A solar interface evaporator, preparation and application

By combining chitosan aerogel with vertically arranged channel structures in solar interface evaporators, the problems of slow evaporation efficiency and low light absorption efficiency are solved, rapid evaporation and high-efficiency light absorption are achieved, and self-cleaning mechanism is used to achieve rapid evaporation and high-efficiency light absorption. Improves salt resistance and is suitable for seawater desalination.

CN116143216BActive Publication Date: 2024-11-22TECHNICAL INST OF PHYSICS & CHEMISTRY - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111394275.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-23
Publication Date
2024-11-22
Estimated Expiration
2041-11-23

AI Technical Summary

Technical Problem

The existing solar interface evaporators have problems such as slow evaporation efficiency, low light absorption efficiency and insufficient salt resistance during seawater desalination. The traditional carbonization method may damage the chitosan aerogel structure, affecting the water transportation rate and ion diffusion rate. .

Method used

Using a double-layer structure composed of chitosan aerogel and carbon nanotubes with vertically arranged channel structures, carbon nanotubes are used as photothermal layer to improve light absorption and thermal management. Chitosan aerogels are quickly transported through capillary action. Moisture and self-cleaning is achieved through a salt concentration gradient to form a stable bilayer structure to improve salt resistance.

Benefits of technology

It achieves efficient light absorption, rapid evaporation and good salt resistance, with an evaporation rate of 1.3kg/m²h, an evaporation efficiency of more than 96%, and a light absorption rate of more than 95% in the wavelength range of 200-1500nm, and is also performed in seawater desalination. Prospects for good practical application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116143216B_ABST
    Figure CN116143216B_ABST
Patent Text Reader

Abstract

The present invention discloses a solar interface evaporator, preparation and application. The present invention uses carbon nanotubes with good photothermal conversion performance and wide solar band absorption as a photothermal layer, and then combines it with chitosan aerogel with a vertically arranged pore structure to form a double-layer structure, and quickly transports water to the evaporation interface of the photothermal layer through the capillary action of the chitosan aerogel, and uses the good thermal management ability of the chitosan aerogel to reduce the heat conduction loss of the photothermal layer to the water body, thereby concentrating the heat at the evaporation interface. The solar interface evaporator integrates multiple functions such as light absorption, water transportation, thermal management and salt resistance. Under the synergistic effect of chitosan aerogel and carbon nanotubes, it can efficiently use solar energy for seawater desalination, has the advantages of high light absorption efficiency, fast evaporation rate, green, energy saving, environmental protection, etc., and has good application prospects in the field of solar seawater desalination.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solar seawater desalination, and more specifically, to a solar interface evaporator, preparation and application thereof. Background Art

[0002] With the continuous development of human society, the water demand for life, industry and agriculture has also greatly increased. The shortage of fresh water resources has become an increasingly serious global problem. Solar desalination is considered to be one of the promising and sustainable solutions to solve the shortage of fresh water resources. In recent years, with the emergence of new photothermal materials and new bionic design concepts, solar-driven interfacial evaporators have continued to develop. Due to their advantages of low cost and high photothermal conversion efficiency, they have attracted great attention in application fields such as seawater desalination, sewage treatment and steam power generation.

[0003] Unlike traditional solar desalination technology, the solar-driven interfacial evaporator is a composite material that can float on the water surface. It converts solar energy into thermal energy through photothermal materials, and uses this heat only to heat the water at the interface, thereby achieving efficient water evaporation. An efficient solar interfacial evaporator usually needs to have excellent photothermal conversion performance, good thermal management and fast water transport capabilities. In addition, the evaporator used in the field of seawater desalination also needs to have good salt resistance. Therefore, how to design a solar interfacial evaporator that integrates multiple functions such as light absorption, thermal management, water transportation and salt resistance remains a challenge.

