A catalyst for disproportionation and transalkylation of toluene and heavy aromatics and its preparation method and application

By designing a multi-stage pore structure in the catalyst, using the combination of micropores, intergranular mesopores and macropores, the problem that existing catalysts are difficult to adapt to the mixed raw materials of toluene and heavy aromatic hydrocarbons is solved, and efficient catalytic performance and stability are achieved.

CN115920956BActive Publication Date: 2024-11-29NINGBO ZHONGJIN PETROCHEM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211665022.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-23
Publication Date
2024-11-29
Estimated Expiration
2042-12-23

AI Technical Summary

Technical Problem

The existing toluene and heavy aromatic hydrocarbon disproportionation and alkyl transfer catalysts are difficult to adapt to the complexity of mixed raw materials and cannot promote reaction diffusion to a greater extent, resulting in lower catalytic activity and shorter catalyst life.

Method used

Using microporous molecular sieve, macropore binder and at least two pore-generating agents, a catalyst with a multi-stage pore structure with micropores, intergranular mesopores and macropores is designed to control the volume and distribution of pores at each stage. , adapt to the reaction and diffusion needs of molecules of different sizes.

Benefits of technology

It significantly improves the catalytic performance and stability of the catalyst, extends the service life of the catalyst, and achieves high conversion, high yield and high heavy aromatic conversion capabilities.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of petrochemical technology, and in particular to a catalyst for disproportionation and transalkylation of toluene and heavy aromatics, and a preparation method and application thereof. The raw materials of the catalyst include the following components: a microporous molecular sieve, a macroporous binder, and at least two porogens capable of forming pores of different sizes. In the catalyst of the present invention, the microporous molecular sieve, the macroporous binder, and at least two porogens are matched to achieve the pore characteristics of molecular sieve micropores, intercrystalline mesopores, and macropores on the catalyst, which can adapt to the complexity of reactants, intermediates, and reaction products in the disproportionation and transalkylation reactions of toluene and heavy aromatics, and provide a catalytic site for reaction and diffusion for molecules of different sizes, thereby achieving better catalytic performance and catalytic stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of petrochemical engineering, and in particular to a catalyst for disproportionation and transalkylation of toluene and heavy aromatics, and a preparation method and application thereof. Background Art

[0002] Aromatics are important basic raw materials for the petrochemical industry, among which benzene and paraxylene (PX) are the most in-demand basic aromatic chemical raw materials, which are mainly used to synthesize high-molecular polyester fibers and plastics, and are also widely used in the fields of medicine, pesticides, dyes, etc. At present, large-scale industrial production of aromatics is achieved through aromatics combined units, among which the disproportionation and alkyl transfer of toluene with carbon nine (C9A), carbon ten (C10A) and heavy aromatics above carbon ten (C10+A) is one of the most important key technologies.

[0003] The diffusion of reactants, intermediates, and reaction products is an important factor affecting catalytic performance. Especially for the disproportionation and transalkylation of toluene and heavy aromatics, the raw materials of the reaction usually contain up to about 30 components ranging from toluene with smaller molecular size to polymethyl naphthalene with larger molecular size. Therefore, the pore properties of the catalyst used for the disproportionation and transalkylation of toluene and heavy aromatics have a significant impact on the reaction diffusion and catalytic performance, and are also an important factor affecting the life of the catalyst. In addition, in the future, the reaction materials of toluene disproportionation and transalkylation will gradually develop towards high-content heavy aromatics. High-heavy aromatic raw materials have higher requirements for diffusion and will significantly affect the service life of the catalyst. However, at present, there is little research on the pore structure and reaction diffusion in toluene and heavy aromatics disproportionation and transalkylation catalysts, especially from the perspective of special molecular sieves or catalyst molding processes.

[0004] Although people have realized the importance of the pore structure of molecular sieve catalysts on reaction diffusion and catalytic performance, the main means reported is to use different adhesives to introduce medium and macropores in molecular sieve catalyst particles, which has limited selection conditions, great difficulty in design prediction, and difficulty in controlling the pore size and distribution repeatability. At present, there is still a lack of a practical and effective design of multi-stage pore structure in toluene and heavy aromatics disproportionation and transalkylation catalysts and its preparation method. For example, patent CN100352549C discloses a toluene shape-selective disproportionation catalyst for preparing p-xylene, and its catalyst has the property of multi-stage pores, which can improve catalytic performance to a certain extent, but the patent only introduces medium and macropores by means of selecting adhesives, and the pore size and distribution are difficult to control, and the total pore volume of the catalyst is not large, which can adapt to the disproportionation reaction of toluene, but when used in the disproportionation and transalkylation reaction of toluene and heavy aromatics, it is difficult to adapt to the mixed raw materials of toluene and heavy aromatics with large molecular size differences, and it is impossible to promote reaction diffusion to a large extent, resulting in low catalytic activity, poor stability of the catalyst, and short life. Summary of the invention

[0005] In order to solve the technical problem that the existing disproportionation and transalkylation catalysts are difficult to adapt to the mixed raw materials of toluene and heavy aromatics and cannot promote the reaction diffusion to a large extent, the present invention provides a toluene and heavy aromatics disproportionation and transalkylation catalyst. The catalyst can adapt to the complexity of reactants, intermediates and reaction products in the disproportionation and transalkylation reaction of toluene and heavy aromatics, effectively promote the reaction diffusion, thereby achieving higher catalytic performance and better catalytic stability.

[0006] The specific technical scheme of the present invention is:

[0007] In a first aspect, the present invention provides a catalyst for the disproportionation and transalkylation of toluene and heavy aromatics, wherein the raw materials of the catalyst include the following components: a microporous molecular sieve, a macroporous binder, and at least two porogens capable of forming pores of different sizes.

