A composite graphite negative electrode material and its preparation method and application
By adopting catalytic graphitization process and nano-silicon embedding process in the negative electrode material of lithium-ion battery, combining hard carbon coating and zwitterionic polymer coating and carbon nanotubes, the volume expansion problem caused by lithium embedded in silicon-based materials is solved. Improve rate performance and energy density, achieving high stability and fast charging performance of the electrode.
Patent Information
- Application Number
- CN202311157389.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-09-07
AI Technical Summary
The prior art fails to effectively alleviate the volume expansion and rapid performance decay caused by lithium-ion battery anode materials due to lithium embedded in silicon-based materials.
Using composite graphite negative electrode material, graphitized particles are prepared through catalytic graphitization process, and nanosilicon particles are embedded inside the graphite particles to form silicon-based particles with hard carbon coating layer, combining zwitterionic polymer coating layer and carbon nanometers tube, forming a porous structure to improve ionic conductivity and electrical conductivity.
It significantly improves the transmission path of lithium ions, alleviates the volume expansion of silicon particles when embedded in lithium, improves the rate performance and energy density of the material, and ensures the stability of the electrode structure and high fast charging performance.
Smart Images

Figure CN117117136B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and specifically relates to a composite graphite negative electrode material and a preparation method and application thereof. Background Art
[0002] With the continuous development of the new energy vehicle industry, the power battery industry has continued to progress, and the requirements for battery fast charging performance and energy density have continued to increase. In 2021, the power battery industry showed that the increase in new energy vehicle sales has driven the continued growth in demand for power batteries, the competition among power battery companies has become fierce, and companies have continued to make efforts in capacity layout and joint ventures. The coating process is an effective means to improve the rate performance of materials. Resin materials can form a hard carbon layer after carbonization as a coating material. Hard carbon is isotropic and has a larger interlayer spacing than graphite. During the charging process, lithium ions diffuse quickly and have good rate performance. Ionic smart polymer materials as coating materials are beneficial to improving ionic conductivity. The ionic structure on their chain segments can effectively promote Li + The granulation process is also an important means to improve the rate performance of materials. Compared with single-granular products, the granulated products greatly improve the overall isotropy of the materials, thereby improving the rate performance.
[0003] In the prior art, patent CN115692638A prepares nano-silicon composite negative electrode materials by combining silicon, carbon and graphite; patent CN113206249A discloses coating amorphous carbon, carbon nanomaterials and solid electrolytes (in two distribution forms) on the surface of silicon oxide particles; patent CN113745489A discloses coating a layer of flexible polymer material on silicon carbon material; although the technical solutions of the above patents can improve the performance of negative electrode materials; however, the above patents only alleviate the volume expansion caused by lithium insertion from the perspective of providing expansion space and improving binding capacity, but fail to maintain close contact between silicon-based material particles. Summary of the invention
[0004] The main purpose of the present invention is to provide a composite graphite negative electrode material and a preparation method and application thereof, so as to overcome the deficiencies of the prior art.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0006] The embodiment of the present invention provides a composite graphite negative electrode material, which includes:
[0007] A plurality of secondary particles, wherein the secondary particles include primary particles and a zwitterionic polymer coating layer that encapsulates the primary particles, the primary particles include graphitized particles having a hard carbon coating layer and silicon-based particles having a hard carbon coating layer, the graphitized particles have a porous structure, and the silicon-based particles include graphite particles with nano-silicon particles distributed on the surface and inside;
[0008] And, the carbon nanotubes are at least connected between a plurality of the secondary particles.
[0009] The embodiment of the present invention also provides a method for preparing a composite graphite negative electrode material, which comprises:
[0010] The coke raw material is subjected to catalytic graphitization treatment by adopting a catalytic graphitization process to obtain graphitized particles;
[0011] The silicon-based particles are obtained by embedding nano-silicon particles into the internal pores and surface of graphite particles using a spheroidization process;
[0012] The graphitized particles, silicon-based particles, and water-soluble resin are added into water and mixed thoroughly, and then dried and carbonized to obtain primary particles; wherein the primary particles include graphitized particles with a hard carbon coating layer and silicon-based particles with a hard carbon coating layer;
[0013] Furthermore, the zwitterionic polymer is coated on the surface of the primary particles by a spray drying process to form a secondary particle structure, and then mixed with carbon nanotubes to obtain a composite graphite negative electrode material.
[0014] The embodiments of the present invention also provide the use of the aforementioned composite graphite negative electrode material or the composite graphite negative electrode material prepared by the aforementioned preparation method in preparing a battery negative electrode sheet or a lithium ion battery.
[0015] The embodiment of the present invention further provides a lithium-ion battery negative electrode sheet, which includes the aforementioned composite graphite negative electrode material or the composite graphite negative electrode material prepared by the aforementioned preparation method.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] (1) The preparation method of the composite graphite negative electrode material provided in the present invention can improve the interface ion conductivity;
[0018] (2) The present invention is beneficial to improving the capacity of the material by introducing silicon, and by compounding nano-silicon particles and graphite particles to provide space and stress to relieve the volume expansion of silicon particles when lithium is inserted, and is beneficial to relieve the rapid performance attenuation caused by the volume expansion of silicon materials due to lithium insertion;
[0019] (3) The present invention introduces zwitterionic polymer as a coating material, which improves ionic conductivity and promotes Li + Transfer from the electrolyte to the surface of the negative electrode material particles, effectively shortening the transmission path of lithium ions, that is, shortening the Li + The distance to the surface of the active material and then to the reaction center improves the rate performance; the ionic bonds on the molecular chain segments of the zwitterionic polymer can form a "smart switch" structure, which can maintain effective connections between particles to achieve the purpose of alleviating the rapid performance attenuation of silicon particles caused by volume expansion during lithium insertion;
[0020] (4) The structure of the composite graphite negative electrode material in the present invention can effectively shorten the transmission path of lithium ions, that is, shorten the Li + The distance to the surface of the active material and then to the reaction center, and the "smart switch" structure and carbon nanotubes are beneficial to maintaining the stability and integrity of the electrode structure, and alleviating the rapid performance decay caused by the volume expansion of silicon particles when lithium is embedded. It has the characteristics of good isotropy, fast ion transfer rate, multiple transfer channels, and stable electrode structure. The lithium-ion battery electrode prepared by it has the characteristics of high energy density and good fast charging performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 It is a preparation process and structural schematic diagram of a composite graphite negative electrode material with high capacity and high rate performance in a typical embodiment of the present invention;
[0023] Figure 2 In a typical embodiment of the present invention, Li + Model diagram of the transfer from the surface of negative electrode material particles to the active center;
[0024] Figure 3 The "intelligent switch" structure between the granulated particles in a typical embodiment of the present invention and its Li + Schematic diagram of the action during the deintercalation process;
[0025] Figure 4 The "intelligent switch" structure between particles in the granulated product in a typical embodiment of the present invention and its Li + Schematic diagram of the action during the deintercalation process;
[0026] Figure 5This is a structural diagram of a zwitterionic smart polymer PDMAPS in a typical embodiment of the present invention;
[0027] Figure 6 This is an infrared image of zwitterionic smart polymer PDMAPS in a typical embodiment of the present invention;
[0028] Figure 7 is a SEM morphology of a graphitized particle product in a typical embodiment of the present invention;
[0029] Figure 8 is a SEM morphology image of silicon-based particles in a typical embodiment of the present invention;
[0030] Figure 9a and Figure 9b is an EDS spectrum of a cross section of a silicon-based particle in a typical embodiment of the present invention;
[0031] Fig.10 is a SEM morphology of carbon nanotubes in a typical embodiment of the present invention;
[0032] Figure 11-Figure 12 This is a SEM morphology image of a finished composite graphite negative electrode material with high capacity and high rate performance in a typical embodiment of the present invention. DETAILED DESCRIPTION
[0033] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The high-capacity and high-rate composite graphite negative electrode material in the present invention is a granulated product of a silicon-based composite material coated with an ionic smart polymer material. The capacity of the graphite material is improved by a catalytic graphitization process; the capacity and rate performance are further improved by adding a silicon-based material; the rate performance is improved by granulation and hard carbon coating; the ionic smart polymer coating layer can improve the ionic conductivity through its ionic bond effect, promote Li + On the other hand, the "intelligent switch" structure formed can maintain effective connection between particles to achieve the purpose of alleviating the rapid performance decay caused by the volume expansion of silicon particles when lithium is inserted; the introduction of carbon nanotubes not only improves the conductivity, but also provides support when the silicon particles expand in volume due to lithium insertion, maintaining the stability and integrity of the electrode conductive structure. The carbon nanotubes used in the present invention not only have a conductive function, but also a supporting function.