[0004] In recent years, solar evaporators have attracted great attention. For example, Chinese patent CN 111170393 A discloses a solar evaporator with a hollow structure, a preparation method and an application thereof, wherein the solar evaporator is prepared by using a hollow foam with a porous polymer skeleton structure as a base material and then wrapping a layer of photothermal material on its outer surface. The internal hollow structure enables it to have excellent thermal insulation performance, which is conducive to reducing the loss of heat to the water body. However, due to the high tortuosity of the porous polymer skeleton structure, the water transport rate and ion diffusion rate of the solar evaporator are slow. In addition, during the long-term seawater desalination process, salt will gradually precipitate and block the pores, resulting in the inability of steam to overflow, which significantly reduces the photoevaporation performance. In order to improve the water transport rate and ion diffusion rate, Chinese patent CN 112794307 A discloses a method for preparing a double-layer integral photothermal conversion material, wherein a chitosan aerogel matrix with a vertical pore structure is prepared by low-temperature freezing and freeze-drying, and then high-temperature carbonization is performed to obtain an in-situ carbonized chitosan aerogel. A large number of vertically arranged pore structures can provide sufficient water for the upper light absorber of the solar evaporator. However, the partial carbonization method may cause the destruction of the upper structure of the chitosan aerogel and the shrinkage of the volume, interfering with the water transport rate and ion diffusion rate. In addition, the light absorption rate of the photothermal material formed by partial carbonization needs to be improved. Summary of the invention

[0005] The first purpose of the present invention is to provide a solar interface evaporator, which integrates multiple functions such as light absorption, water transportation, thermal management and salt resistance, has the advantages of high light absorption efficiency, fast evaporation rate, green, energy saving, environmental protection, etc., and can achieve self-floating.

[0006] The second object of the present invention is to provide a method for preparing a solar interface evaporator. The method has simple process, abundant raw material sources, and is green and renewable.

[0007] The third object of the present invention is to provide an application of the above solar interface evaporator in solar seawater desalination.

[0008] In order to achieve the above first object, the present invention adopts the following technical scheme:

[0009] The invention discloses a solar interface evaporator, which is composed of chitosan aerogel with a vertically arranged pore structure used as a lower water supply layer and carbon nanotubes used as an upper photothermal layer.

[0010] In the present invention, carbon nanotubes with good photothermal conversion performance and wide solar band absorption are used as the photothermal layer, and then combined with chitosan aerogel with a vertically arranged pore structure to form a double-layer solar interface evaporator structure, which not only solves the problems of slow evaporation efficiency and low light absorption efficiency of traditional solar interface evaporators, but also has a self-cleaning function, thereby improving the salt resistance of the solar interface evaporator.

[0011] Specifically, first, as a known ultra-black material, carbon nanotubes have extremely high light absorption rate and good photothermal conversion performance in the entire solar spectrum, which can effectively absorb solar energy and efficiently convert it into thermal energy; second, through the vertically arranged channels and capillary action of the lower chitosan aerogel, water can be quickly transported to the evaporation interface of the photothermal layer, and the heat can be fully concentrated at the evaporation interface, thereby reducing the energy loss of the photothermal layer and improving the evaporation efficiency. In addition, the salt precipitated at the evaporation interface can be transported back to the water body through the salt concentration gradient after the light stops, thereby achieving self-cleaning, having good cycle stability, and improving its salt resistance; third, chitosan contains a large number of positively charged amino groups, which will be firmly adsorbed together with the carbon nanotubes containing negatively charged carboxyl groups under the action of electrostatic adsorption to form a stable double-layer structure, preventing the problem of double-layer structure detachment when the solar interface evaporator is in use; fourth, the carbon nanotubes in the photothermal layer have nanopores. After combining with the chitosan aerogel with micron pores, the micro-nano multi-level channels are conducive to light absorption, thereby further improving the light absorption efficiency. Therefore, under the synergistic effect of chitosan aerogel and carbon nanotubes, the solar interface evaporator has higher light absorption efficiency and faster evaporation rate.

[0012] In the present invention, the prepared chitosan aerogel has a pore diameter of 20 to 50 μm and an interlayer spacing of 50 μm.

[0013] Furthermore, the water supply layer has a thickness of 2 to 2.5 cm.

[0014] Furthermore, the photothermal layer has a thickness of 20 to 40 μm.

[0015] In order to achieve the above second purpose, the present invention adopts the following technical solutions:

[0016] The present invention discloses a method for preparing the above solar interface evaporator, comprising the following steps:

[0017] The carbon nanotube suspension is deposited on a chitosan aerogel having a vertically arranged pore structure, wherein the chitosan aerogel having a vertically arranged pore structure is prepared by an ice template method.

