A lunar dust protection coating on the surface of a solar cell and its preparation method and dust protection efficiency evaluation method

By forming a lunar dust protective coating containing fluorine silica sol and polydimethylsiloxane on the surface of the solar cell, the problem of reduced power generation efficiency caused by lunar dust deposition on the solar cell array in the lunar environment has been solved, and efficient lunar power generation has been achieved. Dust protection and accurate dust protection efficiency evaluation, suitable for long-term lunar surface missions.

CN116656155BActive Publication Date: 2024-10-18LANZHOU INST OF PHYSICS CHINESE ACADEMY OF SPACE TECH

Patent Information

Application Number
CN202310579295.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-10-18
Estimated Expiration
2043-05-22

AI Technical Summary

Technical Problem

During the lunar exploration mission, the power generation efficiency of the solar cell array was reduced due to lunar dust deposition. Existing technology cannot effectively protect lunar dust in the lunar environment without external energy supply, and there is a lack of effective dust prevention efficiency evaluation methods.

Method used

A layered lunar dust protective coating and adhesion layer are used. The coating is made of materials such as fluorine-containing silica sol and polydimethylsiloxane. A protective layer is formed on the surface of the solar cell through dipping and pulling methods and provides protection against Dust efficiency evaluation method, using vacuum system and uniform dust spreading device to conduct experiments.

Benefits of technology

The lunar dust protection efficiency of solar cells is improved, the service life is extended, the cost is saved, and high light transmittance and high temperature and ultraviolet radiation resistance are achieved, while the dust protection efficiency is accurately evaluated.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116656155B_ABST
    Figure CN116656155B_ABST
Patent Text Reader

Abstract

The present invention provides a lunar dust protection coating on the surface of a solar cell, a preparation method thereof, and a dust prevention efficiency evaluation method, which relate to the field of aerospace. The lunar dust protection coating comprises a lunar dust protection layer and an adhesion layer which are stacked, wherein: the raw materials of the lunar dust protection layer comprise fluorine-containing silica sol and a solvent; the raw materials of the adhesion layer comprise polydimethylsiloxane, a curing agent, and a solvent. The lunar dust protection coating can realize lunar dust protection for solar cells in the lunar environment, so that lunar dust will not be deposited on the surface of solar cells for a long time, causing solar cells to overheat, shielding the light absorption rate of solar cells, and reducing power generation efficiency. The lunar dust protection coating has a strong bonding force with the solar cell substrate, and has good adaptability to the lunar surface environment, can be used in orbit for a long time, has a long service life, and greatly saves costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of aerospace technology, and in particular to a lunar dust protection coating on the surface of a solar cell, a preparation method thereof, and a dust protection efficiency evaluation method thereof. Background Art

[0002] In lunar exploration missions, using solar arrays to generate electricity is the main source of power on orbit. In actual lunar exploration missions, lunar dust splashed by engine plumes is the largest source of pollution on the surface of solar arrays. When lunar dust is deposited on the surface of solar cells, it will prevent sunlight from entering the solar cells and cause the solar cell arrays to overheat, resulting in a serious reduction in power generation efficiency. After lunar dust was deposited on the solar cells on the lunar rovers and spacecraft of the Apollo mission, the surface temperature rose to 82°C, far exceeding its safe operating temperature range.

[0003] Regarding lunar dust protection on the surface of solar cells, CN 111471995 A realizes lunar dust protection coating on the surface of aluminum substrate by chemical etching, but the coating is not transparent, and there is a great difference between the lunar dust protection of metal substrate and solar cell surface substrate. In addition, the chemical etching method cannot be applied to large-area solar cell substrates; CN113731772 A adopts sol-gel method to prepare a self-cleaning anti-reflection film for lunar dust protection, and the solution is prepared by mixing silica sol with silica dispersion, and the solution is spin-coated on the surface of solar cells, but the dust protection efficiency is not tested, the particle size of lunar dust particles is much smaller than the diameter of water droplets, a single contact angle cannot reflect the dust protection performance, and the adaptability to space environment is not explained; CN 203300671 U discloses a solar cell lunar dust protection device, but the device needs on-orbit energy supply to achieve lunar dust protection, and does not belong to passive protection technology; CN 112885504 A discloses a lunar dust protection film with a regular inverted pyramid structure, whose substrate is aluminum metal. The protective film has conductive opaque properties and cannot be applied to solar cells.