[0035] The first step is to prepare graphitized particles through catalytic graphitization process, which can not only improve the degree of graphitization and capacity, thereby improving energy density, but also its surface is rich in pores, which can increase the transmission channel of lithium ions and provide Li + Providing a transmission path to the interior of the particle and the reaction center is beneficial to improving the rate performance;
[0036] The second step is to embed nano-silicon into the internal pores and surface of graphite particles through a spheroidization process to prepare silicon-based particles, which provides space and stress relief for the volume expansion of silicon particles when lithium is embedded, and helps to alleviate the rapid performance decay of silicon particles caused by volume expansion when lithium is embedded.
[0037] In the third step, the graphitized particles and silicon-based particles prepared in the first two steps are mixed in a certain proportion, coated with a resin material in liquid phase and dried to form particles with a resin coating layer, and then carbonized to form single particles with a hard carbon coating layer. The hard carbon structure is conducive to increasing the transfer channel of lithium ions, further improving the isotropy of the material, and promoting the transfer of lithium ions into the particles;
[0038] In the fourth step, an aqueous solution of an ionic smart polymer material (i.e., a zwitterionic polymer) is added, and granulated by a spray drying process to obtain a granulated product having an ionic smart polymer material coating layer, and then carbon nanotubes are added and mixed to obtain a high-capacity, high-rate composite graphite negative electrode material product, such as Figure 1 Granulation can improve the isotropy of the material, thereby improving the rate performance. The zwitterionic structure on the polymer chain segment is beneficial to improving the conductivity of lithium ions and effectively promoting Li + Transfer from the electrolyte to the surface of the negative electrode material particles, shortening the transmission path of lithium ions, that is, shortening the Li + The distance to the surface of the active substance and then to the reaction center, such as Figure 2 As shown, the zwitterions on the polymer chain segments can form a "smart switch" structure. + When embedded, the volume of silicon particles expands, and the "switch" between particles and inside the granules is turned on. + After the escape, due to the action of ionic bonds, the "switch" is closed, such as Figure 3 and Figure 4 As shown in the figure, the structure of the "smart switch" is conducive to maintaining the stability and integrity of the electrode structure and alleviating the rapid performance degradation caused by the volume expansion of silicon particles when lithium is inserted. The addition of carbon nanotubes not only improves the conductivity, but also provides support when the silicon particles expand in volume due to lithium insertion, maintaining the stability and integrity of the electrode conductive network.
[0039] In short, the structure of the composite graphite negative electrode material prepared in the above manner can effectively shorten the transmission path of lithium ions, that is, shorten the Li +The distance to the surface of the active material and then to the reaction center, and the "smart switch" structure and carbon nanotubes are beneficial to maintaining the stability and integrity of the electrode structure, and alleviating the rapid performance decay caused by the volume expansion of silicon particles when lithium is embedded. It has the characteristics of good isotropy, fast ion transfer rate, multiple transfer channels, and stable electrode structure. The lithium-ion battery electrode prepared by it has the characteristics of high energy density and good fast charging performance.
[0040] Specifically, as one aspect of the technical solution of the present invention, a composite graphite negative electrode material involved includes:
[0041] A plurality of secondary particles, wherein the secondary particles include primary particles and a zwitterionic polymer coating layer that encapsulates the primary particles, the primary particles include graphitized particles having a hard carbon coating layer and silicon-based particles having a hard carbon coating layer, the graphitized particles have a porous structure, and the silicon-based particles include graphite particles with nano-silicon particles distributed on the surface and inside;
[0042] And, the carbon nanotubes are at least connected between a plurality of the secondary particles.
[0043] In some preferred embodiments, the graphitized particles having a hard carbon coating layer include graphitized particles as a core structure and a hard carbon coating layer coated on the surface of the graphitized particles.
[0044] In some preferred embodiments, the graphitized particles in the graphitized particles having a hard carbon coating layer are micron-sized single particles, and the graphitized particles include any one or more combinations of natural graphite, artificial graphite, expanded graphite, oxidized graphite, and microcrystalline graphite, but are not limited thereto.
[0045] In some preferred embodiments, the particle size D50 of the graphitized particles having the hard carbon coating layer is 3-20 μm.
[0046] Furthermore, the particle size D50 of the graphitized particles in the graphitized particles having the hard carbon coating layer is 5 to 10 μm.
[0047] In some preferred embodiments, the content of the hard carbon coating layer in the graphitized particles having the hard carbon coating layer is 0.01-5 wt %.
[0048] Furthermore, the content of the hard carbon coating layer in the graphitized particles having the hard carbon coating layer is 0.01 to 3 wt %.
[0049] In some preferred embodiments, the silicon-based particles having a hard carbon coating layer include silicon-based particles as a core structure and a hard carbon coating layer coated on the surface of the silicon-based particles.
[0050] In some preferred embodiments, the nano-silicon particles in the silicon-based particles are distributed in the internal pores and surfaces of the graphite particles.
[0051] In some preferred embodiments, the median particle size of the nano-silicon particles is 20-100 nm.
[0052] In some preferred embodiments, the graphite particles include any one or more combinations of natural graphite, expanded graphite, oxidized graphite, and microcrystalline graphite, but are not limited thereto.
[0053] In some preferred embodiments, the porosity of the graphite particles is 5-50%.
[0054] In some preferred embodiments, the particle size D50 of the graphite particles is 1-10 μm.
[0055] Furthermore, the particle size D50 of the graphite particles is 1 to 5 μm.
[0056] Furthermore, the content of nano silicon particles in the silicon-based particles having the hard carbon coating layer is 0.01 to 50 wt %.
[0057] Furthermore, the content of nano silicon particles in the silicon-based particles having the hard carbon coating layer is 1 to 30 wt %.
[0058] In some preferred embodiments, the content of the hard carbon coating layer in the silicon-based particles having the hard carbon coating layer is 0.01-5 wt %.