[0018] Furthermore, the carbon nanotube suspension is prepared by mixing carbon nanotubes, a dispersant and water; the concentration of the carbon nanotube suspension is 3 to 10 mg / mL.

[0019] Further, the steps of preparing chitosan aerogel by ice template method are as follows:

[0020] The chitosan is dissolved in an acetic acid aqueous solution to prepare a chitosan slurry, and then the chitosan slurry is injected into an axial freezing device with an axial temperature gradient for freeze molding, and then the frozen chitosan slurry is freeze-dried and vacuum-dried in sequence to obtain the product.

[0021] Furthermore, the axial temperature gradient of the freeze molding is -196°C to -10°C; and the freeze molding time is 15 to 30 minutes.

[0022] In a specific embodiment, the axial freezing device includes a mold for holding chitosan slurry, the bottom of the mold is a copper plate with good thermal conductivity, and the side wall is polytetrafluoroethylene with good thermal insulation and stable chemical properties. The chitosan slurry is frozen and formed by applying a cold source to the bottom to form an axial temperature gradient. The purpose of this is to allow the chitosan slurry to grow vertically upward ice crystals under different temperature gradients, and then sublimate the ice crystals to obtain a vertically arranged pore structure.

[0023] The directional freezing ice template method can be used to prepare chitosan aerogels with low density, high porosity and highly oriented vertically arranged pore structure, achieving the unity of self-floating, thermal management and water transport.

[0024] Furthermore, in the raw materials of the chitosan aerogel, the mass ratio of chitosan, acetic acid and water is 1:2-3:6-8, wherein the chitosan can be obtained by external purchase, the deacetylation degree thereof is controlled at 80-95%, and the viscosity is controlled at 50-800 mPa·s.

[0025] Furthermore, the freeze-drying temperature is -50 to -20°C; the freeze-drying time is 10 to 100 hours; and the freeze-drying pressure is 1 to 100 Pa. Further, in certain specific embodiments of the present invention, for example, the freeze-drying time is 10 to 50 hours, 30 to 70 hours, 50 to 80 hours, 60 to 80 hours, 70 to 85 hours, 70 to 100 hours, etc.; and the freeze-drying pressure is 1 to 50 Pa, 10 to 50 Pa, 20 to 30 Pa, 20 to 70 Pa, 30 to 100 Pa, 50 to 100 Pa, etc.

[0026] Furthermore, the vacuum drying temperature is 60-80°C; the vacuum drying time is 6-12 hours; and the vacuum drying pressure is 100-1000 Pa. Furthermore, in certain specific embodiments of the present invention, for example, the vacuum drying pressure is 100-300 Pa, 100-500 Pa, 200-800 Pa, 500-1000 Pa, 300-600 Pa, etc.

[0027] Furthermore, the mass ratio of the carbon nanotubes to the dispersant is 1:1-2.

[0028] Furthermore, the dispersant includes but is not limited to one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate or sodium dodecyl sulfonate.

[0029] In order to achieve the third objective mentioned above, the present invention discloses an application of the solar interface evaporator as described above in solar seawater desalination.

[0030] In a specific embodiment, when the solar interface evaporator is working, the lower water supply layer provides moisture to the upper photothermal layer, and the upper photothermal layer converts the absorbed solar energy into thermal energy to evaporate the moisture, providing power for the transmission of water in the capillary channels in the lower water supply layer, thereby achieving evaporation and purification of water.

[0031] The beneficial effects of the present invention are as follows:

[0032] The present invention discloses a solar interface evaporator, preparation and application. The solar interface evaporator is composed of chitosan aerogel with a vertically arranged pore structure as a lower water supply layer and carbon nanotubes as an upper photothermal layer. The present invention uses carbon nanotubes with good photothermal conversion performance and wide solar band absorption as the photothermal layer, and then combines them with chitosan aerogel with a vertically arranged pore structure to form a double-layer structure. Water is quickly transported to the evaporation interface of the photothermal layer through the capillary action of the chitosan aerogel, and the good thermal management ability of the chitosan aerogel is used to reduce the heat conduction loss of the photothermal layer to the water body, thereby concentrating the heat at the evaporation interface. The solar interface evaporator integrates multiple functions such as light absorption, water transportation, thermal management and salt resistance. Under the synergistic effect of chitosan aerogel and carbon nanotubes, it can efficiently use solar energy for seawater desalination. It has the advantages of high light absorption efficiency, fast evaporation rate, green, energy saving, environmental protection, etc. After testing, 1 sun illumination intensity (1kW m -2 ) under the condition that the evaporation rate of the solar interface evaporator is 1.3kgm -2 h -1 The evaporation efficiency is above 96%, and the light absorption rate is greater than 95% in the wavelength range of 200 to 1500 nm where the sunlight energy is the strongest. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0034] Figure 1 Actual photos of CA and CA-5 are shown.

