbon-containing tantalum-niobium alloy in view of the deficiencies of the above-mentioned prior art. The method uses an electrolytic method to separate all carbides from the carbon-containing tantalum-niobium alloy in the form of an anode precipitate, thereby extracting carbides from the carbon-containing tantalum-niobium alloy. Since the electrolytic method can ensure that all carbides in the carbon-containing tantalum-niobium alloy are precipitated without damage and deposited separately in the anode precipitate, the accurate morphology, size, and content of the carbides are obtained, and the analysis error of the C element is further avoided, which is conducive to the precise control of the alloy composition, organizational structure, and mechanical properties of the carbon-containing tantalum-niobium alloy.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for extracting carbides from a carbon-containing tantalum-niobium alloy, characterized in that the method comprises the following steps:

[0007] Step 1: Using the carbon-containing tantalum-niobium alloy as an electrolytic anode and tantalum as an electrolytic cathode, and then performing electrolytic treatment in an electrolyte;

[0008] Step 2: filtering the electrolyte after the electrolytic treatment in step 1 to obtain an anode precipitate;

[0009] Step 3: Wash and dry the anode precipitate obtained in step 2 and weigh it to obtain carbides in the carbon-containing tantalum-niobium alloy.

[0010] The anode of the present invention is the carbon-containing tantalum-niobium alloy to be tested. Tantalum is selected as the cathode because of its good conductivity, good mechanical properties, stable chemical properties, and no dissolution. Electrolysis is performed to dissolve the carbon-containing tantalum-niobium alloy. This process includes the following steps: 1. Destruction of the lattice of the carbon-containing tantalum-niobium alloy to generate adsorbed metal atoms; 2. Electron transfer Me→Me n+ +ne; 3. Hydration or complexation of metal ions; the carbon-containing tantalum-niobium alloy is slowly dissolved into the electrolyte, and the second phase of carbides therein are all deposited in the anode precipitate, and then the anode precipitate is filtered, washed and dried to obtain carbide components with intact quality and morphology. Since the electrolysis method can ensure that all carbides in the carbon-containing tantalum-niobium alloy are precipitated and deposited in the anode precipitate, the accurate content of carbides is obtained, which further avoids the analysis error of the C element and is conducive to the precise regulation of the composition and mechanical properties of the carbon-containing tantalum-niobium alloy;

[0011] The present invention determines the composition and content of carbides in the carbon-containing tantalum-niobium alloy by weighing and quantifying the anodic precipitate, and then adopts X-ray diffraction analysis, scanning electron microscopy combined with energy spectrum analysis and transmission electron microscopy detection, so as to achieve optimal regulation of the organizational structure, composition, performance, etc. of the carbon-containing tantalum-niobium alloy.

[0012] The above-mentioned method for extracting carbides from a carbon-containing tantalum-niobium alloy is characterized in that the carbon-containing tantalum-niobium alloy in step 1 is made of the following components by mass fraction: W: 5% to 30%, Ta: 10% to 35%, Zr: 0.1% to 1%, C: 0.05% to 1.0%, and the remainder is Nb and unavoidable impurities; the particle size of the niobium carbide powder in the carbon-containing tantalum-niobium alloy is not greater than 15μm. The present invention is suitable for extracting carbides from carbon-containing tantalum-niobium alloys with a high tantalum content, and is suitable for extracting carbides from carbon-containing tantalum-niobium alloys with a particle size of the added niobium carbide powder not greater than 15μm.

