Carbon fiber, magnesium alloy microstructure reinforced composite plate and preparation method thereof
By combining low-temperature resistant magnesium alloy material and microstructure design in carbon fiber reinforced resin-based composite materials, the microstructure reinforced composite panel of carbon fiber and magnesium alloy is formed, which solves the problem of insufficient low-temperature performance and achieves stable performance in ice and snow sports equipment and Impact resistance, suitable for ice and snow sports equipment and other fields.
Patent Information
- Application Number
- CN202211601102.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-13
AI Technical Summary
The poor performance of existing carbon fiber reinforced resin-based composite materials in low temperature environments limits their use in ice and snow sports equipment applications.
The low-temperature resistant magnesium alloy material is combined with carbon fiber, and the microstructure of carbon fiber and magnesium alloy is formed through microstructure design to enhance the toughness of the material, and the impact resistance of magnesium alloy is combined with the microstructure magnesium alloy core and carbon fiber board The layer forms a composite material with good low temperature resistance and structural strength.
It realizes the stable performance of composite materials in low temperature environments, improves impact resistance and service life, and maintains the lightweight properties of the materials, and is suitable for ice and snow sports equipment and other fields.
Smart Images

Figure CN115871288B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a carbon fiber and magnesium alloy microstructure reinforced composite plate and a preparation method thereof, belonging to the technical field of preparation and application of nonferrous metal composite materials. Background Art
[0002] There is a big gap between my country and foreign countries in the field of ice and snow equipment manufacturing. Most of the ice and snow sports equipment currently used are imported products, especially high-end ice and snow sports equipment. Therefore, in order to meet the needs of the rapid development of ice and snow sports in my country, it is urgent to develop my country's independent ice and snow equipment manufacturing industry.
[0003] The main structure of a ski board is a sandwich composite structure. Currently, most of the structures used are wooden cores covered with fiber layers. The wooden cores are expensive and heavy, and a new composite material structure design is urgently needed to make them lightweight. The invention patent of China Publication Patent No. CN 105711209 A proposes a method for preparing a ski board reinforced with a foamed polypropylene and graphite fiber composite material. The inner core of the ski board prepared with fiber-reinforced polypropylene material is light in weight and high in strength. The bottom plate adopts high-strength ABS resin and has good wear resistance. The invention patent of China Publication Patent No. CN 106075873 A proposes a method for preparing a modified fiber-reinforced ski board, which adopts PS resin and graphite fiber composite material as the surface layer, modified polyethylene resin and carbon fiber composite material as the inner core layer, and polyethylene material as the bottom plate. The modified chlorinated polypropylene binder is used for bonding, and the strength is improved, the surface friction is reduced, the sliding speed is increased, and the service life of the ski board is also extended.
[0004] Magnesium and its alloys are the fastest-applied and fastest-growing nonferrous metal materials in the world. Magnesium alloys have high specific strength, high specific stiffness, high elastic modulus, excellent anti-vibration and noise reduction, impact resistance and good castability. However, they also have defects such as low strength, poor plasticity, poor corrosion resistance and flammability, which greatly affect the widespread application of magnesium and magnesium alloys. In addition, the low-temperature resistance of magnesium alloys is not very good, and their application in ice and snow scenes will also be limited.
[0005] Carbon fiber is a special fiber composed of carbon elements. It has the characteristics of light weight, good fineness, high tensile strength, etc. It also has the advantages of high temperature resistance, friction resistance, electrical conductivity, thermal conductivity, and small expansion coefficient. Parts processed with carbon fiber have strong designability and can be formed in one piece. Therefore, carbon fiber can be used as a reinforcing base in composite materials to improve material performance and make up for the shortcomings of base material performance. At present, the low-temperature performance of carbon fiber reinforced resin-based composite materials is not very good. In low-temperature environments, especially in ice and snow sports equipment applications, their application is limited. Summary of the invention
[0006] As a new type of structural material, microstructured materials take into account the requirements of lightweight components and high performance. By structurally treating the inside of the material, various advantages of the material can be brought into play, and ultimately the best product performance can be achieved. In response to the problem that the low-temperature performance of existing carbon fiber reinforced resin-based composite materials is poor, the present invention provides a carbon fiber, magnesium alloy microstructure reinforced composite plate and a preparation method thereof. A low-temperature resistant magnesium alloy material is used, and carbon fibers and other fibers are combined to form a low-temperature resistant resin-based composite material. Combined with the microstructure form design, a new type of composite plate is developed, which gives full play to the impact resistance of magnesium alloys, and uses carbon fibers to make up for the shortcomings of insufficient toughness of magnesium alloy materials. The combination of the two makes the composite material have better low-temperature resistance, and has better structural strength and impact resistance, and can be used in the fields of ice and snow sports equipment.