[0059] Furthermore, the content of the hard carbon coating layer in the silicon-based particles having the hard carbon coating layer is 0.01 to 3 wt %.
[0060] In some preferred embodiments, the zwitterionic polymer coating layer includes a zwitterionic polymer polypropanesulfonate betaine (PDMAPS), but is not limited thereto.
[0061] In some preferred embodiments, the content of the zwitterionic polymer coating layer in the composite graphite negative electrode material is 0.01-20 wt %.
[0062] Furthermore, the content of the zwitterionic polymer coating layer in the composite graphite negative electrode material is 0.01 to 10 wt %.
[0063] In some preferred embodiments, the content of carbon nanotubes in the composite graphite negative electrode material is 0.01-3 wt %.
[0064] Furthermore, the content of carbon nanotubes in the composite graphite negative electrode material is 0.01-1 wt%.
[0065] In some preferred embodiments, the particle size D50 of the composite graphite negative electrode material is 5 to 30 μm.
[0066] Furthermore, the particle size D50 of the composite graphite negative electrode material is 8 to 20 μm.
[0067] In some more specific embodiments, the composite graphite negative electrode material is a granulated product of a silicon-based composite material coated with an ionic smart polymer material, and the granulated product of the silicon-based composite material coated with an ionic smart polymer material includes: a plurality of secondary particles, the secondary particles include primary particles and a zwitterionic polymer coating layer wrapping the primary particles, the primary particles include graphitized particles with a hard carbon coating layer and silicon-based particles with a hard carbon coating layer, the graphitized particles have a porous structure, and the silicon-based particles include graphite particles with nano-silicon particles distributed on the surface and inside; and carbon nanotubes, at least connected between a plurality of the secondary particles.
[0068] Furthermore, the graphitized particles in the graphitized particles with a hard carbon coating layer are single graphite micron-sized particles, including one or more combinations of natural graphite, artificial graphite (prepared by a catalytic graphitization process), expanded graphite, oxidized graphite and microcrystalline graphite. The particle size D50 of the above-mentioned single graphite particles is 3-20μm, for example, 3μm, 5μm, 7μm, 9μm, 10μm, 12μm, 15μm, 18μm or 20μm, preferably D50=5-10μm; the catalyst added to the artificial graphite (prepared by a catalytic graphitization process) during the graphitization process is one or more combinations of ferric oxide, silicon carbide and boron oxide; the amount of catalyst added is 0.1~20wt%, preferably 1~10wt%.
[0069] Furthermore, the median particle size of the nano-silicon particles used in the silicon-based particles with a hard carbon coating layer is 20 to 100 nm, the graphite particles used include one or more combinations of natural graphite, expanded graphite, oxidized graphite and microcrystalline graphite, and the particle size of the graphite particles is D50 = 1 to 10 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, preferably 1-5 μm; the mass of the nano-silicon particles accounts for 0.01-50wt% of the mass of the prepared silicon-based material, for example, 0.01wt%, 0.1wt%, 1wt%, 5wt%, 10wt%, 20wt%, 30wt%, 40wt% or 50wt%; preferably 1-30wt%.
[0070] Furthermore, the precursor of the hard carbon coating layer of the graphitized particles with a hard carbon coating layer and the silicon-based particles with a hard carbon coating layer is a water-soluble resin material, which is one or more combinations of phenolic resin, epoxy resin, furfural resin, acrylic resin, polyurethane resin, acrylic-polyurethane copolymer, furan resin, polyvinyl alcohol, chitosan, cellulose, styrene-butadiene rubber, and glucose. The graphite single particle, silicon-based composite material, water-soluble resin material and water are mixed and dried, and a single particle product with a hard carbon coating layer is formed after carbonization, wherein the mass of the hard carbon coating layer accounts for 0.01-5wt% of the single particle product, such as 0.01wt%, 0.1wt%, 1wt%, 2wt%, 3wt%, 4wt% or 5wt%; preferably 0.01-3%. The mass of the hard carbon precursor accounts for 0.1-20wt% of the single particle product.
[0071] Furthermore, the above-mentioned single particle product with a hard carbon coating layer is added to a zwitterionic smart polymer aqueous solution, mixed, and then granulated by a spray drying process, and then carbon nanotubes are added and fully mixed to prepare a high-capacity, high-rate composite graphite negative electrode material product. The ionic smart polymer is a zwitterionic polymer (polypropanesulfonate betaine, PDMAPS), such as Figure 5 As shown, its infrared image is Figure 6 As shown. The mass of the zwitterionic smart polymer material accounts for 0.01-20wt% of the entire finished negative electrode material, such as 0.01wt%, 0.1wt%, 1wt%, 3wt%, 5wt%, 10wt%, 15wt% or 20wt%; preferably 0.01-10wt%. The mass of the carbon nanotubes accounts for 0.01-3wt% of the entire finished negative electrode material, such as 0.01wt%, 0.1wt%, 0.5wt%, 1wt%, 2wt%1 or 3wt%; preferably 0.01-1%. The particle size of the finished product is D50 = 5-30μm, such as 5μm, 10μm, 15μm, 20μm, 25μm or 30μm; preferably D50 = 8-20μm.
[0072] Another aspect of the embodiments of the present invention further provides a method for preparing a composite graphite negative electrode material, which comprises:
[0073] The coke raw material is subjected to catalytic graphitization treatment by adopting a catalytic graphitization process to obtain graphitized particles;
[0074] The silicon-based particles are obtained by embedding nano-silicon particles into the internal pores and surface of graphite particles using a spheroidization process;
[0075] The graphitized particles, silicon-based particles, and water-soluble resin are added into water and mixed thoroughly, and then dried and carbonized to obtain primary particles; wherein the primary particles include graphitized particles with a hard carbon coating layer and silicon-based particles with a hard carbon coating layer;
[0076] Furthermore, the zwitterionic polymer is coated on the surface of the primary particles by a spray drying process to prepare a secondary particle structure, which is then mixed with carbon nanotubes to prepare a composite graphite negative electrode material.
[0077] In some preferred embodiments, the method for preparing the graphitized particles comprises: mixing the coke raw material with the catalyst and performing a catalytic graphitization treatment at 2800-3000° C. to obtain graphitized particles;
[0078] In some preferred embodiments, the catalyst includes any one or more combinations of ferric oxide, silicon carbide, and boron trioxide, but is not limited thereto.
[0079] In some preferred embodiments, the coke raw material includes any one or more combinations of petroleum coke, needle coke, and coal-based coke, but is not limited thereto.
[0080] In some preferred embodiments, the particle size D50 of the coke raw material is 3-20 μm.
[0081] Furthermore, the particle size D50 of the coke raw material is 5 to 10 μm.
[0082] In some preferred embodiments, the added amount of the catalyst is 0.1-20 wt % of the sum of the coke feedstock and the catalyst.
[0083] Furthermore, the added amount of the catalyst is 1 to 10 wt % of the sum of the coke raw material and the catalyst.
[0084] In some preferred embodiments, the device used for the catalytic graphitization treatment includes an Acheson furnace, a box furnace, an inner series furnace or a continuous graphitization furnace.
[0085] In some preferred embodiments, the preparation method specifically includes: fully stirring and mixing the graphitized particles, silicon-based particles, water-soluble resin and water to coat and dry them to obtain single particles with a resin coating layer, and then carbonizing them in a protective atmosphere to obtain single particles with a hard carbon coating layer.