[0004] Therefore, it is necessary to design a lunar dust protection coating for the surface of solar cells to protect the solar cells from the impact of lunar dust deposition without consuming energy on the lunar surface, thereby ensuring normal energy supply for lunar activities.

[0005] In addition, in previous studies, the deposition rate and mass of lunar dust splashed by the plume during the soft landing process could not be quantitatively calculated, making it impossible to test the lunar dust protection efficiency experiment based on actual on-orbit data. Therefore, proposing a new method for evaluating the dust protection efficiency of lunar dust protection coatings on solar cell surfaces has become a technical problem that needs to be solved urgently in this field. Summary of the invention

[0006] Therefore, the main purpose of the present invention is to provide a lunar dust protection coating for the surface of a solar cell and a preparation method and a dust protection efficiency evaluation method thereof, which can achieve lunar dust protection under the condition of no external energy supply in the lunar environment, so that the solar cell can work normally in orbit and ensure the energy supply during long-term lunar activities in subsequent manned lunar exploration and long-term lunar residence missions.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] In a first aspect, the present invention provides a lunar dust protection coating on the surface of a solar cell, comprising a lunar dust protection layer and an adhesion layer stacked in layers, wherein:

[0009] The raw materials of the lunar dust protective layer include fluorine-containing silica sol and solvent;

[0010] The raw materials of the adhesive layer include polydimethylsiloxane, a curing agent and a solvent.

[0011] Furthermore, in the raw materials of the adhesive layer, the mass ratio of the polydimethylsiloxane to the curing agent is 1:10-12, the sum of the masses of the polydimethylsiloxane and the curing agent accounts for 4%-6% of the total mass of the raw materials of the adhesive layer, and the solvent is ethane.

[0012] Preferably, in the raw materials of the adhesive layer, the mass ratio of the polydimethylsiloxane to the curing agent is 1:12, the sum of the masses of the polydimethylsiloxane and the curing agent accounts for 5% of the total mass of the raw materials of the adhesive layer, and the solvent is ethane.

[0013] Furthermore, in the raw materials of the lunar dust protective layer, the mass percentage of the fluorine-containing silica sol is 0.4-0.6%, and the solvent is a mixture of ethanol, ethyl acetate and deionized water, and the mass ratio is 96-98:0.1-0.5:2.0-3.0.

[0014] Preferably, in the raw materials of the lunar dust protective layer, the mass percentage of the fluorine-containing silica sol is 0.4%, and the solvent is a mixture of ethanol, ethyl acetate and deionized water, and the mass ratio is 97.5:0.1:2.0.

[0015] Furthermore, the fluorine-containing silica sol is obtained by hydrolysis and polycondensation of methyltrimethoxysilane and tridecafluorooctyltrimethoxysilane.

[0016] Furthermore, the lunar dust protective coating has a thickness of 250 to 350 nm and a roughness of 30 to 60 nm.

[0017] Preferably, the lunar dust protective coating has a thickness of 300 nm and a roughness of 30 nm.

[0018] In a second aspect, the present invention provides a method for preparing the lunar dust protective coating on the surface of a solar cell, comprising the following steps:

[0019] (1) Surface pretreatment of solar cells: The surface of the solar cell is sequentially wiped with alcohol, cleaned with deionized water, and treated with oxygen plasma, and then placed in a vacuum system to stand;

[0020] (2) Preparation of the adhesive layer by immersion and pulling method: immerse the solar cell treated in step (1) in the prepared adhesive layer raw material solution, pull it upward to form an adhesive layer on the surface of the solar cell, and then place it in a vacuum system and let it stand;

[0021] (3) Preparation of lunar dust protection layer by immersion and pulling method: Immerse the solar cell treated in step (2) in the prepared lunar dust protection layer raw material solution, pull it upward to form a lunar dust protection layer on the surface of the adhesion layer, and then put it into a vacuum system to dry.