[0007] The present invention provides a carbon fiber and magnesium alloy microstructure reinforced composite plate, the structure of which is composed of an upper carbon fiber plate 1, a lower carbon fiber plate 5, an interlayer fiber layer and a microstructure magnesium alloy plate core 3;
[0008] The upper carbon fiber plate 1 and the lower carbon fiber plate 5 are formed by composite hot pressing and curing of carbon fiber cloth and thermosetting resin, and the mass ratio of thermosetting resin to fiber is preferably 1:1; the thickness of the upper carbon fiber plate 1 after curing is 5 to 8 mm, and the thickness of the lower carbon fiber plate 5 after curing is 7 to 12 mm;
[0009] Preferably, the carbon fiber cloth is T series carbon fiber cloth, and the thermosetting resin material is polydicyclopentadiene (PDCPD) or DP460 epoxy resin;
[0010] Preferably, the thickness of the lower carbon fiber plate 5 is thicker than that of the upper carbon fiber plate 1, in order to ensure the wear resistance and service life of the material.
[0011] The microstructured magnesium alloy plate core 3 is composed of two parts: a foamed plastic 31 and a microstructured magnesium alloy material 32 ; the foamed plastic 31 is filled in the gaps of the microstructured magnesium alloy material 32 ; the mass ratio of the foamed plastic 31 to the microstructured magnesium alloy material 32 is preferably 1:6.
[0012] The microstructure forms of the microstructure magnesium alloy material 32 include: three-dimensional double-arrow negative Poisson's ratio multi-cell microstructure, gradient honeycomb structure and corrugated paper structure; the foamed plastic 31 is a low-density foamed plastic, preferably a chemically cross-linked polyethylene (XPE) foamed plastic.
[0013] Among them, the microstructure of the microstructure magnesium alloy material 32 is a three-dimensional double-arrow negative Poisson's ratio multi-cell microstructure, and the size of the microstructure unit can be 15mm×15mm×12mm~17mm×17mm×15mm;
[0014] The microstructure of the microstructured magnesium alloy material 32 is a gradient honeycomb structure. The microstructure units are arranged in three layers. The middle layer is a small-sized honeycomb structure. The same large-sized honeycomb structures are arranged on the upper and lower sides of the middle layer. The ratio of the side length of the small-sized honeycomb structure unit in the middle layer to the side length of the large-sized honeycomb structures on the upper and lower sides is 1:(2~3).
[0015] The upper interlayer fiber layer 2 is arranged between the upper carbon fiber plate 1 and the microstructure magnesium alloy plate core 3, and the lower interlayer fiber layer 4 is arranged between the lower carbon fiber plate 5 and the microstructure magnesium alloy plate core 3. The upper interlayer fiber layer 2 and the lower interlayer fiber layer 4 have a thickness of 1.0mm-1.5mm, and are both composed of a resin base and a large mesh size fiber material with a mesh diameter of 0.5-1.0mm. The fiber materials include: carbon fiber, glass fiber and Kevlar fiber; the resin base is a thermosetting resin, preferably polydicyclopentadiene (PDCPD) or DP460 epoxy resin; the mass ratio of the fiber material to the resin base is between 1:(1~1.5).