[0086] Furthermore, the mass ratio of the graphitized particles, the silicon-based particles and the water-soluble resin is (1-100): (1-80): (0.01-5).
[0087] Furthermore, the water-soluble resin includes any one or more combinations of phenolic resin, epoxy resin, furfural resin, acrylic resin, polyurethane resin, acrylic-polyurethane copolymer, furan resin, polyvinyl alcohol, chitosan, cellulose, styrene-butadiene rubber, and glucose, and is not limited thereto.
[0088] Furthermore, the stirring speed is 10-2000 r / min, and the stirring time is 10 min-10 h.
[0089] Furthermore, the drying treatment adopts a drying temperature of 40 to 150° C. and a drying time of 0.5 to 20 hours.
[0090] Furthermore, the temperature of the carbonization treatment is 400-1300°C.
[0091] Furthermore, the carbonization treatment time is 2 to 15 hours.
[0092] Further, the protective atmosphere includes a nitrogen atmosphere, but is not limited thereto.
[0093] Furthermore, the mass ratio of the water-soluble resin to water is (0.1-90):(99.9-10).
[0094] In some preferred embodiments, the preparation method specifically comprises:
[0095] The primary particles are mixed with an aqueous solution containing a zwitterionic polymer, subjected to a spray drying and granulation treatment, and then mixed with carbon nanotubes to obtain a composite graphite negative electrode material;
[0096] Wherein, the content of the zwitterionic polymer in the aqueous solution containing the zwitterionic polymer is 0.1-90wt%.
[0097] In some more specific embodiments, the method for preparing the composite graphite negative electrode material includes:
[0098] (1) The coke raw material and the catalyst are weighed and mixed uniformly according to a certain proportion, and then graphitized to obtain graphitized particles, such as Figure 7 As shown, the graphitization process can adopt an Acheson furnace, a box furnace, an inner series furnace or a continuous graphitization furnace;
[0099] (2) Nano-silicon particles and graphite particles are weighed in proportion and added into a spheroidizer to prepare silicon-based particles, such as Figure 8 and Figure 9a-9b As shown;
[0100] (3) The graphitized particles prepared in step (1), the silicon-based particles prepared in step (2) and the water-soluble resin material are weighed in proportion and added to water, fully stirred and dried, and carbonized to form a uniform hard carbon coating layer. The stirring speed is 10-2000r / min, the stirring time is 10min-10h, the drying temperature is 40-150°C, the drying time is 0.5-20h, the carbonization temperature is 400-1300°C, the carbonization time is 2-15h, and the process is carried out in a protective gas atmosphere, which can be nitrogen.
[0101] (4) adding the graphitized particles with a hard carbon coating layer and the silicon-based particles with a hard carbon coating layer prepared in step (3) to an aqueous solution containing an ionic smart polymer material, granulating the particles by a spray drying process, and then adding carbon nanotubes (such as Fig.10 As shown) and fully mixed, a high-capacity, high-rate composite graphite negative electrode material product is prepared, such as Figure 11-Figure 12 The ionic intelligent polymer material is a zwitterionic polymer, the solid content of the solution thereof is 0.1-90wt%, and the addition amount thereof is 0.1-10wt% of the entire negative electrode active material.
[0102] The comprehensive carbon-based skeleton of the present invention can provide buffer space and stress for the volume expansion of silicon-based materials when lithium is embedded, carbon nanotubes can improve conductivity, flexible polymers can improve the binding ability of silicon-based materials, and have the beneficial effect of a high ionic conductivity coating layer, and further introduces an "intelligent switch" structure, which can not only provide binding ability for the volume expansion of silicon-based materials when lithium is embedded and play a certain degree of relief effect, but also can further improve the binding ability of the secondary particles as a whole through the "switch" structure and maintain the effective connection between particles and the integrity of the conductive network to achieve the purpose of alleviating the rapid performance decay of silicon particles caused by the volume expansion when lithium is embedded.
[0103] Another aspect of the embodiments of the present invention further provides the use of the aforementioned composite graphite negative electrode material or the composite graphite negative electrode material prepared by the aforementioned preparation method in preparing a battery negative electrode sheet or a lithium-ion battery.
[0104] Another aspect of the embodiments of the present invention further provides a lithium-ion battery negative electrode sheet, which includes the aforementioned composite graphite negative electrode material or the composite graphite negative electrode material prepared by the aforementioned preparation method.
[0105] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0106] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.
[0107] 1. Preparation of graphitized particles: Using coke micron particles with D50=8μm as raw materials and boron trioxide as catalyst, weigh them in proportion and mix them evenly, and then prepare graphitized particles through a graphitization process at 3000℃ in an Acheson furnace.
[0108] Example 1
[0109] 990 g of coke micron particles (D50=8 μm) and 10 g of boron trioxide were added into a VC machine for mixing at a stirring speed of 300 r / min and a mixing time of 60 min, and then graphitized to prepare graphitized particles.
[0110] Example 2
[0111] 950 g of coke micron particles (D50=8 μm) and 50 g of boron trioxide were added into a VC machine for mixing at a stirring speed of 300 r / min and a mixing time of 60 min, and then graphitized to prepare graphitized particles.
[0112] Example 3
[0113] 900 g of coke micron particles (D50=8 μm) and 100 g of boron trioxide were added into a VC machine for mixing at a stirring speed of 300 r / min and a mixing time of 60 min, and then graphitized to prepare graphitized particles.
[0114] Example 4
[0115] 850 g of coke micron particles (D50=8 μm) and 150 g of boron trioxide were added into a VC machine for mixing at a stirring speed of 300 r / min and a mixing time of 60 min, and then graphitized to prepare graphitized particles.
[0116] Example 5
[0117] 800 g of coke micron particles (D50=8 μm) and 200 g of boron trioxide were added into a VC machine for mixing at a stirring speed of 300 r / min and a mixing time of 60 min, and then graphitized to prepare graphitized particles.
[0118] Comparative Example 1
[0119] 1000 g of coke micron particles (D50=8 μm) were graphitized to prepare graphitized particles.
[0120] Table 1 Basic indicators and power-off test results of graphitized particles in Examples 1-5 and Comparative Example 1
[0121]
[0122]
[0123] The above results show that as the amount of catalyst added increases, the degree of graphitization increases, the capacity and rate performance improve, and the specific surface area increases, indicating that the surface pores increase, but the tap compaction decreases. Taking into account various indicators, furnace loading and cost, the graphitized particles prepared in Example 3 with a catalyst addition of 10% were selected as the substrate for subsequent example experiments.
[0124] 2. Preparation of silicon-based particles: Nano silicon particles and graphite particles were weighed in proportion, mixed evenly, and added to a spheroidizer to prepare silicon-based particles. For parallel performance comparison, the particle size of the silicon-based particles prepared in Examples 6 to 10 was controlled at about D50 = 5 μm by adjusting the spheroidization parameters.
[0125] Example 6
[0126] 50 g of nano silicon particles and 950 g of graphite particles were added to a VC machine for mixing at a stirring speed of 300 r / min. After mixing for 60 min, the mixture was added to a spheroidizer for spheroidization to prepare silicon-based particles.