[0022] Furthermore, in step (1), the number of alcohol wiping is 3 to 6 times, the number of deionized water washing is 3 to 6 times, the time of oxygen plasma treatment is 2 to 3 minutes, and the pressure of the vacuum system is 10 -4 Pa, standing time is 1 to 2 hours;

[0023] Preferably, in step (1), the number of alcohol wiping is 4 times, the number of deionized water washing is 4 times, the oxygen plasma treatment time is 2 minutes, and the pressure of the vacuum system is 10 -4 Pa, the standing time is 2h.

[0024] Furthermore, in step (2), the pulling speed is 10-15 mm / min, the pulling times are 2-3 times, the vacuum system temperature is 50-70°C, the pressure is 10 -4 Pa, standing time is 40 to 60 minutes;

[0025] Preferably, in step (2), the pulling speed is 10 mm / min, the pulling times are 2 times, the vacuum system temperature is 70°C, the pressure is 10 -4 Pa, the standing time is 40min.

[0026] Furthermore, in step (3), the pulling speed is 10-15 mm / min, the pulling times are 2-5 times; the vacuum system temperature is 30-50°C, the pressure is 10 -4 Pa, drying time is 10 to 15 hours.

[0027] Preferably, in step (3), the pulling speed is 10 mm / min, the pulling times are 2 times, the vacuum system temperature is 30°C, the pressure is 10 -4Pa, drying time is 10h.

[0028] In a third aspect, the present invention provides a method for evaluating the dustproof efficiency of a lunar dust protective coating on the surface of a solar cell. The experiment is carried out in a vacuum system equipped with a lunar dust uniform dust sprinkling device. During the experiment, the temperature of the vacuum system is maintained at 30-35° C. The dustproof efficiency evaluation method comprises the following steps:

[0029] 1) Place a certain mass of lunar dust into the lunar dust carrying plate of the uniform dust sprinkling device;

[0030] 2) Place the sample coated with the lunar dust protective coating directly under the lunar dust carrier plate, and pump the system to 10 -4 Pa vacuum;

[0031] 3) Turn on the dust sprinkling device and sprinkle the lunar dust evenly on the sample surface;

[0032] 4) Divide the sample surface into 13 sub-areas, numbered 1 to 13;

[0033] 5) Use a camera to photograph the surface of the protective coating sprinkled with lunar dust in the vacuum system. After judging that the lunar dust is evenly deposited and covers the surface of the sample, continue the experiment. If it is judged that the lunar dust is not evenly deposited or does not cover the sample, replace the sample and repeat steps 1) to 3) until the lunar dust is evenly deposited.

[0034] 6) Centrifuge the sample;

[0035] 7) After centrifugal rotation, the sample is turned over, kept in place, and a picture of the lunar dust residue on the sample surface is taken;

[0036] 8) If it is determined that the moon dust residue on the sample surface does not change after the flipping, and the number of moon dust residues in a single sub-area does not change with the flipping, the dust prevention efficiency analysis is performed on the moon dust residue images;

[0037] 9) Perform threshold determination and screening on the areas not covered and covered by lunar dust in different sub-regions to determine the lunar dust covered areas in different sub-regions;

[0038] 10) According to Calculate the lunar dust protection efficiency η of the sample surface, where represents the number of pixels occupied by lunar dust in sub-areas 1 to 13 after the experiment, N1 to N 13 Indicates the total number of pixels in sub-regions 1 to 13.