[0008] During the disproportionation and transalkylation reaction of toluene and heavy aromatics, the composition of the raw materials and the intermediate products of the reaction are relatively complex, especially in the raw materials with high C9 and C10 contents, the larger molecules have higher requirements on the catalytic and diffusion performance of the catalyst. The present invention adopts microporous molecular sieves, macroporous binders and at least two porogens to match, and endow the catalyst with multi-level pore characteristics of micropores, intercrystalline mesopores and macropores, which is more suitable for providing a catalytic place for reaction and diffusion for molecules of different sizes, and can adapt to the complexity of reactants, intermediates and reaction products in the disproportionation and transalkylation reaction of toluene and heavy aromatics, and greatly improve the catalytic performance and service life (stability) of the catalyst in the disproportionation and transalkylation reaction of toluene and heavy aromatics. In addition, by realizing multi-level pores in the manner of the present invention, it is easy to control the pore size and distribution, and can solve the difficult problems of difficult control of multi-level pore structure distribution and low preparation repeatability in the preparation of molecular sieve catalysts.

[0009] Preferably, the volume of micropores in the catalyst is 0.10 to 0.25 mL / g, the volume of mesopores is 0.10 to 0.35 mL / g, and the volume of macropores is 0.10 to 0.30 mL / g.

[0010] In the disproportionation and transalkylation reaction of toluene and heavy aromatics, the micropores and mesopores in the catalyst can provide active sites and provide space for the diffusion of small-sized molecules, and the macropores can promote the diffusion of molecules of different sizes. On this basis, the present invention combines the characteristics of reactants, intermediates and reaction products in the disproportionation and transalkylation reaction of toluene and heavy aromatics, and after a large number of tests, the volumes of micropores, hollows and macropores in the catalyst are controlled within the ranges of 0.10-0.25mL / g, 0.10-0.35mL / g and 0.10-0.30mL / g, respectively, which is conducive to the collision, reaction and diffusion of the reaction molecules during the catalytic reaction, so that the catalyst has good catalytic performance and stability, and can achieve high conversion rate, high yield, high stability and high heavy aromatic conversion capacity in the disproportionation and transalkylation reaction of toluene and heavy aromatics. When the space occupied by micropores and mesopores in the catalyst is too large and the space occupied by macropores is too small, it will be unfavorable for the diffusion of large-sized molecules, resulting in poor catalytic performance and stability. In addition, it is easy to cause side reactions, which will lead to catalyst deactivation. When the space occupied by micropores and mesopores is too small and the space occupied by macropores is too large, the probability of molecular collision per unit space will be small, which is not conducive to the catalytic reaction.

[0011] Furthermore, the volume of micropores in the catalyst is 0.12-0.20 mL / g, the volume of mesopores is 0.10-0.30 mL / g, and the volume of macropores is 0.10-0.25 mL / g.

[0012] Preferably, the mass ratio of the microporous molecular sieve to the macroporous molecular sieve is 50:45 to 85:15; the mass of the porogen is 3 to 15% of the total mass of the microporous molecular sieve and the macroporous binder.

[0013] Preferably, the microporous molecular sieve comprises one or more of ZSM-12, ZSM-5, MOR, MCM-22, Y and Beta molecular sieves.

[0014] Furthermore, the microporous molecular sieve is a symbiotic molecular sieve having two molecular sieve crystal phases; the symbiotic molecular sieve having two molecular sieve crystal phases includes one or more of MCM-22 / Y, ZSM-5 / MOR, ZSM-12 / MOR, MOR / MCM-22 and ZSM-5 / Beta, wherein the mass ratio of the two molecular sieve crystal phases is 1:10 to 10:1.

[0015] The present invention selects the above-mentioned symbiotic molecular sieve with two specific molecular sieve crystal phases according to the different compositions of toluene and heavy aromatics in the reaction raw materials, and controls the mass ratio of the two molecular sieve crystal phases within a certain range, so as to obtain higher benzene and xylene selectivity, thereby achieving a higher reaction yield.

[0016] Preferably, the microporous molecular sieve is a metal-modified hybrid molecular sieve; the metal includes one or more of platinum, palladium, nickel, cobalt, iron, copper, molybdenum, beryllium, magnesium, calcium, scandium, yttrium, lanthanum, cerium, antimony, bismuth, gold, silver, vanadium, chromium, zinc, gallium, ruthenium, zirconium and niobium.

[0017] When the raw materials for the disproportionation and transalkylation of toluene and heavy aromatics contain a high content of heavy aromatics (C9A, C10A, C10+A), it is easy to cause coking in the microporous molecular sieve, causing it to lose its catalytic activity. However, the hybrid molecular sieve modified with specific metals can hydrogenate and saturate the components that are easy to coke, thereby avoiding the loss of catalytic activity of the microporous molecular sieve in the catalyst and making the catalyst have better stability.

[0018] Preferably, the specific surface area of ​​the microporous molecular sieve is 200 to 600 m 2 / g, pore volume is 0.15~0.45cm 3 / g.

[0019] Preferably, in the microporous molecular sieve, the molar ratio of silicon oxide to aluminum oxide is 30:1 to 150:1.

[0020] Preferably, the macroporous binder includes one or more of macroporous silica gel, macroporous alumina, natural clay, diatomaceous earth, attapulgite, and acidic montmorillonite.

[0021] Preferably, the porogen includes at least two of sesbania powder, starch, methyl cellulose, polyacrylic acid, polyacrylamide, polyethylene glycol, acylated chitosan and chitosan.

[0022] Furthermore, the porogen includes a liquid porogen and a solid porogen; the liquid porogen includes liquid polyethylene glycol and / or liquid polyacrylic acid; the solid porogen includes one or more of sesbania powder, acylated chitosan, methyl cellulose and chitosan.

[0023] When the above-mentioned liquid porogen and solid porogen are combined, not only at least two pores with different sizes can be obtained, but also the following effects are achieved: the liquid porogen polyethylene glycol and / or polyacrylic acid is synthesized from chemical reactions, and the molecular weight can be autonomously regulated according to the characteristics of the reactants, thereby achieving a specific catalytic reaction effect and reducing the generation of by-products; the solid porogen listed in the present invention can play the role of a binder and a lubricant in the process of preparing the catalyst, which is beneficial to the preparation and molding of the catalyst, making the pore size and distribution easy to control, thereby improving the catalytic performance of the catalyst, making the reaction have a higher conversion rate and yield, and making the catalyst have better stability.

[0024] Furthermore, the mass ratio of the liquid porogen to the solid porogen is 0.1:1 to 0.7:1.