[0127] Example 7
[0128] 150 g of nano silicon particles and 850 g of graphite particles were added to a VC machine for mixing at a stirring speed of 300 r / min. After mixing for 60 min, the mixture was added to a spheroidizer for spheroidization to prepare silicon-based particles.
[0129] Example 8
[0130] 300 g of nano silicon particles and 700 g of graphite particles were added to a VC machine for mixing at a stirring speed of 300 r / min. After mixing for 60 min, the mixture was added to a spheroidizer and spheroidized to prepare silicon-based particles.
[0131] Example 9
[0132] 400 g of nano silicon particles and 600 g of graphite particles were added to a VC machine for mixing at a stirring speed of 300 r / min. After mixing for 60 min, the mixture was added to a spheroidizer for spheroidization to prepare silicon-based particles.
[0133] Example 10
[0134] 500 g of nano silicon particles and 500 g of graphite particles were added to a VC machine for mixing at a stirring speed of 300 r / min. After mixing for 60 min, the mixture was added to a spheroidizer and spheroidized to prepare silicon-based particles.
[0135] Table 2. Test results of the silicon-based particles in Examples 6-10.
[0136]
[0137]
[0138] 3. Preparation of primary particles: Graphitized particles and silicon-based particles are mixed in proportion, coated with a resin material in liquid phase and carbonized to form single particles with a hard carbon coating layer, i.e., primary particles, including graphitized particles with a hard carbon coating layer and silicon-based particles with a hard carbon coating layer.
[0139] The graphitized particles prepared in the above-mentioned Example 3 and the silicon-based particles prepared in Example 7 are fully mixed in a mass ratio of 7:3 and used as aggregates for subsequent processes. The above-mentioned aggregates and water-soluble resin materials are weighed in proportion and added into water, and stirred thoroughly at a stirring speed of 300 r / min for 60 min. After drying, they are carbonized to form a uniform hard carbon coating layer. The drying temperature is 40-150°C and the drying time is 0.5-20h. The carbonization adopts a high sand kiln at a temperature of 1150°C and a carbonization time of 10h in a nitrogen atmosphere.
[0140] In order to compare the performance in parallel, the hard carbon precursors used were all water-soluble phenolic resins, and the residual carbon was calculated as 50%.
[0141] Embodiment 11
[0142] 99.5g of the mixed aggregates are added into 100g of phenolic resin dispersion with a solid content of 1%, and stirred thoroughly. After drying, the mixture is added into a high sand kiln for carbonization to prepare a composite single particle product with a hard carbonization layer mass of 0.5%, i.e., a primary particle.
[0143] Example 12
[0144] 99g of the mixed aggregates are added into 100g of phenolic resin dispersion with a solid content of 2%, and stirred thoroughly. After drying, the mixture is added into a high sand kiln for carbonization to prepare a composite single particle product with a hard carbonized layer of 1% by mass, i.e., a primary particle.
[0145] Example 13
[0146] 98g of the mixed aggregate is added into 100g of phenolic resin dispersion with a solid content of 4% and stirred thoroughly. After drying, it is added into a high sand kiln for carbonization to prepare a composite single particle product with a hard carbonized layer of 2% by mass, i.e., a primary particle.
[0147] Embodiment 14
[0148] 97g of the mixed aggregate is added into 100g of phenolic resin dispersion with a solid content of 6%, and stirred thoroughly. After drying, it is added into a high sand kiln for carbonization to prepare a composite single particle product with a hard carbonized layer of 3% by mass, i.e., primary particles.
[0149] Embodiment 15
[0150] 95g of the mixed aggregate is added into 100g of phenolic resin dispersion with a solid content of 10%, and stirred thoroughly. After drying, it is added into a high sand kiln for carbonization to prepare a composite single particle product with a hard carbonized layer of 5% by mass, namely, a primary particle.
[0151] Table 3. Test results of primary particles in Examples 11-15.
[0152]
[0153] The above results show that with the increase of hard carbon coating content, the rate performance is improved, but the effect of improving the expansion of the electrode is not obvious, which means that the hard carbon layer can significantly improve the rate performance, but has no obvious restraining effect on the volume expansion of silicon particles caused by the lithium insertion process.
[0154] 4. Preparation of secondary particles: Add the primary particles into a solution containing zwitterionic smart polymer materials, stir thoroughly and then granulate by spray drying process, so that the zwitterionic smart polymer materials are evenly coated on the surface of the primary particles.
[0155] In order to compare the performance in parallel, Examples 16 to 23 all used the single granules prepared in Example 14 to carry out experiments, and the particle size of the granules was adjusted to D50 = 15 μm by adjusting the parameters of the spray drying process. The zwitterionic polymer in the following examples is polypropanesulfonate betaine.
[0156] Example 16
[0157] 99.5g of the single granule product was added into 100g of a zwitterionic polymer solution with a solid content of 0.5%, stirred evenly, and then spray-dried to prepare a granulated product containing a zwitterionic polymer coating layer, namely, secondary granules.
[0158] Embodiment 17
[0159] 99g of the single granule product was added into 100g of a zwitterionic polymer solution with a solid content of 1%, stirred evenly, and then spray-dried to prepare a granulated product containing a zwitterionic polymer coating layer, namely, secondary granules.
[0160] Embodiment 18
[0161] 97g of the single granule product was added into 100g of a zwitterionic polymer solution with a solid content of 3%, stirred evenly, and then spray-dried to prepare a granulated product containing a zwitterionic polymer coating layer, namely, secondary granules.
[0162] Embodiment 19
[0163] 95g of the single granule product was added into 100g of a zwitterionic polymer solution with a solid content of 5%, stirred evenly, and then spray-dried to prepare a granulated product containing a zwitterionic polymer coating layer, namely, secondary granules.
[0164] Embodiment 20
[0165] 92g of the single granule product was added into 100g of a zwitterionic polymer solution with a solid content of 8%, stirred evenly, and then spray-dried to prepare a granulated product containing a zwitterionic polymer coating layer, namely, secondary granules.
[0166] Embodiment 21
[0167] 90g of the single granule product was added into 100g of a zwitterionic polymer solution with a solid content of 10%, stirred evenly, and then spray-dried to prepare a granulated product containing a zwitterionic polymer coating layer, namely, secondary granules.
[0168] Embodiment 22
[0169] 85g of the single granule product was added into 100g of a zwitterionic polymer solution with a solid content of 15%, stirred evenly, and then spray-dried to prepare a granulated product containing a zwitterionic polymer coating layer, namely, secondary granules.
[0170] Embodiment 23
[0171] 80g of the single granule product was added into 100g of a zwitterionic polymer solution with a solid content of 20%, stirred evenly, and then spray-dried to prepare a granulated product containing a zwitterionic polymer coating layer, namely, secondary granules.
[0172] Table 4: Test results of the granules containing zwitterionic polymer coating layers in Examples 16-23
[0173]
[0174] The above results show that with the increase in the amount of zwitterionic polymer added, the ionic conductivity of the electrode increases, the rate performance improves, and the electrode expansion rate is significantly reduced, indicating that the zwitterionic polymer has a significant restraining effect on the expansion of the electrode, that is, the volume expansion of silicon particles due to lithium insertion, which is beneficial to resolve the rapid performance attenuation caused by the volume expansion of silicon particles when lithium is inserted.