[0039] Furthermore, in step 6), the speed of centrifugal rotation is 1300-1500 r / min, the duration of a single rotation is 10-20 s, and the number of rotations is 2-4 times; in step 7), the flipping angle is 45°-60°, and it is maintained for 1-3 minutes after flipping.

[0040] Preferably, in step 6), the speed of centrifugal rotation is 1300-1500 r / min, the single rotation time is 10 s, and the number of rotations is 3 times; in step 7), the flipping angle is 45°, and it is kept for 1 minute after flipping.

[0041] Furthermore, in step 5), the basis for judging whether the lunar dust is uniformly deposited is that the number of lunar dust particles in the 13 sub-regions on the sample surface differs from each other by less than 1%; the basis for judging whether the lunar dust covers the entire sample surface is that the lunar dust particles in a single sub-region occupy 100% of the sub-region area.

[0042] The technical solution of the present invention has the following advantages:

[0043] 1. The lunar dust protection coating on the surface of solar cells provided by the present invention can realize lunar dust protection of solar cells in the lunar environment, and the lunar dust protection efficiency is improved by 66.3% compared with the solar cell without the lunar dust protection coating, so that the lunar dust will not be deposited on the surface of the solar cell for a long time, causing the solar cell to overheat, shield the light absorption rate of the solar cell, and reduce the power generation efficiency. The lunar dust protection coating has a strong bonding force with the solar cell substrate and has good adaptability to the lunar surface environment, can be used in orbit for a long time, has a long service life, and greatly saves costs.

[0044] 2. The moon dust protection coating on the surface of the solar cell provided by the present invention has high light transmittance and will not affect the light receiving efficiency of the solar cell itself, that is, it does not affect the light absorption rate of the solar energy itself while taking into account the moon dust protection effect. The transmittance of visible light, ultraviolet light and infrared light is increased by 2.28%, 0.64% and 3.14% respectively compared with the transmittance without the moon dust protection coating.

[0045] 3. The thickness of the lunar dust protection coating on the surface of the solar cell provided by the present invention is about 300nm, and it has the advantage of light weight; the fluorine-containing silica sol forms 5-10nm fluorine silicon particle aggregates, which are used to construct the micro-nano structure of the lunar dust protection coating, and the roughness is about 30nm, which is much smaller than the average particle size of the lunar dust particles, and can achieve protection of extremely small-size lunar dust particles.

[0046] 4. The lunar dust protective coating on the surface of the solar cell provided by the present invention has good high temperature resistance, and its performance remains unchanged within 300°C; it has good resistance to electrons (30 hours at 30KeV) and ultraviolet radiation (32 hours at 395nm wavelength); and it has good wear resistance.

[0047] 5. The lunar dust protective coating on the surface of solar cells provided by the present invention is a passive protective coating that does not require on-orbit energy supply and is an energy-saving protection method.

[0048] 6. The preparation of the lunar dust protective coating on the surface of the solar cell provided by the present invention adopts the immersion pulling method, which can be used for large-area irregular protective surfaces and has a great supporting effect on subsequent engineering applications.

[0049] 7. The dust-proof efficiency evaluation method of the lunar dust protection coating on the surface of solar cells provided by the present invention can realize the efficiency evaluation of lunar dust particles with an accuracy of up to 1 μm. The dust-proof efficiency obtained by the weighing method does not take into account the fine particles adhering to the surface. Therefore, the new method proposed by the present invention greatly improves the accuracy of dust-proof efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0051] Figure 1 This is a comparison of the surface coated with the lunar dust protective coating and the surface not coated with the lunar dust protective coating;

[0052] Figure 2 The contact angle test results before and after surface treatment, where: (a) is the contact angle of 23.2° before surface treatment, and (b) is the contact angle of 0° after surface treatment;

[0053] Figure 3 The figures are contact angle test results of moon dust protective coatings prepared by different dipping times, wherein: (a) is Example 1, (b) is Example 2, (c) is Example 3, and (d) is Example 4;