[0016] A method for preparing a carbon fiber and magnesium alloy microstructure reinforced composite plate,
[0017] 1) Using carbon fiber cloth and thermosetting resin material to composite and heat-press and cure, to obtain an upper carbon fiber plate 1 with a thickness of 5 to 8 mm;
[0018] 2) Using carbon fiber cloth and thermosetting resin material to composite and heat-press and cure, to obtain a lower carbon fiber plate 5 with a thickness of 7 to 12 mm;
[0019] 3) Fill the foamed plastic 31 into the gaps of the microstructured magnesium alloy material 32, and after the foaming is completed, obtain a blank of the microstructured magnesium alloy plate core 3; perform mechanical processing on the obtained blank to remove excess material to obtain the required size of the microstructured magnesium alloy plate core 3, and perform frosting on the upper and lower surfaces of the microstructured magnesium alloy plate core 3 to improve the roughness.
[0020] 4) A large mesh size fiber material with a mesh diameter of 0.5-1.0 mm is compounded with a thermosetting resin in a prepreg manner and then wound and laid on the outside of the microstructured magnesium alloy plate core 3, and an upper interlayer fiber layer 2 and a lower interlayer fiber layer 4 with a thickness of 1.0 mm-1.5 mm are respectively obtained on the upper and lower surfaces of the microstructured magnesium alloy plate core 3;
[0021] 5) The upper carbon fiber board 1 and the lower carbon fiber board 5 are placed above and below the upper interlayer fiber layer 2 and the lower interlayer fiber layer 4 respectively, and are bonded together by hot pressing and curing to obtain the carbon fiber and magnesium alloy microstructure reinforced composite board.
[0022] In step 3), the microstructured magnesium alloy material 32 is obtained by selective laser sintering technology.
[0023] In step 4), the laying angles used during winding and laying are 0°, 45° and 90°, and the laying is alternately carried out in three directions.
[0024] The carbon fiber cloth in step (1) and step (2) is divided into a first part, a second part, a third part, a fourth part and a fifth part from top to bottom according to different prepreg laying methods; wherein the first part and the fifth part are made of at least six layers of unidirectional carbon fiber cloth prepreg laid alternately from top to bottom in the order of 0° / 45° / 90° / 0° / 45° / 90°, the second part and the fourth part are made of several layers of unidirectional carbon fiber cloth prepreg laid alternately from top to bottom in the order of 90° / 0°, and the third part is made of several layers of unidirectional carbon fiber cloth prepreg laid alternately from top to bottom in the order of 90° / 0°.
[0025] The beneficial effects of the present invention are:
[0026] The microstructured magnesium alloy material 32 in the present invention is presented in various microstructure forms such as three-dimensional double-arrow negative Poisson's ratio multi-cellular microstructure, gradient honeycomb structure, corrugated paper structure, etc.; magnesium alloy has high specific strength, high specific stiffness, high elastic modulus and excellent seismic and noise reduction, impact resistance and good castability. Compared with directly using magnesium alloy sheets, forming the core in the form of a microstructure is beneficial to improving the overall moment of inertia of the magnesium alloy material, can withstand shear loads, and improves the overall bending resistance and impact resistance.
[0027] The foamed plastic 31 filled in the microstructured magnesium alloy material 32 can effectively improve the material's shock absorption, noise reduction and impact resistance, while also supporting and cushioning the magnesium alloy microstructure to prevent damage caused by ultra-high-intensity impact.
[0028] The high-strength carbon fiber used in the present invention enables the material as a whole to obtain higher mechanical properties, while making up for the shortcoming of insufficient toughness of the magnesium alloy.
[0029] The present invention adopts a novel PDCPD resin system, which has a bending modulus of 1790-2070MPa, a tensile strength of 34MPa, and an Izod beam notched impact strength of 427J / m, and has excellent mechanical properties; it does not change at -40°C, and can ensure its stable working performance at low temperatures; in addition, it also has excellent weather resistance, wear resistance, surface coating, electrical insulation, acid and alkali resistance, and waterproofness to ensure the service life of the entire material.
[0030] Laying the interlayer fiber layers in the structure in the form of prepreg improves the uniformity of the resin compared to other methods such as manual application, and can obtain a higher quality composite material interlayer structure, improve the interlayer bonding strength and material service life.