[0013] The above-mentioned method for extracting carbides from a carbon-containing tantalum-niobium alloy is characterized in that the electrolyte used in the electrolytic treatment in step 1 is a bromine-tartaric acid-methanol solution, wherein the volume concentration of tartaric acid is 1% to 5%, and the mass concentration of bromine is 0.8% to 1.2%. In the present invention, the electrolyte is a methanol weak electrolyte containing a small amount of acid and a small amount of oxidant. The use of a weak electrolyte can control the electrolysis rate within a relatively low range, thereby facilitating the full dissolution of the carbon-containing tantalum-niobium alloy matrix into the electrolyte, further ensuring that all carbides in the carbon-containing tantalum-niobium alloy are deposited in the anode precipitate, and the weak electrolyte does not damage the carbide precipitation phase of the niobium alloy, which is conducive to the damage-free separation of the carbides. A small amount of acid is added to the electrolyte to improve the conductivity of the electrolyte, and a small amount of oxidizing bromine is added to speed up the electrolysis process, save electrolysis time, and improve electrolysis efficiency. By controlling the volume concentration of tartaric acid and the mass concentration of bromine, it is conducive to the damage-free precipitation of the second phase of carbides in the electrolysis process and the dissolution of the niobium alloy.

[0014] The above-mentioned method for extracting carbides from a carbon-containing tantalum-niobium alloy is characterized in that the current density of the electrolytic treatment in step 1 is 0.5A / cm 2 ~0.8A / cm 2 The time is 60h-70h, and the inter-electrode distance is 2cm-2.5cm. The present invention is suitable for electrolyzing carbon-containing tantalum-niobium alloy by controlling the parameters of electrolysis treatment, and adopts higher electrolysis treatment current density and shorter electrolysis time to realize the extraction of carbides in carbon-containing tantalum-niobium alloy.

[0015] Compared with the prior art, the present invention has the following advantages:

[0016] 1. The present invention adopts an electrolytic method to separate all carbides in the carbon-containing tantalum-niobium alloy in the form of anodic precipitates, thereby extracting carbides from the carbon-containing tantalum-niobium alloy. Since the electrolytic method can ensure that all carbides in the carbon-containing tantalum-niobium alloy are precipitated without damage and deposited separately in the anodic precipitates, the accurate morphology, size and content of the carbides are obtained, and the analysis error of the C element is further avoided, which is conducive to the precise control of the alloy composition, organizational structure and mechanical properties of the carbon-containing tantalum-niobium alloy.

[0017] 2. The present invention uses electrolysis to separate carbides in carbon-containing tantalum-niobium alloys, and can directly weigh and detect carbides, avoiding the error influence of instrument testing methods in the prior art that use gas as the detection target, and solving the problem of inaccurate carbide analysis in carbon-containing tantalum-niobium alloys.

[0018] 3. After extracting carbides from the carbon-containing tantalum-niobium alloy, the present invention combines X-ray diffraction analysis, scanning electron microscopy combined with energy spectrum analysis and transmission electron microscopy detection to perform morphology, size detection, and carbide composition and content analysis on the carbides, thereby intuitively and comprehensively improving the accuracy of carbide analysis.

[0019] 4. The present invention uses bromine-tartaric acid-methanol solution as the electrolyte to separate carbides in the niobium alloy without damage, thereby reducing the agglomeration of carbides, better maintaining the morphology of carbides, and further improving the accuracy of carbide analysis.

[0020] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 3 is a scanning electron microscope image of the carbon-containing tantalum-niobium alloy of Example 1 of the present invention.

[0022] Figure 2 This is the X-ray diffraction pattern of carbides in the carbon-containing tantalum-niobium alloy obtained in Example 1 of the present invention.

[0023] Figure 3 This is a transmission electron microscope image of carbides in the carbon-containing tantalum-niobium alloy obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0024] Example 1

[0025] This embodiment includes the following steps:

[0026] Step 1: Use the carbon-containing tantalum-niobium alloy as an electrolytic anode and tantalum as an electrolytic cathode, and then perform electrolytic treatment in an electrolyte; the carbon-containing tantalum-niobium alloy is made of the following components by mass fraction: W: 5%, Ta: 30%, Zr: 0.4%, C: 0.11%, and the remainder is Nb and unavoidable impurities; the particle size of the niobium carbide powder in the carbon-containing tantalum-niobium alloy is not more than 15μm; the electrolyte used in the electrolytic treatment is a bromine-tartaric acid-methanol solution, wherein the volume concentration of tartaric acid is 5%, and the mass concentration of bromine is 1%; the current density of the electrolytic treatment is 0.8A / cm 2 , time is 60h, inter-electrode distance is 2.2cm;

[0027] Step 2: filtering the electrolyte after the electrolytic treatment in step 1 to obtain an anode precipitate;

[0028] Step 3: Wash the anode precipitate obtained in step 2 with deionized water and anhydrous ethanol in turn, then dry and weigh it to obtain carbides in the carbon-containing tantalum-niobium alloy.