[0054] Figure 4 Schematic diagram of surface roughness test of moon dust protective coatings prepared by different dipping times, wherein: (a) is Example 1, (b) is Example 2, and (c) is Example 3;

[0055] Figure 5 It is a schematic diagram of coating thickness test of moon dust protective coating prepared by different dipping times;

[0056] Figure 6 This is a schematic diagram of the sub-area numbering of the dustproof efficiency test samples;

[0057] Figure 7 The dust protection efficiency test diagram of the surface coated with the moon dust protection coating and the surface not coated with the moon dust protection coating, wherein: (a) is the uncoated surface, (b) is the coated surface of Example 2, 1, 3, 7 and 11 represent Figure 5 The corresponding sub-region in . DETAILED DESCRIPTION

[0058] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0059] The solar cell model used in the embodiment is a triple-junction gallium arsenide cell purchased from Tianjin No. 18 Institute. The solar cells used in the experiment are all from the same batch.

[0060] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the art can be used. The raw materials or instruments used are all conventional products that can be obtained commercially, including but not limited to the raw materials or instruments used in the examples of this application.

[0061] Example 1

[0062] This embodiment provides a method for preparing a lunar dust protective coating on the surface of a solar cell, and the specific steps are as follows:

[0063] (1) Surface pretreatment of solar cells: The surface of the solar cell was first wiped with alcohol 4 times, then cleaned with deionized water 4 times, and then treated with oxygen plasma for 2 minutes, and then placed in a vacuum system (10 -4 Pa) and allowed to stand for 2 h;

[0064] (2) Preparation of the adhesive layer by immersion and pulling method: The solar cell treated in step (1) is immersed in the prepared adhesive layer raw material solution, and pulled upward at a speed of 10 mm / min for 2 times to form an adhesive layer on the surface of the solar cell, and then placed in a 70°C vacuum system (10 -4 Pa) and allowed to stand for 40 min;

[0065] (3) Preparation of lunar dust protection layer by immersion and pulling method: The solar cell treated in step (2) is immersed in the prepared lunar dust protection layer raw material solution, and pulled upward at a speed of 10 mm / min, and pulled once to form a lunar dust protection layer on the surface of the adhesive layer, and then placed in a 30°C vacuum system (10 -4 Pa) for 10 h.

[0066] The adhesive layer raw material solution in step (2) is prepared from polydimethylsiloxane, a curing agent and ethane, the mass ratio of polydimethylsiloxane to the curing agent is 1:12, and the sum of the masses of polydimethylsiloxane and the curing agent accounts for 5% of the total mass of the adhesive layer raw material.

[0067] The raw material solution of the lunar dust protective layer in step (3) is prepared from fluorine-containing silica sol and solvent, the mass percentage of fluorine-containing silica sol is 0.4%, and the solvent is a mixture of ethanol, ethyl acetate and deionized water, and the mass ratio is 97.5:0.1:2.0. Among them, the fluorine-containing silica sol is obtained by hydrolysis and polycondensation of methyltrimethoxysilane and tridecafluorooctyltrimethoxysilane, and the specific preparation method is: add 1mL of methyltrimethoxysilane and 1mL of tridecafluorooctyltrimethoxysilane in a container, stir for 30 minutes at room temperature, then add 0.2mL of oxalic acid solution, continue stirring for 30 minutes, let stand for 20 hours, and then drop 7.5mL of ammonia water, and self-condense after aging at room temperature to obtain fluorine-containing silica sol.

[0068] Example 2

[0069] This embodiment provides a method for preparing a lunar dust protective coating on the surface of a solar cell. The specific steps are referred to in Example 1, except that the pulling times in step (3) are 2 times. The prepared protective surface is as follows: Figure 1 As shown in the figure, the uncoated surface means that no protective coating is applied to the solar cell glass sheet, and it is only subjected to plasma surface treatment. By comparing the coated and uncoated surfaces, it can be found that the surface coated with the protective coating has coating reflection under light, and the coating does not affect the transparency of the glass before and after coating, and no obvious blurring effect is found.