[0031] The materials and structural designs used in the present invention are all lightweight materials, which can achieve higher performance while ensuring light weight, and are conducive to use in ice and snow equipment or other fields with lightweight requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0033] Figure 1 The present invention is a schematic diagram of the composite plate split structure of a carbon fiber and magnesium alloy microstructure reinforced composite plate and a preparation method thereof.
[0034] Figure 2 Schematic diagram of the structure of microstructured magnesium alloy material with gradient honeycomb structure.
[0035] In the figure: 1-upper carbon fiber board, 2-upper interlayer fiber layer, 3-microstructure magnesium alloy plate core, 31-foamed plastic, 32-microstructure magnesium alloy material, 4-lower interlayer fiber layer, 5-lower carbon fiber board. DETAILED DESCRIPTION
[0036] The present invention is further explained and illustrated in the following by way of specific embodiments, but the present invention is not limited to the following embodiments, and a variety of different implementation methods can be formed by combining different forms of microstructures used and different types of other materials.
[0037] Embodiment 1:
[0038] The carbon fiber and magnesium alloy microstructure reinforced composite plate prepared in this embodiment is as follows Figure 1 As shown, the preparation steps are as follows:
[0039] 1) Using T series carbon fiber cloth and polydicyclopentadiene (PDCPD) thermosetting resin material for composite hot pressing and curing to obtain an upper carbon fiber plate 1 with a thickness of 5 to 8 mm;
[0040] 2) using T series carbon fiber cloth and polydicyclopentadiene (PDCPD) thermosetting resin material for composite hot pressing and curing to obtain a lower carbon fiber plate 5 with a thickness of 7 to 12 mm;
[0041] 3) Fill the foamed plastic 31 into the gaps of the microstructured magnesium alloy material 32, and after the foaming is completed, obtain a blank of the microstructured magnesium alloy plate core 3; perform mechanical processing on the obtained blank to remove excess material to obtain the required size of the microstructured magnesium alloy plate core 3, and perform frosting on the upper and lower surfaces of the microstructured magnesium alloy plate core 3 to improve the roughness.
[0042] Among them, the microstructure of the microstructured magnesium alloy material 32 is a three-dimensional double-arrow negative Poisson's ratio cellular microstructure, which is manufactured according to the shape of the required part through selective laser sintering technology; the microstructure unit size is 15mm×15mm×12mm, the size is selected according to actual conditions, and a single layer is set.
[0043] 4) A large mesh size fiber material with a mesh diameter of 0.5-1.0 mm is compounded with a polydicyclopentadiene (PDCPD) thermosetting resin in a prepreg manner and then wound and laid on the outside of the microstructured magnesium alloy plate core 3, and an upper interlayer fiber layer 2 and a lower interlayer fiber layer 4 with a thickness of 1.0 mm-1.5 mm are respectively obtained on the upper and lower surfaces of the microstructured magnesium alloy plate core 3; the laying angles are alternately 0° / 45° / 90°;
[0044] 5) The upper carbon fiber board 1 and the lower carbon fiber board 5 are combined with the microstructured magnesium alloy plate core 3 wrapped with the upper interlayer fiber layer 2 and the lower interlayer fiber layer 4, and hot-pressed and bonded together to obtain the carbon fiber and magnesium alloy microstructure reinforced composite plate.
[0045] Example 2
[0046] The difference between this embodiment and Embodiment 1 is that the microstructure of the microstructure magnesium alloy material 32 is a gradient honeycomb structure, which is manufactured by selective laser sintering technology according to the desired shape of the part; the microstructure unit is arranged in three layers, the middle layer is a small-sized honeycomb structure, and the same large-sized honeycomb structures are arranged on the upper and lower sides of the middle layer, and the ratio of the side length of the small-sized honeycomb structure unit in the middle layer to the side length of the large-sized honeycomb structures on the upper and lower sides is 1:2 to 1:3.
[0047] Example 3
[0048] The difference between this embodiment and one of the specific embodiments 1 or 2 is that the carbon fiber cloth in step (1) and step (2) is divided into a first part, a second part, a third part, a fourth part and a fifth part from top to bottom according to different prepreg laying methods; wherein the first part and the fifth part are made of at least six layers of unidirectional carbon fiber cloth prepreg laid alternately from top to bottom in the order of 0° / 45° / 90° / 0° / 45° / 90°, the second part and the fourth part are made of several layers of unidirectional carbon fiber cloth prepreg laid alternately from top to bottom in the order of 90° / 0°, and the third part is made of several layers of unidirectional carbon fiber cloth prepreg laid alternately from top to bottom in the order of 90° / 0°.