[0025] In the porogen, as the proportion of liquid porogen increases, it is beneficial to improve the specificity of the catalyst, but it will have an adverse effect on the catalyst formation, thereby affecting the catalytic activity. Therefore, based on the catalytic specificity and catalytic activity of the catalyst, the present invention controls the mass ratio of the liquid porogen to the solid porogen within the range of 0.1:1 to 0.7:1, which is beneficial to reduce the generation of by-products and improve the conversion rate and yield.

[0026] Furthermore, the molecular weight of the liquid porogen is 400-1000 Da.

[0027] Preferably, the catalyst is loaded with active metal oxides; the active metal oxides include one or more oxides of platinum, palladium, nickel, cobalt, iron, copper, molybdenum, beryllium, magnesium, calcium, scandium, yttrium, lanthanum, cerium, antimony, bismuth, gold, silver, vanadium, chromium, zinc, gallium, ruthenium, zirconium and niobium.

[0028] Xylene is one of the most important products of the toluene disproportionation and transalkylation reaction process. However, the boiling points of the byproduct ethylbenzene and the target product xylene are very close, and the separation is difficult. The present invention uses a specific active metal oxide to modify the catalyst, which can play the following two roles at the same time: on the one hand, it can reduce the generation of ethylbenzene, thereby reducing the load and energy consumption of the subsequent distillation process section; on the other hand, it can also avoid coking in the molecular sieve and improve the stability of the catalyst. In addition, when the above-mentioned active metal oxide is selected, it can produce a strong interaction with the surface of the microporous molecular sieve, which is beneficial to control the grain size and dispersion uniformity of the metal oxide, and is convenient for adjusting the active sites of the catalyst, so as to better play the role of reducing the generation of byproducts and improving the stability of the catalyst.

[0029] Preferably, the mass of the active metal oxide is 0.1-10% of the total mass of the microporous molecular sieve and the macroporous binder.

[0030] In a second aspect, the present invention provides a method for preparing the catalyst, comprising the following steps: mixing a microporous molecular sieve, a macroporous binder and at least two porogens capable of forming pores of different sizes to form catalyst particles, and then calcining the particles to obtain a toluene and heavy aromatic hydrocarbon disproportionation and transalkylation catalyst.

[0031] Preferably, the calcination is carried out in a multi-stage temperature-raising calcination mode, and during the temperature-raising process, a constant temperature plateau period of 1 to 4 hours is maintained at at least two different temperature points, and the calcination temperature is 200 to 600°C.

[0032] The above-mentioned multi-stage temperature-raising calcination method can make the obtained catalyst have higher catalytic activity, and at the same time can improve the catalytic specificity and reduce the generation of by-products.

[0033] Preferably, after calcination, a metal oxide precursor is loaded into the catalyst particles, wherein the metal oxide precursor is a metal ion, and then calcination is performed to convert the metal ions into active metal oxides.

[0034] In a third aspect, the present invention provides an application of the catalyst in the disproportionation and transalkylation reaction of toluene and heavy aromatics.

[0035] Preferably, the reaction conditions for the disproportionation and transalkylation of toluene and heavy aromatics are: reaction pressure 1-4 MPa, reaction temperature 300-480°C, hydrogen-to-hydrocarbon molar ratio 1.0-10, liquid weight space velocity 0.5-6.0 h -1 .

[0036] Compared with the prior art, the present invention has the following advantages:

[0037] (1) In the catalyst of the present invention, a microporous molecular sieve, a macroporous binder and at least two porogens are used in combination, so that the catalyst has the pore characteristics of molecular sieve micropores, intercrystalline mesopores and macropores, which can provide a catalytic site for reaction and diffusion of molecules of different sizes in the disproportionation and transalkylation reactions of toluene and heavy aromatics, thereby achieving better catalytic performance and catalytic stability;

[0038] (2) The catalyst of the present invention can adapt to the complexity of reactants, intermediates and reaction products in the disproportionation and transalkylation reactions of toluene and heavy aromatics by comprehensively controlling the volumes of micropores, mesopores and macropores, and can effectively promote the collision and reaction of reaction molecules while achieving better reaction diffusion, thereby achieving better catalytic performance and catalytic stability;

[0039] (3) In the catalyst of the present invention, by controlling the selection of microporous molecular sieves and porogens, the catalytic specificity and catalytic activity of the disproportionation and transalkylation reactions of toluene and heavy aromatics can be improved, thereby improving the conversion rate and yield, and reducing the generation of by-products; (4) In the catalyst of the present invention, by using hybrid microporous molecular sieves modified with specific metals and loading specific active metal oxides in the catalyst, the generation of by-product ethylbenzene can be reduced, the catalytic stability can be improved, and the catalyst life can be extended. DETAILED DESCRIPTION

[0040] The present invention will be further described below in conjunction with the embodiments.

[0041] Overall embodiment

[0042] A catalyst for disproportionation and transalkylation of toluene and heavy aromatics, wherein the micropore volume of the catalyst is 0.10-0.25 mL / g, the mesopore volume is 0.10-0.35 mL / g, and the macropore volume is 0.10-0.30 mL / g. As further preferred, the micropore volume of the catalyst is 0.12-0.20 mL / g, the mesopore volume is 0.10-0.30 mL / g, and the macropore volume is 0.10-0.25 mL / g.

[0043] As a specific implementation, the raw materials of the catalyst include the following components: a microporous molecular sieve, a macroporous binder and at least two porogens capable of forming pores of different sizes.

[0044] Optionally, the mass ratio of the microporous molecular sieve to the macroporous molecular sieve is 50:45 to 85:15; the mass of the porogen is 3 to 15% of the total mass of the microporous molecular sieve and the macroporous binder.

[0045] Optionally, the microporous molecular sieve includes one or more of ZSM-12, ZSM-5, MOR, MCM-22, Y and Beta molecular sieves. As a further preference, the microporous molecular sieve is a symbiotic molecular sieve having two molecular sieve crystal phases; the symbiotic molecular sieve having two molecular sieve crystal phases includes one or more of MCM-22 / Y, ZSM-5 / MOR, ZSM-12 / MOR, MOR / MCM-22 and ZSM-5 / Beta, wherein the mass ratio of the two molecular sieve crystal phases is 1:10 to 10:1.