[0070] Example 3

[0071] This embodiment provides a method for preparing a lunar dust protective coating on the surface of a solar cell. The specific steps refer to those of Embodiment 1, with the only difference being that the number of pulling times in step (3) is 3.

[0072] Example 4

[0073] This embodiment provides a method for preparing a lunar dust protective coating on the surface of a solar cell. The specific steps refer to those of Embodiment 1, with the only difference being that the number of pulling times in step (3) is 4.

[0074] The surface of the comparative solar cell was first wiped with alcohol 4 times, then cleaned with deionized water 4 times, and then treated with oxygen plasma for 2 minutes, and then placed in a vacuum system (10 -4 Pa) for 2 h.

[0075] like Figure 2 As shown, the contact angles of the sample surface before and after treatment were measured respectively, and it can be concluded that the contact angle of the sample surface after treatment is almost 0°.

[0076] Experimental Example 1 Contact Angle Test

[0077] The lunar dust protective coatings on the solar cell surfaces prepared in Examples 1 to 4 were tested for contact angles. The results are shown in Tables 1 and Figure 3 shown.

[0078] Table 1 Contact angle test results of Examples 1 to 4

[0079]

[0080] Experimental Example 2 Roughness Test

[0081] The lunar dust protective coating on the surface of the solar cell prepared in Examples 1 to 3 was tested for surface roughness. The experimental process was as follows: the prepared protective coating was tested for roughness, and the results of 5 times were averaged to obtain the roughness value. The results are shown in Table 2 and Figure 4 shown.

[0082] Table 2 Roughness test results of Examples 1 to 3

[0083]

[0084] like Figure 4 As shown, with the increase of the number of pull-up coating times, the roughness gradually decreases and the surface micro / nanoscale structure gradually disappears.

[0085] Experimental Example 3 Thickness Test

[0086] The moon dust protective coating on the surface of the solar cell prepared in Examples 1 to 3 was tested for thickness. The experimental process was as follows: a film thickness tester was used to test it, 5 points were selected on the surface, and the film thickness results of the test were averaged. The results are shown in Table 3 and Figure 5 shown.

[0087] Table 3 Thickness test results of Examples 1 to 3

[0088]

[0089] Experimental Example 4: Light transmittance test

[0090] The solar cell surface moon dust protective coating prepared in Examples 1 to 3 was tested for light transmittance on its surface, and the surface treated in the comparative example was used as a control. The experimental process was as follows: the protective film was tested by a light transmittance tester, and 5 points were selected on a single protective surface to take the average value. The results are shown in Table 4.

[0091] Table 4 Transmittance test results of Examples 1 to 3

[0092]

[0093] As shown in Table 4, Example 2 has the best light transmission effect, and the transmittance is increased by 2.28% (ultraviolet light), 0.64% (visible light), and 3.14% (infrared light) compared with the uncoated surface (comparative example).

[0094] Experimental Example 5 Temperature Resistance Test

[0095] The moon dust protective coating on the surface of the solar cell prepared in Example 2 was tested for temperature resistance. The experimental process was as follows: the moon dust protective coating sample was placed in a vacuum system. After the system was evacuated, the temperature was set to 50°C, 100°C, 150°C, 200°C, 250°C and 300°C respectively. The target temperature was maintained for 30 hours. The contact angle of the sample surface was measured immediately after the sample was taken out. The results are shown in Table 5.

[0096] Table 5 Example 2 Temperature resistance test results

[0097]

[0098] Experimental Example 6 Ultraviolet radiation resistance test

[0099] The moon dust protective coating on the surface of the solar cell prepared in Example 2 was tested for ultraviolet radiation resistance. The experimental process was as follows: the moon dust protective coating sample was placed in a vacuum system, and the sample was placed 10 cm directly below the vacuum ultraviolet lamp. After the system was evacuated, the vacuum ultraviolet lamp was turned on, and the wavelength was 395 nm. The ultraviolet lamp irradiation time was 32 hours. After the irradiation was completed, the sample was taken out and the contact angle was measured immediately. The results are shown in Table 6.