[0049] Example 4
[0050] The difference between this embodiment and one of Examples 1 to 3 is that the resin in steps (1), (2) and (4) is DP460 epoxy resin glue, and the rest is the same as Specific Examples 1 to 3.
[0051] Example 5
[0052] The difference between this embodiment and any one of Examples 1 to 4 is that the microstructure unit size of the microstructure magnesium alloy material 32 in step (3) is 17 mm×17 mm×15 mm, and the rest is the same as Specific Examples 1 to 4.
[0053] The carbon fiber and magnesium alloy microstructure reinforced composite plate obtained in Example 1 was subjected to a load test. It can be seen that the maximum load of the carbon fiber and magnesium alloy microstructure reinforced composite plate obtained in Example 1 at 25°C is 14063.3N, and the maximum load of the -20°C low temperature test is 13875.4N. From the results, it can be seen that although the performance is reduced at low temperatures, it can still meet the use requirements. Other embodiments have the same or similar technical effects.
[0054] The content of the present invention is not limited to the content of the above embodiments. The combination of one or several specific embodiments can also achieve the purpose of the invention.
Claims
1. A carbon fiber and magnesium alloy microstructure reinforced composite plate, It is characterized in that The structure of the composite plate is composed of an upper carbon fiber plate (1), a lower carbon fiber plate (5), an interlayer fiber layer and a microstructured magnesium alloy plate core (3); The upper carbon fiber plate (1) and the lower carbon fiber plate (5) are formed by hot-pressing and curing a carbon fiber cloth and a thermosetting resin; the mass ratio of the thermosetting resin to the fiber in the upper carbon fiber plate (1) and the lower carbon fiber plate (5) is 1:1; the thickness of the upper carbon fiber plate (1) after curing is 5 to 8 mm, and the thickness of the lower carbon fiber plate (5) after curing is 7 to 12 mm; The microstructured magnesium alloy plate core (3) is composed of two parts: a foamed plastic (31) and a microstructured magnesium alloy material (32); the foamed plastic (31) is filled in the gaps of the microstructured magnesium alloy material (32); the mass ratio of the foamed plastic (31) to the microstructured magnesium alloy material (32) is 1:6; The microstructure forms of the microstructured magnesium alloy material (32) include: a three-dimensional double-arrow negative Poisson's ratio multi-cell microstructure, a gradient honeycomb structure, and a corrugated paper structure; the foamed plastic (31) is a low-density foamed plastic; The upper interlayer fiber layer (2) is arranged between the upper carbon fiber plate (1) and the microstructured magnesium alloy plate core (3), and the lower interlayer fiber layer (4) is arranged between the lower carbon fiber plate (5) and the microstructured magnesium alloy plate core (3). The upper interlayer fiber layer (2) and the lower interlayer fiber layer (4) have a thickness of 1.0 mm to 1.5 mm and are both composed of a resin matrix and a large mesh fiber material with a mesh diameter of 0.5 to 1.0 mm. The mass ratio of the fiber material to the resin matrix is between 1:(1 to 1.5); the fiber material includes: carbon fiber, glass fiber and Kevlar fiber; and the resin matrix is a thermosetting resin.
2. The carbon fiber and magnesium alloy microstructure reinforced composite plate according to claim 1, It is characterized in that The carbon fiber cloth in the upper carbon fiber plate (1) and the lower carbon fiber plate (5) is T series carbon fiber cloth, and the thermosetting resin in the upper carbon fiber plate (1), the lower carbon fiber plate (5), the upper interlayer fiber layer (2) and the lower interlayer fiber layer (4) is polydicyclopentadiene or DP460 epoxy resin.
3. The carbon fiber and magnesium alloy microstructure reinforced composite plate according to claim 1, It is characterized in that The thickness of the lower carbon fiber plate (5) is thicker than that of the upper carbon fiber plate (1).