[0046] Optionally, the microporous molecular sieve is a metal-modified hybrid molecular sieve; the metal includes one or more of platinum, palladium, nickel, cobalt, iron, copper, molybdenum, beryllium, magnesium, calcium, scandium, yttrium, lanthanum, cerium, antimony, bismuth, gold, silver, vanadium, chromium, zinc, gallium, ruthenium, zirconium and niobium.

[0047] Optionally, the specific surface area of ​​the microporous molecular sieve is 200 to 600 m 2 / g, pore volume is 0.15~0.45cm 3 / g, and the molar ratio of silicon oxide to aluminum oxide is 30:1 to 150:1.

[0048] Optionally, the macroporous binder includes one or more of macroporous silica gel, macroporous alumina, natural clay, diatomaceous earth, attapulgite, and acidic montmorillonite.

[0049] Optionally, the porogen includes a liquid porogen and a solid porogen; the liquid porogen includes liquid polyethylene glycol and / or liquid polyacrylic acid; the solid porogen includes one or more of sesbania powder, acylated chitosan, methyl cellulose and chitosan. As further preferred, the mass ratio of the liquid porogen to the solid porogen is 0.1:1 to 0.7:1. As further preferred, the molecular weight of the liquid porogen is 400 to 1000 Da.

[0050] As a specific embodiment, the catalyst is loaded with active metal oxides; the active metal oxides include one or more oxides of platinum, palladium, nickel, cobalt, iron, copper, molybdenum, beryllium, magnesium, calcium, scandium, yttrium, lanthanum, cerium, antimony, bismuth, gold, silver, vanadium, chromium, zinc, gallium, ruthenium, zirconium and niobium.

[0051] Optionally, the mass of the active metal oxide is 0.1-10% of the total mass of the microporous molecular sieve and the macroporous binder.

[0052] A method for preparing the catalyst comprises the following steps: mixing a microporous molecular sieve, a macroporous binder and at least two porogens capable of forming pores of different sizes to form catalyst particles, and then calcining the particles to obtain a toluene and heavy aromatic hydrocarbon disproportionation and transalkylation catalyst.

[0053] As a specific implementation, after calcination, a metal oxide precursor is loaded into the catalyst particles, wherein the metal oxide precursor is a metal ion, and then calcination is performed to convert the metal ions into active metal oxides.

[0054] As a specific implementation manner, the calcination adopts a multi-stage temperature rising calcination method, and during the temperature rising process, a constant temperature plateau period of 1 to 4 hours is maintained at at least two different temperature points, and the calcination temperature is 200 to 600°C.

[0055] The catalyst is applicable to the disproportionation and transalkylation reaction of toluene and heavy aromatics.

[0056] As a specific embodiment, the reaction conditions of the disproportionation and transalkylation reaction of toluene and heavy aromatics are: reaction pressure 1-4 MPa, reaction temperature 300-480°C, hydrogen-to-hydrocarbon molar ratio 1.0-10, liquid weight space velocity 0.5-6.0 h -1 .

[0057] Example 1

[0058] The silicon oxide / aluminum oxide molar ratio is 48 / 1 and the specific surface area is 385m 2 / g, pore volume is 0.41cm 3 / g, hydrogen-type 1wt% Ag hybrid (i.e., the mass proportion of Ag in Beta molecular sieve is 1wt%) Beta molecular sieve with a crystal phase ratio of 7 / 3, macroporous alumina, polyethylene glycol with a molecular weight of 400Da, and methyl cellulose with a molecular weight of 10000Da are kneaded, extruded, dried, and crushed into catalyst particles with a length of 2 to 4mm in a mass ratio of 75:25:3:8. The above catalyst particles are heated to 350°C at a heating rate of 3°C / min in a muffle furnace with ventilation circulation, and calcined for 1h, and then heated to 540°C at a heating rate of 1°C / min and calcined for 3h to obtain multi-level porous hydrogen-type Beta catalyst particles. Then, using nickel nitrate solution as a precursor solution, 0.5% Ni (0.5% means that the mass of Ni species on the catalyst after subsequent calcination is 0.5% of the mass of the catalyst) is loaded on the above catalyst particles by an equal volume vacuum impregnation method, and after calcination at 520°C for 2 hours in a ventilated circulation muffle furnace, a 0.5% Ni / 1% Ag-Beta catalyst is obtained. Then, using ammonium molybdate and lanthanum nitrate solution as precursor solutions, 1.5% Mo and 4% La are loaded on the catalyst by an equal volume impregnation method (1.5% and 4% means that the mass of Mo species and La species on the catalyst after subsequent calcination is 1.5% and 4% of the mass of the catalyst, respectively), and after calcination at 520°C for 2 hours in a ventilated circulation muffle furnace, a 1.5% Mo / 4% La / 0.5% Ni / 1% Ag-Beta catalyst, i.e., a toluene and heavy aromatics disproportionation and transalkylation catalyst, is obtained. The micropore volume of the prepared catalyst is 0.20 mL / g, the mesopore volume is 0.25 mL / g, the macropore volume is 0.16 mL / g, the compressive strength of the catalyst is 118 N / cm, and the wear rate of the catalyst is 0.08%.

[0059] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 55 / 45, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 18wt%. At a reaction temperature of 378°C and a liquid phase space velocity of 3.0h -1 The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: the raw material reaction conversion rate was 49.1%, the benzene and xylene yields were 91.7%, and the catalyst stability remained unchanged at the fixed bed reaction temperature for 1000 hours of continuous reaction while maintaining the reaction conversion rate greater than 48.5wt%.