[0100] Table 6 UV radiation resistance test results of Example 2

[0101] Group Adhesion layer dipping times Protective layer impregnation times UV duration Contact angle Example 2 2 2 32h 147.25°

[0102] Experimental Example 7: Electron Radiation Resistance Test

[0103] The lunar dust protective coating on the surface of the solar cell prepared in Example 2 was tested for resistance to electron radiation. The experimental process was as follows: the lunar dust protective coating sample was placed in a vacuum system, and the sample was placed 15 cm directly below the electron gun. After the system was evacuated, the electron gun energy was set to 30 KeV, and the electron gun was turned on for 30 hours of irradiation. After the electron radiation was completed, the sample was taken out and the contact angle was immediately measured. The results are shown in Table 7.

[0104] Table 7 Test results of electronic radiation resistance of Example 2

[0105] Group Adhesion layer dipping times Protective layer impregnation times Radiation duration Contact angle Example 2 2 2 30h 145.14°

[0106] Experimental Example 8 Wear Resistance Test

[0107] The lunar dust protective coating on the surface of the solar cell prepared in Example 2 was subjected to a wear resistance test, and the experimental process was as follows: peeling with an adhesive tape, and measuring the contact angle of the protective coating after 20 peelings. The results are shown in Table 8.

[0108] Table 8 Wear resistance test results of Example 2

[0109] Group Adhesion layer dipping times Protective layer impregnation times Contact angle Example 2 2 2 150.40°

[0110] Experimental Example 9 Dust protection efficiency test

[0111] The moon dust protection coating on the surface of the solar cell prepared in Example 2 was taken and its protection efficiency was tested. The experiment was carried out in a vacuum system equipped with a moon dust uniform dust sprinkling device. During the experiment, the temperature of the vacuum system was maintained at 30° C. The experimental process was as follows:

[0112] 1) Weigh 10g of lunar dust and put it into the lunar dust carrying plate of the uniform dust sprinkling device;

[0113] 2) Place the sample prepared in Example 2 5 cm below the lunar dust carrier and pump the system to 10 -4 Pa vacuum;

[0114] 3) Turn on the dust sprinkling device and sprinkle the lunar dust evenly on the sample surface;

[0115] 4) If Figure 6 As shown, the sample surface is evenly divided into 13 sub-areas, numbered 1 to 13;

[0116] 5) Using a camera to photograph the surface of the protective coating sprinkled with lunar dust in the vacuum system, and continuing the experiment after judging that the lunar dust is evenly deposited and covers the sample surface, if it is judged that the lunar dust is unevenly deposited or does not cover the sample, then changing the sample and repeating steps 1) to 3) until the lunar dust is evenly deposited, wherein the basis for judging the uniform deposition of lunar dust is that the number of lunar dust particles on the 13 sub-regions of the sample surface differs from each other by less than 1%, and the basis for judging that the lunar dust covers the sample surface is that the lunar dust particles on a single sub-region occupy 100% of the sub-region area;

[0117] 6) The sample was centrifuged at a speed of 1300-1500 r / min, with a single rotation time of 10 s and a rotation number of 3 times;

[0118] 7) After centrifugal rotation, flip the sample 45°, keep it for 1 minute, and then take a picture of the lunar dust residue on the sample surface;

[0119] 8) If it is determined that the moon dust residue on the sample surface does not change after the flipping, and the number of moon dust residues in a single sub-area does not change with the flipping, the dust prevention efficiency analysis is performed on the moon dust residue images;

[0120] 9) Perform threshold determination and screening on the areas not covered and covered by lunar dust in different sub-regions to determine the lunar dust covered areas in different sub-regions;

[0121] 10) According to Calculate the lunar dust protection efficiency η of the sample surface, where represents the number of pixels occupied by lunar dust in sub-areas 1 to 13 after the experiment, N1 to N 13 Indicates the total number of pixels in sub-regions 1 to 13.