[0029] After testing, the mass of carbide in the carbon-containing tantalum-niobium alloy of this embodiment is 0.50g, the weight loss of niobium alloy is 29.7g, and the carbide content in the carbon-containing tantalum-niobium alloy is calculated to be 1.68wt%. Based on Nb2C converted to C, the carbon content of the carbon-containing tantalum-niobium alloy of this embodiment is 0.1%.

[0030] Figure 1 is a scanning electron microscope image of the carbon-containing tantalum-niobium alloy of this embodiment. Figure 1 It can be seen that the morphology of carbides is mainly needle-shaped.

[0031] Figure 2 is the X-ray diffraction pattern of carbides in the carbon-containing tantalum-niobium alloy obtained in this example. Figure 2 It can be seen that the 2θ of the three strongest peaks of carbide are 37.977°, 35.982° and 49.754°, which are all characteristic peaks of Nb2C, indicating that the main component of carbide is niobium carbide.

[0032] Figure 3 is a transmission electron microscope image of carbides in the carbon-containing tantalum-niobium alloy obtained in this example. Figure 3 It can be seen that the morphology of carbides is mainly needle-shaped.

[0033] Example 2

[0034] This embodiment includes the following steps:

[0035] Step 1: Use the carbon-containing tantalum-niobium alloy as an electrolytic anode and tantalum as an electrolytic cathode, and then perform electrolytic treatment in an electrolyte; the carbon-containing tantalum-niobium alloy is made of the following components by mass fraction: W: 30%, Ta: 10%, Zr: 1%, C: 0.6%, and the balance is Nb and unavoidable impurities; the particle size of the niobium carbide powder in the carbon-containing tantalum-niobium alloy is not more than 15μm; the electrolyte used in the electrolytic treatment is a bromine-tartaric acid-methanol solution, wherein the volume concentration of tartaric acid is 1%, and the mass concentration of bromine is 0.8%; the current density of the electrolytic treatment is 0.5A / cm 2 , time is 70h, inter-electrode distance is 2cm;

[0036] Step 2: filtering the electrolyte after the electrolytic treatment in step 1 to obtain an anode precipitate;

[0037] Step 3: Wash the anode precipitate obtained in step 2 with deionized water and anhydrous ethanol in turn, then dry and weigh it to obtain carbides in the carbon-containing tantalum-niobium alloy.

[0038] After testing, the mass of carbide in the carbon-containing tantalum-niobium alloy of this embodiment is 2.23g, the weight loss of niobium alloy is 23.46g, and the carbide content in the carbon-containing tantalum-niobium alloy is calculated to be 9.51wt%. Based on Nb2C converted to C, the carbon content of the carbon-containing tantalum-niobium alloy of this embodiment is 0.57%.

[0039] Example 3

[0040] This embodiment includes the following steps:

[0041] Step 1: Use the carbon-containing tantalum-niobium alloy as an electrolytic anode and tantalum as an electrolytic cathode, and then perform electrolytic treatment in an electrolyte; the carbon-containing tantalum-niobium alloy is made of the following components by mass fraction: W: 10%, Ta: 35%, Zr: 0.1%, C: 0.3%, and the remainder is Nb and unavoidable impurities; the particle size of the niobium carbide powder in the carbon-containing tantalum-niobium alloy is not more than 15μm; the electrolyte used in the electrolytic treatment is a bromine-tartaric acid-methanol solution, wherein the volume concentration of tartaric acid is 3%, and the mass concentration of bromine is 1.2%; the current density of the electrolytic treatment is 0.7A / cm 2 , time is 65h, inter-electrode distance is 2.5cm;

[0042] Step 2: filtering the electrolyte after the electrolytic treatment in step 1 to obtain an anode precipitate;

[0043] Step 3: Wash the anode precipitate obtained in step 2 with deionized water and anhydrous ethanol in turn, then dry and weigh it to obtain carbides in the carbon-containing tantalum-niobium alloy.