[0060] Example 2

[0061] The silicon oxide / aluminum oxide molar ratio is 35 / 1 and the specific surface area is 413m 2 / g, pore volume is 0.44cm 3 / g, hydrogen-type 2wt% Fe and 0.5wt% Ni hybrid symbiotic MOR / MCM-22 molecular sieve with a crystal phase ratio of 8 / 2 (i.e., the mass proportions of Fe and Ni in the symbiotic MOR / MCM-22 molecular sieve are 2wt% and 0.5wt%, respectively), macroporous alumina, natural clay, dry starch with a molecular weight of 1000Da, and field sesbania powder with a molecular weight of 50000Da are mixed and kneaded in a mass ratio of 80:20:4:4, extruded, dried and crushed into catalyst particles with a length of 2 to 4mm. The above catalyst particles are heated to 540°C at a heating rate of 3°C / min in a muffle furnace with ventilation circulation, and calcined for 2h to obtain multi-level porous hydrogen-type MOR / Y catalyst particles. Then, ammonium molybdate and palladium nitrate solution are used as precursor solutions, and 4% Mo and 0.3% Pd are loaded on the above catalyst particles by an equal volume vacuum impregnation method (4% and 0.3% refer to the mass of Mo species and Pd species on the catalyst after subsequent calcination, which are 4% and 0.3% of the mass of the catalyst, respectively). After calcination at 520° C. for 2 hours in a muffle furnace with ventilation circulation, a 4% Mo / 0.3% Pd / 2% Fe+0.5% Ni-MOR / MCM-22 catalyst, i.e., a catalyst for the disproportionation and transalkylation of toluene and heavy aromatics, is obtained. The prepared catalyst has a micropore volume of 0.18 mL / g, a mesopore volume of 0.21 mL / g, a macropore volume of 0.23 mL / g, a compressive strength of 103 N / cm, and a wear rate of 0.1%.

[0062] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 50 / 50, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 15wt%. The reaction temperature was 375°C and the liquid phase space velocity was 3.0h -1 The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: feed conversion rate was 49.8%, benzene and xylene yields were 93.1%, and the catalyst stability remained unchanged at the fixed bed reaction temperature for 1000 hours of continuous reaction while maintaining the reaction conversion rate greater than 49.3wt%.

[0063] Example 3

[0064] The silicon oxide / aluminum oxide molar ratio is 32 / 1 and the specific surface area is 437m 2 / g, pore volume is 0.46cm 3 / g, hydrogen-type 1wt% Zn hybrid symbiotic ZSM-5 / MOR molecular sieve with a crystal phase ratio of 4 / 6 (i.e., the mass proportion of Zn in the symbiotic ZSM-5 / MOR molecular sieve is 1wt%), acidic montmorillonite, and methyl cellulose with a molecular weight of 10000Da are kneaded, extruded, dried, and crushed into catalyst particles with a length of 2 to 4 mm in a mass ratio of 80:20:8. The above catalyst particles are heated to 380°C at a heating rate of 2°C / min in a muffle furnace with ventilation circulation, roasted for 1h, and then heated to 540°C at a heating rate of 2°C / min, and roasted for 2h to obtain multi-level porous hydrogen-type ZSM-5 / MOR catalyst particles. Then, cerium nitrate solution was used as a precursor solution, and 4% Ce was loaded on the above catalyst particles by an equal volume vacuum impregnation method (4% means that the mass of Ce species on the catalyst after subsequent calcination is 4% of the mass of the catalyst), and 4% Ce / 1% Zn-ZSM-5 / MOR catalyst was obtained after calcination at 520°C for 2 hours in a muffle furnace with ventilation circulation. Then, bismuth nitrate solution was used as a precursor solution, and 3% Bi was loaded on the catalyst by an equal volume impregnation method (3% means that the mass of Bi species on the catalyst after subsequent calcination is 3% of the mass of the catalyst), and 3% Bi-4% Ce / 1% Zn-ZSM-5 / MOR catalyst, i.e., toluene and heavy aromatics disproportionation and transalkylation catalyst, was obtained after calcination at 520°C for 2 hours in a muffle furnace with ventilation circulation. The micropore volume of the prepared catalyst is 0.16 mL / g, the mesopore volume is 0.26 mL / g, the macropore volume is 0.14 mL / g, the compressive strength of the catalyst is 127 N / cm, and the wear rate of the catalyst is 0.06%.

[0065] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 53 / 47, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 22wt%. The reaction temperature was 380°C and the liquid phase space velocity was 3.5h -1 The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: feed conversion rate 48.5%, benzene and xylene yields 92.3%, and catalyst stability at a fixed bed reaction temperature of 1000 hours of continuous reaction while maintaining a reaction conversion rate greater than 48.3wt%.

[0066] Example 4

[0067] The silicon oxide / aluminum oxide molar ratio is 52 / 1 and the specific surface area is 409m 2 / g, pore volume is 0.52cm 3 / g, a hydrogen-type 1.2wt% Co hybrid symbiotic ZSM-12 / MOR molecular sieve with a crystal phase ratio of 2 / 8 (i.e., the mass proportion of Co in the symbiotic ZSM-5 / MOR molecular sieve is 1.2wt%), acidic montmorillonite, polyethylene glycol with a molecular weight of 600Da, and chitosan with a molecular weight of 30000Da are kneaded, extruded, dried, and crushed into catalyst particles with a length of 2 to 4mm in a mass ratio of 70:30:3:3. The above catalyst particles are heated to 350°C at a heating rate of 2°C / min in a muffle furnace with ventilation circulation, calcined for 1h, and then heated to 540°C at a heating rate of 2°C / min, calcined for 2h, to obtain hydrogen-type ZSM-12 / MOR catalyst particles with multi-level pores. Then, using copper nitrate and ammonium molybdate solution as precursor solution, 1.5% Cu and 4% Mo are loaded on the above catalyst particles by equal volume vacuum impregnation method (1.5% and 4% means that the mass of Cu species and Mo species on the catalyst after subsequent calcination is 1.5% and 4% of the mass of the catalyst respectively), and 1.5% Cu / 4% Mo / 1.2% Co-ZSM-12 / MOR catalyst is obtained after calcination at 520° C. for 2 hours in a muffle furnace with ventilation circulation. Then, using chloroplatinic acid solution as precursor solution, 0.2% Pt is loaded on the catalyst by equal volume impregnation method (0.2% means that the mass of Pt species on the catalyst after subsequent calcination is 0.2% of the mass of the catalyst), and 0.2% Pt-1.5% Cu / 4% Mo / 1.2% Co-ZSM-12 / MOR catalyst, i.e., toluene and heavy aromatics disproportionation and transalkylation catalyst, is obtained after calcination at 520° C. for 2 hours in a muffle furnace with ventilation circulation. The micropore volume of the prepared catalyst is 0.20 mL / g, the mesopore volume is 0.24 mL / g, the macropore volume is 0.20 mL / g, the compressive strength of the catalyst is 121 N / cm, and the wear rate of the catalyst is 0.09%.