[0035] Figure 2 SEM images showing the microstructure of CA;

[0036] Among them, (a) is the CA longitudinal cross-sectional view, and (b) is the CA transverse cross-sectional view.

[0037] Figure 3 A diagram showing the effect of the dye solution rising along the vertical channels inside the CA.

[0038] Figure 4 Scanning electron microscope images (SEM) of the CNT photothermal layers of CA-1, CA-5, and CA-10 are shown;

[0039] Among them, (a) is the SEM image of CA-1, (b) is the SEM image of CA-5, and (c) is the SEM image of CA-10.

[0040] Figure 5 The UV-Vis-NIR absorption spectra of CA and CA-5 are shown.

[0041] Figure 6 The graph shows the temperature variation at the evaporation interface of pure water, CA and CA-5 over time when irradiated for 1 hour under one sun intensity.

[0042] Figure 7 The photographs show the evaporation interface of CA-5 in saline after 8 h of illumination and 4 h of no illumination.

[0043] Figure 8 A schematic diagram of an outdoor condensation water collection device is shown;

[0044] Among them, 1 sunlight, 2 slope, 3 water trough, 4 crystallization dish, 5 solar interface evaporator, 6 high temperature steam, and 7 water droplets.

[0045] Fig. 9 The curves showing the evaporation rate, light intensity and temperature at the evaporation interface of CA-5 from 9:00 to 16:00 are plotted over time.

[0046] Fig.10 The figure shows the changes in ion concentration before and after CA-5 is used in real seawater desalination. DETAILED DESCRIPTION

[0047] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments and figures. It should be understood by those skilled in the art that the content described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0048] The experimental methods used in the following examples are conventional methods unless otherwise specified; the reagents, materials, etc. used in the following examples are commercially available unless otherwise specified. The purchased carbon nanotubes are multi-walled carbon nanotubes with an inner diameter of 5 to 10 nm, an outer diameter of 20 to 40 nm, and a length of 10 to 30 μm.

[0049] Example 1

[0050] Chitosan aerogel (CA) with vertically aligned pore structure was prepared by ice template method:

[0051] (1) Weigh 12 g of chitosan into a 250 mL beaker, add 200 mL of deionized water and then dropwise add 6 mL of acetic acid, and continue stirring for 12 h to completely dissolve the chitosan, thereby preparing a chitosan slurry;

[0052] (2) Weigh 150g of chitosan slurry and pour it into the mold, and then place it on a freezing device for directional freezing. The freezing device includes a cold source pool, a copper plate and liquid nitrogen. Place the mold on the copper plate, pour a certain amount of liquid nitrogen at regular intervals during the freezing process, so that the liquid nitrogen maintains a certain height in the cold source pool, and freeze for 30 minutes to completely solidify the chitosan slurry;

[0053] (3) placing the solidified chitosan slurry into a freeze dryer, with a freeze drying pressure of 20 Pa and a freeze drying time of 72 h;

[0054] (4) The dried sample was placed in a vacuum drying oven. The pressure during the vacuum drying process was 100 Pa and the vacuum drying time was 6 h to obtain CA.

[0055] The scanning electron micrograph of the obtained CA is shown in Figure 2 ,Depend on Figure 2 It is known that the chitosan aerogel prepared by the cold template method has a vertically arranged pore structure with a pore diameter of about 20 to 50 μm and an interlayer spacing of about 50 μm. This vertically arranged pore structure is conducive to transporting water from bottom to top to the top CNT photothermal layer through capillary action.