4. The carbon fiber and magnesium alloy microstructure reinforced composite plate according to claim 1, It is characterized in that The foamed plastic (31) in the microstructured magnesium alloy plate core (3) is chemically cross-linked polyethylene foamed plastic.
5. The carbon fiber and magnesium alloy microstructure reinforced composite plate according to claim 1, It is characterized in that The microstructure of the magnesium alloy material (32) is a three-dimensional double-arrow negative Poisson's ratio multi-cell microstructure, and the size of the microstructure unit is 15mm×15mm×12mm~17mm×17mm×15mm; Alternatively, the microstructure of the microstructured magnesium alloy material (32) is a gradient honeycomb structure, the microstructure units are arranged in three layers, the middle layer is a small-sized honeycomb structure, and the same large-sized honeycomb structures are arranged on the upper and lower sides of the middle layer, and the ratio of the side length of the small-sized honeycomb structure unit in the middle layer to the side length of the large-sized honeycomb structures on the upper and lower sides is 1:(2~3).
6. A method for preparing a carbon fiber and magnesium alloy microstructure reinforced composite plate according to any one of claims 1 to 5, It is characterized in that The specific steps of this method are as follows: 1) Using carbon fiber cloth and thermosetting resin material in a mass ratio of 1:1 to perform composite hot pressing and curing to obtain an upper carbon fiber plate (1) with a thickness of 5 to 8 mm; 2) using a carbon fiber cloth and a thermosetting resin material in a mass ratio of 1:1 to perform composite hot pressing and curing to obtain a lower carbon fiber plate (5) with a thickness of 7 to 12 mm; 3) Filling the foamed plastic (31) into the gaps of the microstructured magnesium alloy material (32), and after the foaming is completed, obtaining a blank of the microstructured magnesium alloy plate core (3); the mass ratio of the foamed plastic (31) to the microstructured magnesium alloy material (32) is 1:6; machining the obtained blank to remove excess material to obtain the required size of the microstructured magnesium alloy plate core (3), and frosting the upper and lower surfaces of the microstructured magnesium alloy plate core (3) to increase the roughness; 4) a large mesh size fiber material with a mesh diameter of 0.5-1.0 mm is composited with a thermosetting resin in a prepreg manner and then wound and laid on the outside of the microstructured magnesium alloy plate core (3), wherein the mass ratio of the fiber material to the resin matrix is between 1:(1-1.5); an upper interlayer fiber layer (2) and a lower interlayer fiber layer (4) with a thickness of 1.0 mm-1.5 mm are respectively obtained on the upper and lower surfaces of the microstructured magnesium alloy plate core (3); 5) placing the upper carbon fiber plate (1) and the lower carbon fiber plate (5) above and below the upper interlayer fiber layer (2) and the lower interlayer fiber layer (4) respectively, and bonding them together by hot pressing and curing to obtain the carbon fiber and magnesium alloy microstructure reinforced composite plate.
7. The method for preparing the carbon fiber and magnesium alloy microstructure reinforced composite plate according to claim 6, It is characterized in that In step 3), the microstructured magnesium alloy material (32) is obtained by selective laser sintering technology.
8. The method for preparing the carbon fiber and magnesium alloy microstructure reinforced composite plate according to claim 6, It is characterized in that In step 4), the laying angles used in winding and laying are 0°, 45° and 90°, and the laying is alternately carried out in three directions.
9. The method for preparing the carbon fiber and magnesium alloy microstructure reinforced composite plate according to claim 6, It is characterized in that The carbon fiber cloth in step 1) and step 2) is divided into a first part, a second part, a third part, a fourth part and a fifth part from top to bottom according to different prepreg laying methods; wherein the first part and the fifth part are made of at least six layers of unidirectional carbon fiber cloth prepregs laid alternately from top to bottom in the order of 0° / 45° / 90° / 0° / 45° / 90°, the second part and the fourth part are made of several layers of unidirectional carbon fiber cloth prepregs laid alternately from top to bottom in the order of 90° / 0°, and the third part is made of several layers of unidirectional carbon fiber cloth prepregs laid alternately from top to bottom in the order of 90° / 0°.