[0175] 5. Preparation of composite graphite negative electrode material: The granulated product with the zwitterionic polymer coating layer prepared above and carbon nanotubes are weighed in proportion and fully mixed to prepare a high-capacity and high-rate composite graphite negative electrode material product.
[0176] In order to compare the performance in parallel, Examples 24 to 29 all used the granulated product with a zwitterionic polymer coating layer prepared in Example 21 to carry out experiments.
[0177] Embodiment 24
[0178] 99.95 g of the granulated product having the zwitterionic polymer coating layer and 0.05 g of the carbon nanotubes were fully and uniformly mixed to prepare a high-capacity and high-rate composite graphite negative electrode material product.
[0179] Embodiment 25
[0180] 99.9 g of the granulated product having a zwitterionic polymer coating layer and 0.1 g of carbon nanotubes were fully and uniformly mixed to prepare a high-capacity and high-rate composite graphite negative electrode material product.
[0181] Embodiment 26
[0182] 99.5 g of the granulated product having the zwitterionic polymer coating layer and 0.5 g of the carbon nanotubes were fully and uniformly mixed to prepare a high-capacity and high-rate composite graphite negative electrode material product.
[0183] Embodiment 27
[0184] 99 g of the granulated product having a zwitterionic polymer coating layer and 1 g of carbon nanotubes were fully and uniformly mixed to prepare a high-capacity and high-rate composite graphite negative electrode material product.
[0185] Embodiment 28
[0186] 98 g of the granulated product having a zwitterionic polymer coating layer and 2 g of carbon nanotubes were fully and uniformly mixed to prepare a high-capacity and high-rate composite graphite negative electrode material product.
[0187] Embodiment 29
[0188] 97 g of the granulated product having a zwitterionic polymer coating layer and 3 g of carbon nanotubes were fully and evenly mixed to prepare a high-capacity and high-rate composite graphite negative electrode material product.
[0189] Table 5. Results of the withholding test of the finished products of high capacity and high rate composite graphite negative electrode materials of Examples 24-29
[0190]
[0191] The above results show that with the increase of the addition amount of carbon nanotubes, the impedance of the electrode is significantly reduced, indicating that the conductivity is significantly improved, and the electrode expansion rate is slightly reduced but not significantly reduced, indicating that carbon nanotubes have no obvious restraining ability on the volume expansion of silicon particles due to lithium insertion, but can provide a certain support effect, which is beneficial to maintain the stability and integrity of the electrode conductive network, thereby improving the rate performance.
[0192] Based on the test results of the above embodiments, the catalytic graphitized single particle product prepared in Example 3 was used as the substrate to carry out experiments in subsequent embodiments and comparative examples. The hard carbon precursor used was a water-soluble phenolic resin, and the residual carbon was calculated as 50%.
[0193] Embodiment 30
[0194] The catalytic graphitized single particle product and the silicon-based negative electrode material prepared in Example 6 were fully mixed in a mass ratio of 7:3 and used as aggregate for subsequent processes. 98g of the above aggregate was added to 100g of a phenolic resin dispersion with a solid content of 4% and fully stirred. After drying, it was added to a high sand kiln for carbonization. 94.5g of carbide was weighed and added to 100g of a zwitterionic polymer solution with a solid content of 5%. After stirring evenly, a granulated product containing a zwitterionic polymer coating layer was prepared by a spray drying process. Then, 99.5g of the prepared granulated product and 0.5g of carbon nanotubes were fully mixed to prepare a high-capacity, high-rate composite graphite negative electrode material finished product.
[0195] The mass of silicon nanoparticles in the silicon-based composite material used in the prepared graphite negative electrode material product accounts for 5%, the mass of the hard carbon carbonization layer accounts for 2% of the single particle product, the mass of the zwitterionic polymer accounts for 5% of the entire negative electrode material product, and the mass of the carbon nanotubes accounts for 0.5% of the entire negative electrode material product.
[0196] Embodiment 31
[0197] The catalytic graphitized single particle product and the silicon-based negative electrode material prepared in Example 6 were fully mixed in a mass ratio of 7:3 and used as aggregate for subsequent processes. 98g of the above aggregate was added to 100g of a phenolic resin dispersion with a solid content of 4% and fully stirred. After drying, it was added to a high sand kiln for carbonization. 89.5g of carbide was weighed and added to 100g of a zwitterionic polymer solution with a solid content of 10%. After stirring evenly, a granulated product containing a zwitterionic polymer coating layer was prepared by a spray drying process. Then, the prepared 99.5g of the granulated product and 0.5g of carbon nanotubes were fully mixed to prepare a high-capacity, high-rate composite graphite negative electrode material finished product.
[0198] The mass of silicon nanoparticles in the silicon-based composite material used in the prepared graphite negative electrode material product accounts for 5%, the mass of the hard carbon carbonization layer accounts for 2% of the single particle product, the mass of the zwitterionic polymer accounts for 10% of the entire negative electrode material product, and the mass of the carbon nanotubes accounts for 0.5% of the entire negative electrode material product.
[0199] Embodiment 32
[0200] The catalytic graphitized single particle product and the silicon-based negative electrode material prepared in Example 8 were fully mixed in a mass ratio of 7:3 and used as aggregate for subsequent processes. 98g of the above aggregate was added to 100g of a phenolic resin dispersion with a solid content of 4% and fully stirred. After drying, it was added to a high sand kiln for carbonization. 84.5g of carbide was weighed and added to 100g of a zwitterionic polymer solution with a solid content of 15%. After stirring evenly, a granulated product containing a zwitterionic polymer coating layer was prepared by a spray drying process. Then, 99.5g of the prepared granulated product and 0.5g of carbon nanotubes were fully mixed to prepare a high-capacity, high-rate composite graphite negative electrode material finished product.
[0201] The mass of silicon nanoparticles in the silicon-based composite material used in the prepared graphite negative electrode material product accounts for 30%, the mass of the hard carbon carbonization layer accounts for 2% of the single particle product, the mass of the zwitterionic polymer accounts for 15% of the entire negative electrode material product, and the mass of the carbon nanotubes accounts for 0.5% of the entire negative electrode material product.
[0202] Embodiment 33
[0203] The catalytic graphitized single particle product and the silicon-based negative electrode material prepared in Example 10 were fully mixed in a mass ratio of 7:3 and used as aggregate for subsequent processes. 98g of the above aggregate was added to 100g of a phenolic resin dispersion with a solid content of 4% and fully stirred. After drying, it was added to a high sand kiln for carbonization. 79.5g of carbide was weighed and added to 100g of a zwitterionic polymer solution with a solid content of 20%. After stirring evenly, a granulated product containing a zwitterionic polymer coating layer was prepared by a spray drying process. Then, the prepared 99.5g of the granulated product and 0.5g of carbon nanotubes were fully mixed to prepare a high-capacity, high-rate composite graphite negative electrode material finished product.
[0204] The mass of silicon nanoparticles in the silicon-based composite material used in the prepared graphite negative electrode material product accounts for 50%, the mass of the hard carbon carbonization layer accounts for 2% of the single particle product, the mass of the zwitterionic polymer accounts for 20% of the entire negative electrode material product, and the mass of the carbon nanotubes accounts for 0.5% of the entire negative electrode material product.