[0056] In order to better demonstrate the water transport process achieved by capillary action, CA was placed in a dye solution to observe the dye solution rising along the vertical channels of CA. The resulting effect diagram is shown in Figure 3It only takes 30 s for the dye solution to be transported from the bottom to the top of the CA, proving that the prepared CA has fast water transport channels that can quickly transport water to the top photothermal layer.

[0057] Example 2

[0058] Preparation of CA-CNT solar interfacial evaporator by carbon deposition method:

[0059] (1) preparing a carbon nanotube suspension: weighing 0.3 g of carbon nanotubes and an equal amount of sodium dodecyl sulfate and dissolving them in 100 mL of deionized water, and then ultrasonically dispersing the carbon nanotubes for 1 h to uniformly disperse the carbon nanotubes, thereby preparing a 1 mg / mL carbon nanotube suspension;

[0060] (2) 30 mL of the carbon nanotube suspension in step (1) was measured and placed in a crystallization dish, and the upper surface of the chitosan aerogel prepared in Example 1 was immersed in the carbon nanotube suspension. After the chitosan aerogel completely absorbed the water of the carbon nanotube suspension, the carbon nanotubes were deposited on the upper surface, and then freeze-dried for 24 h to obtain a CA-CNT solar interface evaporator, which was named CA-3.

[0061] Example 3

[0062] The preparation steps were similar to those in Example 2, except that the amount of carbon nanotubes and sodium dodecyl sulfate added was changed to 0.5 g, and other conditions remained unchanged. The prepared CA-CNT solar interface evaporator was named CA-5.

[0063] Example 4

[0064] The preparation steps were similar to those of Example 2, except that the amount of carbon nanotubes and sodium dodecyl sulfate added was changed to 0.7 g, and other conditions remained unchanged. The prepared CA-CNT solar interface evaporator was named CA-7.

[0065] Example 5

[0066] The preparation steps were similar to those in Example 2, except that the amount of carbon nanotubes and sodium dodecyl sulfate added was changed to 1 g, and other conditions remained unchanged. The prepared CA-CNT solar interface evaporator was named CA-10.

[0067] Figure 4 The scanning electron microscope images of the CNT photothermal layer of the solar interface evaporator prepared in Example 1, Example 3, and Example 5 are shown in FIG. Figure 4 It can be seen that the carbon nanotubes deposited on the top of CA-1 are loose, the carbon nanotubes deposited on the top of CA-5 are very dense, and the density of the deposition of CA-10 and CA-5 is not much different, indicating that the deposition amount of CA-5 has reached saturation.

[0068] Comparative Example 1

[0069] The preparation steps were similar to those in Example 2, except that the amount of carbon nanotubes and sodium dodecyl sulfate added was changed to 0.1 g, and other conditions remained unchanged. The prepared CA-CNT solar interface evaporator was named CA-1.

[0070] Test Example 1

[0071] The axial and radial thermal conductivity of the CA prepared in Example 1 were tested and compared with the foam, and the results are shown in the following table. As shown in Table 1, the axial and radial thermal conductivity of the CA prepared in Example 1 are not much different from those of the foam with good thermal insulation performance, indicating that the prepared CA has good thermal management capabilities and can concentrate heat at the evaporation interface.

[0072] Table 1 Comparison of thermal conductivity of CA and foam prepared in Example 1

[0073]

[0074] Test Example 2

[0075] CA and CA-5 prepared in Example 1 were subjected to UV-visible-near infrared absorption spectroscopy test, and the results are shown in Figure 5 . Tests show that the average light absorption rate of CA prepared in Example 1 is 38.89% in the entire solar spectrum, while after the carbon nanotubes are deposited on CA-5, the light absorption rate of the solar interface evaporator is greater than 90% in the entire solar spectrum, and the absorption rate is greater than 95% in the wavelength range of 200 to 1500nm where the sunlight energy is the strongest. This is attributed to the black carbon nanotube photothermal layer on its surface, which can not only efficiently absorb the incident light, but also reduce the reflection of the incident light by multiple scattering.