[0068] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 56 / 44, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 25wt%. The reaction temperature was 373°C and the liquid phase space velocity was 3.0h -1 The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: feed conversion rate was 49.3%, benzene and xylene yields were 91.6%, and the catalyst stability remained unchanged at the fixed bed reaction temperature for 1000 hours of continuous reaction while maintaining the reaction conversion rate greater than 49.5wt%.

[0069] Example 5

[0070] The difference between this embodiment and embodiment 2 is that the molar ratio of silicon oxide to aluminum oxide is 35 / 1 and the specific surface area is 413 m2 / g, pore volume is 0.44cm 3 / g, the hydrogen-type 2wt% Fe and 0.5wt% Ni hybrid MOR / MCM-22 molecular sieve with a crystal phase ratio of 8 / 2 was replaced with a silicon oxide / alumina molar ratio of 35 / 1 and a specific surface area of ​​320m 2 / g, pore volume is 0.28cm 3 / g, hydrogen-type 2wt% Fe and 0.5wt% Ni hybrid intergrowth X / ZSM-5 molecular sieve with a crystal phase ratio of 8 / 2. The rest of the raw materials and preparation process are the same.

[0071] The micropore volume of the catalyst prepared in this example is 0.16 mL / g, the mesopore volume is 0.19 mL / g, the macropore volume is 0.17 mL / g, the compressive strength of the catalyst is 90 N / cm, and the wear rate of the catalyst is 0.5%.

[0072] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 50 / 50, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 15wt%. The reaction temperature was 375°C and the liquid phase space velocity was 3.0h -1 The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: feed conversion rate was 43.6%, benzene and xylene yields were 83.1%, and the catalyst stability was maintained at a reaction conversion rate greater than 46wt%. The fixed bed reaction temperature for 1000 hours of continuous reaction increased by 12°C.

[0073] Data analysis and conclusion: Compared with Example 2, the catalyst reaction yield and stability of Example 5 are lower. This indicates that the selection of the co-existing molecular sieve will affect the catalytic activity and stability of the catalyst. When the X / ZSM-5 molecular sieve in Example 5 is used, it is difficult to obtain an ideal catalytic reaction effect.

[0074] Example 6

[0075] The only difference between this example and Example 1 is that the Beta molecular sieve used in this example is not Ag hybridized and modified. The rest of the raw materials and preparation process are the same.

[0076] The micropore volume of the catalyst prepared in this example is 0.18 mL / g, the mesopore volume is 0.22 mL / g, the macropore volume is 0.13 mL / g, the compressive strength of the catalyst is 86 N / cm, and the wear rate of the catalyst is 0.2%.

[0077] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 55 / 45, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 18wt%. At a reaction temperature of 378°C and a liquid phase space velocity of 3.0h -1 The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: raw material conversion rate was 46.3%, benzene and xylene yields were 87.8%, and the catalyst stability was maintained at a reaction conversion rate greater than 46wt%. The fixed bed reaction temperature rose by 8°C for 1000 hours of continuous reaction.

[0078] Data analysis and conclusion: Compared with Example 1, the catalyst stability of Example 6 is poor. This is because the Ag-modified hybrid molecular sieve used in Example 1 can prevent the microporous molecular sieve in the catalyst from losing its catalytic activity, thereby making the catalyst have better stability.

[0079] Example 7

[0080] The difference between this embodiment and embodiment 1 is that the ammonium molybdate and lanthanum nitrate solution are replaced with ammonium perrhenate and phosphotungstic acid solution, and 2.5% rhenium and 3% tungsten are loaded on the catalyst by equal amount impregnation method (2% and 3% means that the mass of Re species and W species on the catalyst after subsequent calcination is 2% and 3% of the mass of the catalyst, respectively). The rest of the raw materials and preparation process are the same.

[0081] The micropore volume of the catalyst prepared in this example is 0.13 mL / g, the mesopore volume is 0.14 mL / g, the macropore volume is 0.08 mL / g, the compressive strength of the catalyst is 72 N / cm, and the wear rate of the catalyst is 0.12%.

[0082] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 55 / 45, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 18wt%. At a reaction temperature of 378°C and a liquid phase space velocity of 3.0h -1 The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: feed conversion rate 46.9%, benzene and xylene yields 89.2%, and catalyst stability. The fixed bed reaction temperature was increased by 10°C for 1000 hours of continuous reaction while maintaining the reaction conversion rate greater than 46.5wt%.

[0083] Data analysis and conclusion: Compared with Example 1, the catalyst yield of Example 7 is lower and the stability is poorer. This is because the interaction between the active metal oxide in Example 7 and the surface of the microporous molecular sieve is weak, which is not conducive to the control of the metal oxide grain size and dispersion uniformity, and thus the active metal oxide has poor effects in reducing by-product formation and improving catalyst stability.

[0084] Example 8

[0085] The only difference between this example and Example 1 is that the polyethylene glycol with a molecular weight of 400 Da is replaced with an equal amount of methyl cellulose with a molecular weight of 10000 Da. The rest of the raw materials and preparation process are the same.

[0086] The micropore volume of the catalyst prepared in this example is 0.15 mL / g, the mesopore volume is 0.19 mL / g, the macropore volume is 0.17 mL / g, the compressive strength of the catalyst is 83 N / cm, and the wear rate of the catalyst is 0.6%.

[0087] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 55 / 45, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 18wt%. At a reaction temperature of 378°C and a liquid phase space velocity of 3.0h -1 The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: raw material conversion rate was 47.3%, benzene and xylene yields were 89.6%, and the catalyst stability was maintained at a reaction conversion rate greater than 47wt%. The fixed bed reaction temperature rose by 6°C for 1000 hours of continuous reaction.

[0088] Example 9

[0089] The difference between this embodiment and embodiment 1 is that the methylcellulose with a molecular weight of 10000Da is replaced with polyethylene glycol with a molecular weight of 400Da of the same mass. The rest of the raw materials and preparation process are the same.