[0205] Comparative Example 2
[0206] The natural graphite single particle product and the silicon-based negative electrode material prepared in Example 6 were fully mixed in a mass ratio of 7:3 and used as aggregate for the subsequent process. 98g of the above aggregate was added to 100g of a phenolic resin dispersion with a solid content of 4% and fully stirred. After drying, it was added to a high sand kiln for carbonization. 89.5g of carbide was weighed and added to 100g of a zwitterionic polymer solution with a solid content of 10%. After stirring evenly, a granulated product containing a zwitterionic polymer coating layer was prepared by a spray drying process. Then, the prepared 99.5g of the granulated product and 0.5g of carbon nanotubes were fully mixed to prepare a finished composite graphite negative electrode material.
[0207] The mass of silicon nanoparticles in the silicon-based composite material used in the prepared graphite negative electrode material product accounts for 5%, the mass of the hard carbon carbonization layer accounts for 2% of the single particle product, the mass of the zwitterionic polymer accounts for 10% of the entire negative electrode material product, and the mass of the carbon nanotubes accounts for 0.5% of the entire negative electrode material product.
[0208] Comparative Example 3
[0209] The natural graphite single particle product and the silicon-based negative electrode material prepared in Example 6 were fully mixed in a mass ratio of 7:3 and used as aggregate for the subsequent process. 196g of the above aggregate was added to 200g of a phenolic resin dispersion with a solid content of 4% and fully stirred. After drying, it was added to a high sand kiln for carbonization. 99.5g of carbide and 0.5g of carbon nanotubes were weighed and fully mixed to prepare a finished composite graphite negative electrode material.
[0210] The mass of silicon nanoparticles in the silicon-based composite material used in the prepared graphite negative electrode material product accounts for 5%, the mass of the hard carbon carbonization layer accounts for 2% of the single particle product, and the mass of the carbon nanotubes accounts for 0.5% of the entire negative electrode material product.
[0211] Comparative Example 4
[0212] The microcrystalline graphite single particle product and the silicon-based negative electrode material prepared in Example 6 were fully mixed in a mass ratio of 7:3 and used as aggregate for subsequent processes. 98g of the above aggregate was added to 100g of a phenolic resin dispersion with a solid content of 4% and fully stirred. After drying, it was added to a high sand kiln for carbonization. 89.5g of carbide was weighed and added to 100g of a zwitterionic polymer solution with a solid content of 10%. After stirring evenly, a granulated product containing a zwitterionic polymer coating layer was prepared by a spray drying process. Then, the prepared 99.5g of the granulated product and 0.5g of carbon nanotubes were fully mixed to prepare a high-capacity, high-rate composite graphite negative electrode material finished product.
[0213] The mass of silicon nanoparticles in the silicon-based composite material used in the prepared graphite negative electrode material product accounts for 5%, the mass of the hard carbon carbonization layer accounts for 2% of the single particle product, the mass of the zwitterionic polymer accounts for 10% of the entire negative electrode material product, and the mass of the carbon nanotubes accounts for 0.5% of the entire negative electrode material product.
[0214] Comparative Example 5
[0215] The microcrystalline graphite single particle product and the silicon-based negative electrode material prepared in Example 6 were fully mixed in a mass ratio of 7:3 and used as aggregate for subsequent processes. 196g of the above aggregate was added to 200g of a phenolic resin dispersion with a solid content of 4% and fully stirred. After drying, it was added to a high sand kiln for carbonization. The prepared 99.5g carbide and 0.5g carbon nanotubes were fully mixed to obtain a finished composite graphite negative electrode material.
[0216] The mass of silicon nanoparticles in the silicon-based composite material used in the prepared graphite negative electrode material product accounts for 5%, the mass of the hard carbon carbonization layer accounts for 2% of the single particle product, and the mass of the carbon nanotubes accounts for 0.5% of the entire negative electrode material product.
[0217] Electrode sheets were prepared using the binders prepared in the examples and comparative examples of the present invention, and the following properties were measured: initial discharge specific capacity, initial charge and discharge efficiency, rate performance, and impedance performance of the electrode.
[0218] The preparation method of the electrode sheet is as follows:
[0219] The above-mentioned graphite negative electrode material was formulated into a slurry in a mass ratio of graphite negative electrode material: carbon black conductive agent SP: binder = 96.5:2:1.5, and mechanically stirred for 30 minutes at room temperature with a stirring speed of 2000r / min. The prepared slurry was coated on the current collector, baked in an oven at 100°C for 30 minutes, and then dried in a vacuum drying oven at 130°C for 8 hours. The prepared pole pieces were assembled into lithium-ion button batteries for constant current charge and discharge tests. The lithium sheet was used as the counter electrode, and LiPF6 was dissolved in a mixed solvent of EC / DEC / EMC=2:3:1 at a concentration of 1 mol / L to form a non-aqueous electrolyte, wherein EC is ethylene carbonate, EMC is methyl ethyl carbonate, and DEC is diethyl carbonate. The batteries were assembled in a glove box.
[0220]
[0221] Where σ is the ionic conductivity R b is the impedance, S and d are the effective area and thickness of the electrode, respectively.
[0222] Table 6 The results of the power-off test of the finished products of high-capacity and high-rate composite graphite negative electrode materials of Examples 30-33 and the products of Comparative Examples 2-5
[0223]
[0224]
[0225] Combined with the test results of Table 1 and Table 6, the rate performance of the graphite negative electrode prepared after hard carbon coating granulation and coating zwitterionic polymer is significantly improved, the impedance is reduced and the ion conductivity is improved, but the addition of too much hard carbon coating layer and zwitterionic polymer will reduce the capacity, first effect and tapping, which is not conducive to improving the energy density of the electrode, the comprehensive performance of comprehensive capacity, first effect, tapping, rate and ion conductivity. The addition amount of the catalyst is preferably 1-10%; the mass of the silicon nanoparticles used in the silicon-based composite material is preferably 1-30%; the mass of the hard carbon coating layer is preferably 0.01-3% of the single particle product; the mass of the zwitterionic intelligent polymer material is preferably 0.01-10% of the entire finished negative electrode material; the mass of the carbon nanotube is preferably 0.01-1% of the entire finished negative electrode material.
[0226] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0227] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. A composite graphite negative electrode material, It is characterized in that include: A plurality of secondary particles, wherein the secondary particles include primary particles and a zwitterionic polymer coating layer that wraps the primary particles, the primary particles include graphitized particles with a hard carbon coating layer and silicon-based particles with a hard carbon coating layer, the graphitized particles have a porous structure, and the silicon-based particles include graphite particles with nano-silicon particles distributed on the surface and inside; wherein the graphitized particles are selected from any one or more combinations of natural graphite, artificial graphite, expanded graphite, oxidized graphite, and microcrystalline graphite; and the zwitterionic polymer in the zwitterionic polymer coating layer is selected from polypropenesulfonate betaine; And, the carbon nanotubes are at least connected between a plurality of the secondary particles.
2. The composite graphite negative electrode material according to claim 1, It is characterized in that The composite graphite negative electrode material has at least one of the following characteristics (1) to (4): (1) The graphitized particles having a hard carbon coating layer include graphitized particles as a core structure and a hard carbon coating layer coated on the surface of the graphitized particles; (2) The graphitized particles having the hard carbon coating layer are single particles of micron size; (3) The particle size D50 of the graphitized particles having the hard carbon coating layer is 3 to 20 μm; (4) The content of the hard carbon coating layer in the graphitized particles having the hard carbon coating layer is 0.01-5 wt %.