[0076] Test Example 3

[0077] This test example is a photoevaporation performance test, and the test process is as follows:

[0078] CA, CA-1, CA-3, CA-5, CA-7 and CA-10 were selected as the test group. 80 mL of deionized water was added to a 100 mL beaker with an inner diameter of 45 mm. The samples of the above test groups were cut into pieces with a size of 2 × 2 × 1.8 cm. 3 The cube was then fixed in a beaker with polyethylene foam of 45 mm in diameter, and the bottom of the evaporator was ensured to be in contact with the water. The beaker was placed on an analytical balance with an accuracy of 0.0001 g. A Fresnel lens with a focal length of 5 cm was used to focus the xenon lamp light (equipped with an AM 1.5G filter) and the distance between the top of the evaporator and the xenon lamp was adjusted so that the light intensity of the circular light spot irradiating the top of the evaporator was 1 sun intensity (1 kW m -2), the analytical balance was connected to a laptop computer, the mass of water lost by evaporation was recorded at regular intervals, and a handheld infrared thermal imager was used to record the temperature of the evaporator and the water body. A beaker without the test group product was prepared as a control group to measure the natural evaporation process of water. The results are shown in Table 2. With the increase in the amount of carbon nanotubes added, the light absorption rate, evaporation rate and evaporation efficiency of the samples all showed an upward trend. When the concentration of carbon nanotubes reached more than 3 mg / mL, the evaporation rate of the samples was 1.3 kg m -2 h -1 The evaporation efficiency is above 96%, and the evaporation rate and evaporation efficiency are at a relatively high level.

[0079] Table 2 Comparison of photoevaporation performance test

[0080]

[0081] Test Example 4

[0082] This test example is used to examine the relationship between temperature and time at the evaporation interface. CA and CA-5 were selected as the test group, and pure water was used as the control group. The results are shown in Figure 6 Under a certain light intensity, the temperature at the evaporation interface of the CA-5 evaporator was significantly higher than that at the evaporation interface of pure water and CA. The evaporation interface temperature of CA-5 rose rapidly from room temperature to 35°C in the first 10 minutes, and stabilized at around 44°C after 1 hour of illumination.

[0083] Test Example 5

[0084] This test example is used to test the salt resistance of the solar interface evaporator. CA-5 was selected for the test. 80 mL of 3.5 wt% salt water was added to a 100 mL beaker with an inner diameter of 45 mm. CA-5 was cut into pieces with a size of 2 × 2 × 1.8 cm. 3 The cube was then fixed in a beaker with polyethylene foam of 45 mm in diameter, and the bottom of the evaporator was ensured to be in contact with the brine. The beaker was placed on an analytical balance with an accuracy of 0.0001 g. A Fresnel lens with a focal length of 5 cm was used to focus the xenon lamp light (equipped with an AM 1.5G filter) and the distance between the top of the evaporator and the xenon lamp was adjusted so that the light intensity of the circular light spot irradiating the top of the evaporator was 1 sun intensity (1 kW m -2 ), taking photos of the upper surface of the CA-5 solar interface evaporator every 2 hours. Figure 7The following are photos of the evaporation interface of the CA-5 evaporator after 8 hours of illumination and 4 hours of stopping illumination in salt water. It can be seen that after 4 hours of illumination, obvious salt precipitation began to occur at the evaporation interface of the CA-5 evaporator. After 2 hours of illumination, the salt precipitation gradually increased. After 8 hours of illumination, large particles of salt precipitation can be seen on the evaporation interface. After 2 hours of stopping illumination, the salt began to gradually dissolve. After 4 hours of stopping illumination, all the salt at the evaporation interface dissolved, indicating that the CA-CNT solar interface evaporator has excellent salt tolerance.