[0122] The results are shown in Table 9 and Figure 7 shown.

[0123] Table 9 Example 2 Moon dust protection efficiency test results

[0124] Group Adhesion layer dipping times Protective layer impregnation times Moon dust protection efficiency Example 2 2 2 66.3%

[0125] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A lunar dust protective coating on the surface of a solar cell, characterized in that: It comprises a lunar dust protection layer and an adhesion layer which are stacked, wherein: The raw materials of the lunar dust protective layer include fluorine-containing silica sol and solvent; The raw materials of the adhesive layer include polydimethylsiloxane, a curing agent and a solvent. In the raw materials of the adhesive layer, the mass ratio of the polydimethylsiloxane to the curing agent is 1:10-12, the sum of the mass of the polydimethylsiloxane and the curing agent accounts for 4%-6% of the total mass of the raw materials of the adhesive layer, and the solvent is ethane; In the raw materials of the lunar dust protective layer, the mass percentage of the fluorine-containing silica sol is 0.4-0.6%, and the solvent is a mixture of ethanol, ethyl acetate and deionized water, and the mass ratio is 96-98:0.1-0.5:2.0-3.0; The fluorine-containing silica sol is obtained by hydrolysis and polycondensation of methyltrimethoxysilane and tridecafluorooctyltrimethoxysilane.

2. The solar cell surface lunar dust protective coating according to claim 1, characterized in that: The thickness of the lunar dust protective coating is 250-350 nm, and the roughness is 30-60 nm.

3. The method for preparing the lunar dust protective coating on the surface of a solar cell according to claim 1 or 2, characterized in that: The following steps are involved: (1) Surface pretreatment of solar cells: The surface of the solar cell is sequentially wiped with alcohol, cleaned with deionized water, and treated with oxygen plasma, and then placed in a vacuum system to stand; (2) Preparation of the adhesive layer by immersion and pulling method: immerse the solar cell treated in step (1) in the prepared adhesive layer raw material solution, pull it upward to form an adhesive layer on the surface of the solar cell, and then place it in a vacuum system and let it stand; (3) Preparation of lunar dust protection layer by immersion and pulling method: Immerse the solar cell treated in step (2) in the prepared lunar dust protection layer raw material solution, pull it upward to form a lunar dust protection layer on the surface of the adhesion layer, and then put it into a vacuum system to dry.

4. The method for preparing the lunar dust protective coating on the surface of a solar cell according to claim 3, characterized in that: In step (1), the number of alcohol wiping is 3 to 6 times, the number of deionized water washing is 3 to 6 times, the time of oxygen plasma treatment is 2 to 3 minutes, and the pressure of the vacuum system is 10 -4 Pa, standing time is 1 to 2 hours; In step (2), the pulling speed is 10-15 mm / min, the pulling times are 2-3 times; the vacuum system temperature is 50-70°C, the pressure is 10 -4 Pa, standing time is 40 to 60 minutes; In step (3), the pulling speed is 10-15 mm / min, the pulling times are 2-5 times; the vacuum system temperature is 30-50°C, the pressure is 10 -4 Pa, drying time is 10 to 15 hours.

Citation Information

Patent Citations

  • Lunar dust protection conductive film with micro-nano structure and preparation method thereof

    CN112885504A

  • Self-cleaning anti-reflection film for lunar dust protection and preparation method thereof

    CN113731772A

  • Lunar dust prevention device for solar cells

    CN203300671U

  • Preparation method of super hydrophobic coating based on super hydrophobic silica and resin

    CN103587185A

Cited By

  • Micro-structure controllable dust removing surface and preparation method thereof

    CN121136598A

  • Lunar dust protection surface ground intelligent efficiency evaluation system and method

    CN122524678A

  • A lunar dust protection surface ground intelligent efficiency evaluation system and method

    CN122524678B