3. The composite graphite negative electrode material according to claim 2, It is characterized in that The composite graphite negative electrode material has at least one of the following characteristics (5) to (6): (5) The particle size D50 of the graphitized particles having the hard carbon coating layer is 5 to 10 μm; (6) The content of the hard carbon coating layer in the graphitized particles having the hard carbon coating layer is 0.01-3 wt %.
4. The composite graphite negative electrode material according to claim 1, It is characterized in that The composite graphite negative electrode material has at least one of the following characteristics (7) to (13): (7) The silicon-based particles having a hard carbon coating layer include silicon-based particles as a core structure and a hard carbon coating layer coated on the surface of the silicon-based particles; (8) The median particle size of the nano-silicon particles is 20 to 100 nm; (9) The graphite particles are selected from any one or more combinations of natural graphite, expanded graphite, oxidized graphite, and microcrystalline graphite; (10) The porosity of the graphite particles is 5-50%; (11) The particle size D50 of the graphite particles is 1-10 μm; (12) The content of nano silicon particles in the silicon-based particles having a hard carbon coating layer is 0.01-50 wt %; (13) The content of the hard carbon coating layer in the silicon-based particles having a hard carbon coating layer is 0.01 to 5 wt %.
5. The composite graphite negative electrode material according to claim 4, It is characterized in that The composite graphite negative electrode material has at least one of the following characteristics (14) to (16): (14) The particle size D50 of the graphite particles is 1-5 μm; (15) The content of nano silicon particles in the silicon-based particles having a hard carbon coating layer is 1 to 30 wt %; (16) The content of the hard carbon coating layer in the silicon-based particles having a hard carbon coating layer is 0.01 to 3 wt %.
6. The composite graphite negative electrode material according to claim 1, It is characterized in that The composite graphite negative electrode material has at least one of the following characteristics (17) to (19): (17) The content of the zwitterionic polymer coating layer in the composite graphite negative electrode material is 0.01-20wt%; (18) The content of carbon nanotubes in the composite graphite negative electrode material is 0.01-3 wt %; (19) The particle size D50 of the composite graphite negative electrode material is 5~30μm.
7. The composite graphite negative electrode material according to claim 6, It is characterized in that The composite graphite negative electrode material has at least one of the following characteristics (20) to (22): (20) The content of the zwitterionic polymer coating layer in the composite graphite negative electrode material is 0.01-10 wt %; (21) The content of carbon nanotubes in the composite graphite negative electrode material is 0.01-1 wt%; (22) The particle size D50 of the composite graphite negative electrode material is 8~20μm.
8. A method for preparing a composite graphite negative electrode material, It is characterized in that include: The coke raw material is subjected to catalytic graphitization treatment by a catalytic graphitization process to obtain graphitized particles; wherein the graphitized particles are selected from any one or more combinations of natural graphite, artificial graphite, expanded graphite, oxidized graphite, and microcrystalline graphite; The nano-silicon particles are embedded into the internal pores and surface of graphite particles by a spheroidization process to obtain silicon-based particles; The graphitized particles, silicon-based particles, and water-soluble resin are added into water and mixed thoroughly, and then dried and carbonized to obtain primary particles; wherein the primary particles include graphitized particles with a hard carbon coating layer and silicon-based particles with a hard carbon coating layer; And, the zwitterionic polymer is coated on the surface of the primary particles by a spray drying process to form a secondary particle structure, and then mixed with carbon nanotubes to obtain a composite graphite negative electrode material, wherein the zwitterionic polymer is selected from polypropanesulfonate betaine.
9. The preparation method according to claim 8, It is characterized in that The preparation method of the graphitized particles comprises: mixing a coke raw material with a catalyst and performing a catalytic graphitization treatment at 2800-3000° C. to obtain graphitized particles; The method for preparing the graphitized particles has at least one of the following characteristics (23) to (26): (23) The catalyst is selected from any one or more combinations of ferric oxide, silicon carbide, and boron trioxide; (24) The coke raw material is selected from any one or more combinations of petroleum coke, needle coke, and coal-based coke; (25) The amount of the catalyst added is 0.1-20 wt% of the sum of the coke raw material and the catalyst; (26) The device used for the catalytic graphitization treatment is selected from an Acheson furnace, a box furnace, an inner series furnace or a continuous graphitization furnace.
10. The preparation method according to claim 9, It is characterized in that The method for preparing the graphitized particles has the following characteristics (27): (27) The amount of the catalyst added is 1-10 wt % of the sum of the coke raw material and the catalyst.
11. The preparation method according to claim 8, It is characterized in that The preparation method specifically comprises: fully stirring and mixing the graphitized particles, silicon-based particles, water-soluble resin and water to coat and dry the mixture to obtain a water-soluble resin coated material, and then carbonizing the mixture in a protective atmosphere to obtain primary particles; The preparation method has at least one of the following characteristics (28) to (34): (28) The mass ratio of the graphitized particles, the silicon-based particles and the water-soluble resin is (1-100): (1-80): (0.01-5); (29) The water-soluble resin is selected from any one or more combinations of phenolic resin, epoxy resin, furfural resin, acrylic resin, polyurethane resin, acrylic-polyurethane copolymer, furan resin, polyvinyl alcohol, chitosan, cellulose, styrene-butadiene rubber, and glucose; (30) The stirring speed used in the stirring is 10-2000 r / min, and the stirring time is 10 min-10 h; (31) The drying temperature used in the drying process is 40-150°C and the drying time is 0.5-20h; (32) The temperature of the carbonization treatment is 400-1300°C; (33) The carbonization treatment time is 2 to 15 hours; (34) The protective atmosphere is selected from a nitrogen atmosphere.
12. The preparation method according to claim 8, It is characterized in that The preparation method specifically comprises: mixing the primary particles with an aqueous solution containing a zwitterionic polymer and subjecting the mixture to a spray drying and granulation process, and then mixing the primary particles with carbon nanotubes to obtain a composite graphite negative electrode material; Wherein, the content of the zwitterionic polymer in the aqueous solution containing the zwitterionic polymer is 0.1-90wt%.
13. Use of the composite graphite negative electrode material according to any one of claims 1 to 7 or the composite graphite negative electrode material prepared by the preparation method according to any one of claims 8 to 12 in preparing a battery negative electrode sheet or a lithium ion battery.
14. A negative electrode sheet for a lithium-ion battery, It is characterized in that The invention comprises the composite graphite negative electrode material according to any one of claims 1 to 7 or the composite graphite negative electrode material prepared by the preparation method according to any one of claims 8 to 12.
Citation Information
Patent Citations
Lithium battery silicon-oxygen composite negative electrode material with good electrochemical performance and preparation method of lithium battery silicon-oxygen composite negative electrode material
CN113206249A
Low-expansion silicon-carbon composite negative electrode material and preparation method thereof
CN113745489A
Nanometer silicon composite negative electrode active material, preparation method, pole piece and lithium ion battery
CN115692638A
Preparation method of silicon / carbon / graphite composite negative material for lithium ion battery
CN104681794A
Silicon-carbon negative electrode material and preparation method thereof
CN106941169A