[0090] The micropore volume of the catalyst prepared in this example is 0.2 mL / g, the mesopore volume is 0.23 mL / g, the macropore volume is 0.11 mL / g, the compressive strength of the catalyst is 91 N / cm, and the wear rate of the catalyst is 0.4%.

[0091] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 55 / 45, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 18wt%. At a reaction temperature of 378°C and a liquid phase space velocity of 3.0h -1The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: raw material conversion rate was 46.8%, benzene and xylene yields were 89.1%, and the catalyst stability was maintained at a reaction conversion rate greater than 46wt%. The fixed bed reaction temperature rose by 7°C for 1000 hours of continuous reaction.

[0092] Data analysis and conclusion: Compared with Example 1, the catalyst yield and stability of Example 8 are lower, and the catalyst conversion rate, yield and stability of Example 9 are lower. This shows that by compounding the solid porogen and the liquid porogen, the catalyst can have higher catalytic activity and specificity. This is because the liquid porogen is easy to control the pore size, thereby achieving a specific catalytic reaction effect and reducing the generation of by-products; while the solid catalyst can play the role of a binder and lubricant during the molding process, so that the catalyst has higher catalytic activity and stability.

[0093] Example 10

[0094] The difference between this embodiment and embodiment 1 is that the mass ratio of Beta molecular sieve, macroporous alumina, polyethylene glycol with a molecular weight of 400 Da, and methyl cellulose with a molecular weight of 10000 Da is changed from 75:25:3:8 to 75:25:1:1. The rest of the raw materials and preparation process are the same.

[0095] The micropore volume of the catalyst prepared in this example is 0.17 mL / g, the mesopore volume is 0.09 mL / g, the macropore volume is 0.09 mL / g, the compressive strength of the catalyst is 95 N / cm, and the wear rate of the catalyst is 0.6%.

[0096] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 55 / 45, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 18wt%. At a reaction temperature of 378°C and a liquid phase space velocity of 3.0h -1 The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: feed conversion rate 47.3%, benzene and xylene yields 90.3%, and catalyst stability. The fixed bed reaction temperature was increased by 10°C for 1000 hours of continuous reaction while maintaining a reaction conversion rate greater than 47wt%.

[0097] Embodiment 11

[0098] The difference between this embodiment and embodiment 1 is that the mass ratio of Beta molecular sieve, macroporous alumina, polyethylene glycol with a molecular weight of 400 Da, and methyl cellulose with a molecular weight of 10000 Da is changed from 75:25:3:8 to 90:10:5:12. The rest of the raw materials and preparation process are the same.

[0099] The micropore volume of the catalyst prepared in this example is 0.27 mL / g, the mesopore volume is 0.31 mL / g, the macropore volume is 0.08 mL / g, the compressive strength of the catalyst is 56 N / cm, and the wear rate of the catalyst is 1.8%.

[0100] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 55 / 45, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 18wt%. At a reaction temperature of 378°C and a liquid phase space velocity of 3.0h -1 The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: raw material conversion rate was 45.8%, benzene and xylene yields were 87.5%, and the catalyst stability was maintained at a reaction conversion rate greater than 45wt%. The fixed bed reaction temperature rose by 7°C for 1000 hours of continuous reaction.

[0101] Data analysis and conclusion: Compared with Example 1, the catalyst conversion rate and yield of Examples 10 and 11 are lower, and the stability is poorer. This shows that the volume of each level of pores in the catalyst will affect the catalytic activity and stability. When the volume of micropores, mesopores and macropores is controlled within the range of the present invention, higher catalytic activity and stability can be achieved.

[0102] Comparative Example 1

[0103] The silicon oxide / aluminum oxide molar ratio is 40 / 1 and the specific surface area is 351m 2 / g, pore volume is 0.41cm 3 / g hydrogen-type MOR molecular sieve and conventional alumina are kneaded, extruded, dried and crushed into catalyst particles with a length of 2 to 4 mm in a mass ratio of 70:30. The above catalyst particles are heated to 350°C at a heating rate of 2°C / min in a ventilated circulation muffle furnace, roasted for 1 hour, and then heated to 540°C at a heating rate of 2°C / min and roasted for 2 hours to obtain MOR catalyst particles. Then, lanthanum nitrate solution is used as a precursor solution, and 2% La is loaded on the above catalyst particles by an equal volume vacuum impregnation method (2% means that the mass of La species on the catalyst after subsequent roasting is 2% of the mass of the catalyst), and 2% La-MOR catalyst is obtained after roasting at 520°C for 2 hours in a ventilated circulation muffle furnace. Then, 0.2% Pt was loaded on the catalyst by equal amount impregnation method using chloroplatinic acid solution as precursor solution (0.2% means that the mass of Pt species on the catalyst after subsequent calcination is 0.2% of the mass of the catalyst), and calcined at 520° C. for 2 hours in a muffle furnace with ventilation circulation to obtain a 0.2% Pt-2% La-MOR catalyst, i.e., a catalyst for disproportionation and transalkylation of toluene and heavy aromatics. The prepared catalyst has a micropore volume of 0.20 mL / g, a mesopore volume of 0.11 mL / g, a macropore volume of 0.08 mL / g, a compressive strength of 121 N / cm, and a wear rate of 0.12%.

[0104] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 55 / 45, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 18wt%. The reaction temperature was 375°C, and the liquid phase space velocity was 3.0h -1 The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: feed conversion rate 43.5%, benzene and xylene yields 90.2%, and catalyst stability. The fixed bed reaction temperature was raised 4 times, each time by 3°C, for 1000 hours of continuous reaction while maintaining the reaction conversion rate greater than 42.5wt%.