[0044] After testing, the mass of carbide in the carbon-containing tantalum-niobium alloy of this embodiment is 1.51g, the weight loss of niobium alloy is 28.1g, and the content of carbide in the carbon-containing tantalum-niobium alloy is calculated to be 5.37wt%. Based on the conversion of Nb2C to C, the carbon content of the carbon-containing tantalum-niobium alloy of this embodiment is 0.32%.

[0045] The carbide analysis results obtained in Examples 1 to 3 of the present invention were compared with the chemical analysis results to obtain Table 1.

[0046] Table 1

[0047]

[0048] *Carbon analysis results are based on the American standard ISPM1941-10 chemical analysis method for refractory metals and activated carbon elements, with steel standard as the standard sample.

[0049] From the comparison of the test results, it can be seen that the chemical analysis method has a large analysis error for the carbon element, and the results of different batches fluctuate greatly, with a difference of 5% to 50%. However, the electrolytic method of the present invention is used to extract carbides in the carbon-containing tantalum-niobium alloy and accurately determine the carbon content in the carbon-containing tantalum-niobium alloy. The result is close to the nominal carbon content.

[0050] The present invention regulates the carbides of the carbon-containing tantalum-niobium alloy according to the method for extracting carbides from the carbon-containing tantalum-niobium alloy, thereby obtaining a carbon-containing tantalum-niobium alloy with good high-temperature performance. The performance comparison is shown in Table 2.

[0051] Table 2

[0052]

[0053] The high temperature test temperature of the homemade carbon-containing tantalum-niobium alloy in Table 2 is only 13°C different from that of the similar high-strength niobium alloy in the United States, but the yield strength and tensile strength are increased by 78MPa, 83MPa and 59MPa, 67MPa, respectively, and the elongation is increased by 5%. By applying the method for extracting carbides from the carbon-containing tantalum-niobium alloy described in the present invention and regulating the carbon in the niobium alloy, a carbon-containing tantalum-niobium alloy with excellent high-temperature mechanical properties has been preliminarily obtained.

[0054] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for extracting carbides from a carbon-containing tantalum-niobium alloy, characterized in that: The method comprises the following steps: Step 1: Use the carbon-containing tantalum-niobium alloy as an electrolytic anode and tantalum as an electrolytic cathode, and then perform electrolytic treatment in an electrolyte; the carbon-containing tantalum-niobium alloy is made of the following components by mass fraction: W: 5% to 30%, Ta: 10% to 35%, Zr: 0.1% to 1%, C: 0.05% to 1.0%, and the remainder is Nb and unavoidable impurities; the particle size of the niobium carbide powder in the carbon-containing tantalum-niobium alloy is not more than 15 μm; the electrolyte used in the electrolytic treatment is a bromine-tartaric acid-methanol solution, wherein the volume concentration of tartaric acid is 1% to 5%, and the mass concentration of bromine is 0.8% to 1.2%; the current density of the electrolytic treatment is 0.5A / cm 2 ~0.8A / cm 2 , time is 60h~70h, inter-electrode distance is 2cm~2.5cm; Step 2: filtering the electrolyte after the electrolytic treatment in step 1 to obtain an anode precipitate; Step 3: Wash and dry the anode precipitate obtained in step 2 and weigh it to obtain carbides in the carbon-containing tantalum-niobium alloy.

Citation Information

Patent Citations

  • Method for performing electrolytic extraction on ultrafine carbide in steel

    CN107576556A

  • Method for extracting carbide from high-chromium cast iron

    CN108871924A

  • Extraction method for carbide in medium- and high-strength niobium alloy

    CN110133021A

  • Method for preparing niobium titanium carbide from niobium-containing minerals

    CN114853016A

  • An improved process for producing tantalum carbide and niobium carbide, more particularly for the production of hard metal

    GB509609A