[0085] Test Example 6

[0086] This test case is used to test the actual seawater desalination performance of the CA-CNT solar interface evaporator. CA-5 was selected for testing. Figure 8 The schematic diagram of the condensate collection device is shown in Figure 1. The solar interface evaporator 5 is placed in a crystallization dish 4 filled with real seawater (taken from the Bohai Sea). The outer wall of the condensate collection device is made of colorless and transparent organic glass. Under the irradiation of sunlight 1, the high-temperature steam 6 generated on the surface of the evaporator condenses on the inner wall with a lower temperature to form water droplets 7, which then slide down the slope 2 to the water tank 3 at the bottom to be collected. The device is placed outdoors under natural light conditions to conduct actual seawater desalination performance tests. The results are shown in Figure 11. Fig. 9 and 10 . Fig. 9 The curves of evaporation rate, light intensity and temperature at the evaporation interface from 9:00 to 16:00 are as follows. It can be seen that the evaporation rate of the evaporator and the temperature at the evaporation interface change with the light intensity. At 13:00, the light intensity reaches the maximum value of 970 W m -2 At this time, the evaporation rate and the temperature at the evaporation interface are 1.59 kg m -2 h -1 and 47.1℃, both of which are slightly higher than the -2 ) is the value measured indoors under the condition of sunlight. This may be because the outdoor ambient temperature is higher than the indoor temperature. The increase in water temperature will reduce the evaporation enthalpy, thereby accelerating the evaporation rate. A total of 55g of condensed water was collected in one day of illumination (8h). By calculation, the condensed water yield is 7.15kg m -2 d -1 , can meet the daily drinking water needs of three people.

[0087] Fig.10 The ion concentration changes before and after the desalination of real seawater. It can be seen that the ion concentration in the desalinated condensed water has decreased by 2 to 3 orders of magnitude and is far below the World Health Organization's drinking water quality standards. In summary, the CA-CNT solar interface evaporator has good practical application prospects in the field of seawater desalination.

[0088] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A solar interface evaporator, characterized in that: The solar interface evaporator is composed of chitosan aerogel with a vertically arranged pore structure as a lower water supply layer and carbon nanotubes as an upper photothermal layer; The solar interface evaporator is prepared according to the following steps: The suspension of carbon nanotubes is deposited on a chitosan aerogel having a vertically arranged pore structure, wherein the chitosan aerogel having a vertically arranged pore structure is prepared by the following steps: The chitosan is dissolved in an acetic acid aqueous solution to obtain a chitosan slurry, and then the chitosan slurry is injected into an axial freezing device with an axial temperature gradient to freeze-form, and then the frozen chitosan slurry is freeze-dried and vacuum-dried in sequence to obtain; The axial temperature gradient of the freeze molding is -196°C to -10°C; the freeze molding time is 15 to 30 minutes; In the raw materials of the chitosan aerogel, the mass ratio of chitosan, acetic acid and water is 1:2-3:6-8.

2. The solar interface evaporator according to claim 1, characterized in that: The thickness of the water supply layer is 2 to 2.5 cm.

3. The solar interface evaporator according to claim 1, characterized in that: The thickness of the photothermal layer is 20-40 μm.

4. A method for preparing a solar interface evaporator according to any one of claims 1 to 3, characterized in that: The steps include: The suspension of carbon nanotubes is deposited on a chitosan aerogel having a vertically arranged pore structure, wherein the chitosan aerogel having a vertically arranged pore structure is prepared by the following steps: The chitosan is dissolved in an acetic acid aqueous solution to obtain a chitosan slurry, and then the chitosan slurry is injected into an axial freezing device with an axial temperature gradient to freeze-form, and then the frozen chitosan slurry is freeze-dried and vacuum-dried in sequence to obtain; The axial temperature gradient of the freeze molding is -196°C to -10°C; the freeze molding time is 15 to 30 minutes; In the raw materials of the chitosan aerogel, the mass ratio of chitosan, acetic acid and water is 1:2-3:6-8.

5. The preparation method according to claim 4, characterized in that: The carbon nanotube suspension is prepared by mixing carbon nanotubes, a dispersant and water; the concentration of the carbon nanotube suspension is 3-10 mg / mL.

6. The preparation method according to claim 4, characterized in that: The freeze drying temperature is -50 to -20°C; the freeze drying time is 10 to 100 hours; and the freeze drying pressure is 1 to 100 Pa.

7. The preparation method according to claim 4, characterized in that: The vacuum drying temperature is 60-80° C.; the vacuum drying time is 6-12 hours; and the vacuum drying pressure is 100-1000 Pa.

8. The preparation method according to claim 4, characterized in that: The mass ratio of the carbon nanotubes to the dispersant is 1:1-2.

9. The preparation method according to claim 4, characterized in that: The dispersant includes one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate or sodium dodecyl sulfonate.

10. Use of the solar interface evaporator according to any one of claims 1 to 3 in solar seawater desalination.