[0105] Comparative Example 2

[0106] The silicon oxide / aluminum oxide molar ratio is 40 / 1 and the specific surface area is 351m 2 / g, pore volume is 0.41cm 3 / g hydrogen-type MOR molecular sieve with a silicon oxide / alumina molar ratio of 32 / 1 and a specific surface area of ​​376m 2 / g, pore volume is 0.43cm 3 / g of hydrogen-type Beta molecular sieve and acidic montmorillonite are kneaded, extruded, dried and crushed into catalyst particles with a length of 2 to 4 mm in a mass ratio of 40:30:30. The above catalyst particles are heated to 350°C at a heating rate of 2°C / min in a ventilation circulation muffle furnace, roasted for 1h, and then heated to 540°C at a heating rate of 2°C / min and roasted for 2h to obtain MOR / Beta mixed catalyst particles. Then, ammonium molybdate and copper nitrate solution are used as precursor solutions, and 4% Mo and 1% Cu are loaded on the above catalyst particles by an equal volume vacuum impregnation method (4% and 1% refer to the mass of Mo species and Cu species on the catalyst after subsequent roasting, which are 4% and 1% of the mass of the catalyst, respectively). After roasting at 520°C for 2 hours in a ventilation circulation muffle furnace, a 4% Mo-1% Cu-MOR / Beta catalyst is obtained, that is, a toluene and heavy aromatic hydrocarbon disproportionation and transalkylation catalyst. The micropore volume of the prepared catalyst is 0.24 mL / g, the mesopore volume is 0.13 mL / g, the macropore volume is 0.06 mL / g, the compressive strength of the catalyst is 106 N / cm, and the wear rate of the catalyst is 0.21%.

[0107] The above catalyst was loaded into a fixed bed microreactor, and an appropriate amount of inert glass beads were filled in the upper and lower parts. A mixed aromatic hydrocarbon of toluene and heavy aromatic hydrocarbons was used as the raw material, and the molar ratio of toluene / heavy aromatic hydrocarbons was 50 / 50, wherein the content of C10 and C11 heavy aromatic hydrocarbons in the mixed aromatic hydrocarbon raw material was 23wt%. At a reaction temperature of 376°C and a liquid phase space velocity of 3.0h -1 The catalytic performance was evaluated under the condition of hydrogen-to-hydrocarbon ratio of 3.0, and the results were as follows: feed conversion rate 43.1%, benzene and xylene yields 90.7%, and catalyst stability. The fixed bed reaction was continuously reacted for 1000 hours under the condition of maintaining the reaction conversion rate greater than 42wt%, and the temperature was raised 3 times, each time by 3°C.

[0108] Data analysis and conclusion: Compared with Examples 1 to 4, the catalyst conversion rate and yield of Comparative Examples 1 and 2 are lower and the stability is poorer. This shows that the present invention can achieve high yield, high conversion rate and high stability for toluene and heavy aromatic hydrocarbon disproportionation and transalkylation catalysts by adopting suitable porogens and controlling factors such as the selection of microporous molecular sieves, the volume of each level of pores and the loading of active metal oxides.

[0109] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0110] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. Use of a catalyst in catalyzing the disproportionation and transalkylation reaction of toluene and heavy aromatics, characterized in that: The raw materials of the catalyst include a microporous molecular sieve, a macroporous binder and at least two porogens capable of forming pores of different sizes; the porogens include a liquid porogen and a solid porogen, the liquid porogen includes liquid polyethylene glycol and / or liquid polyacrylic acid, and the solid porogen includes at least one of sesbania powder, acylated chitosan, methyl cellulose and chitosan; the volumes of micropores, mesopores and macropores in the catalyst are 0.10-0.25 mL / g, 0.10-0 .35mL / g, 0.10~0.30mL / g; the microporous molecular sieve includes at least one of MCM-22 / Y, ZSM-5 / MOR, ZSM-12 / MOR, MOR / MCM-22 and ZSM-5 / Beta, and is modified with one or more metals of platinum, palladium, nickel, cobalt, iron, copper, molybdenum, beryllium, magnesium, calcium, scandium, yttrium, lanthanum, cerium, antimony, bismuth, gold, silver, vanadium, chromium, zinc, gallium, ruthenium, zirconium and niobium.

2. The use according to claim 1, characterized in that The micropore volume of the catalyst is 0.12-0.20 mL / g, the mesopore volume is 0.10-0.30 mL / g, and the macropore volume is 0.10-0.25 mL / g.

3. The use according to claim 1, characterized in that The mass ratio of the microporous molecular sieve to the macroporous binder is 50:45-85:

15.

4. The use according to claim 1, characterized in that The mass of the porogen is 3-15% of the total mass of the microporous molecular sieve and the macroporous binder.

5. The use according to claim 1, characterized in that The specific surface area of ​​the microporous molecular sieve is 200-600 m 2 / g.

6. The use according to claim 1 or 5, characterized in that: The pore volume of the microporous molecular sieve is 0.15~0.45cm 3 / g.

7. The use according to claim 1, characterized in that In the microporous molecular sieve, the molar ratio of silicon oxide to aluminum oxide is 30:1 to 150:

1.

8. The use according to claim 1, characterized in that The catalyst is loaded with active metal oxides; the active metal oxides include one or more oxides of platinum, palladium, nickel, cobalt, iron, copper, molybdenum, beryllium, magnesium, calcium, scandium, yttrium, lanthanum, cerium, antimony, bismuth, gold, silver, vanadium, chromium, zinc, gallium, ruthenium, zirconium and niobium.

9. The use according to claim 1, characterized in that The preparation method of the catalyst comprises the following steps: mixing a microporous molecular sieve, a macroporous binder and at least two porogens capable of forming pores of different sizes to form catalyst particles, and then calcining the particles to obtain a toluene and heavy aromatic hydrocarbon disproportionation and alkyl transfer catalyst.

10. The use according to claim 9, characterized in that The calcination adopts a multi-stage temperature rise calcination method, and during the temperature rise process, at least two different temperature points are kept at a constant temperature for a 1-4h plateau period, and the calcination temperature is 200-600°C.

Citation Information

Patent Citations

  • Preparation method of catalyst for paraxylene produced by toluene selective disproportionation

    CN100352549C

  • Method used for heavy arene light formation and alkyl transfer

    CN100999433A

  • Novel preparation method of hierarchical pore chitin material

    CN111040234A

  • Aromatic disproportionation and transalkylation catalyst as well as preparation method and application thereof

    CN114904571A

  • Amorphous silicon-containing material with hierarchical porosity

    US20110039102A1