An apparatus and method for the clean utilization of multi-component pyrite-type minerals
By using a multi-hearth furnace reactor to carry out an alkaline hydrogen reduction reaction, iron in pyrite is reduced to elemental iron powder and sulfur is converted into sulfate. This solves the problems of SO2 flue gas pollution and sulfuric acid treatment in pyrite-type mineral smelting plants, improves heat and hydrogen utilization, and achieves clean and efficient multi-component utilization.
Patent Information
- Application Number
- CN202311238011.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-09-25
AI Technical Summary
Existing pyrite-type mineral smelters generate SO2 flue gas pollution during the oxidative roasting process and face difficulties in sulfuric acid treatment. Furthermore, the sale and transportation of sulfuric acid are restricted, leading to environmental problems and site selection challenges.
A multi-hearth furnace reactor is used for basic hydrogen reduction reaction to reduce the iron component in pyrite to elemental iron powder, convert the sulfur component into basic sulfides, and generate sulfates through low-temperature oxidation. The countercurrent reaction in the multi-hearth furnace is used to improve heat utilization and hydrogen efficiency, and to realize the countercurrent reaction between the solid and gas phases.
It eliminates SO2 flue gas pollution, improves the utilization value of metal components, enhances heat utilization and hydrogen efficiency, solves sulfuric acid treatment and environmental protection issues, and simplifies the process flow.
Smart Images

Figure CN117490404B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of comprehensive utilization technology of pyrite, specifically relating to an apparatus and method for the clean utilization of multiple components of pyrite-type minerals. Background Technology
[0002] Pyrite-type minerals are the most widely distributed sulfide minerals in the Earth's crust, extensively found in non-ferrous metal sulfide minerals and coal. Current methods for extracting valuable components from pyrite-type minerals primarily employ oxidative roasting. However, oxidative roasting processes inevitably introduce SO2 flue gas pollution and sulfuric acid treatment issues. Although the SO2-containing tail gas produced during the oxidative roasting of pyrite-type minerals undergoes purification treatment, a certain amount of SO2 is still emitted. Furthermore, for sulfuric acid production, its selling price is related to the transportation radius, and the sales area, storage, and transportation of sulfuric acid are strictly limited, posing a significant challenge to pyrite-type mineral smelting enterprises.
[0003] Patent CN202010123459.6 discloses a method for producing sulfur-containing gas, calcium carbonate, and iron concentrate from phosphogypsum and pyrite, comprising the following steps: 1) mixing phosphogypsum and pyrite and then subjecting them to two-stage roasting to obtain sulfur-containing gas and roasting slag; 2) grinding the roasting slag obtained in step 1), leaching the ground slag in a leaching agent, and obtaining leachate and iron concentrate through solid-liquid separation; 3) mixing a carbonate donor with the leachate obtained in step 2) and reacting to obtain calcium carbonate. The method provided by this invention employs a unique phosphogypsum and pyrite recovery process, utilizing the inherent physicochemical properties of the two materials to comprehensively recover two commonly used and difficult-to-treat industrial wastes in a single step, yielding sulfur-containing gas, calcium carbonate, and iron concentrate products.
[0004] Patent CN202211435631.7 discloses a method for gas recycling and utilization in cobalt production, belonging to the field of cobalt production technology. After flotation of cobalt-containing pyrite, sulfation roasting and leaching are performed to prepare tailings and a mixed solution A. Mixed solution A is then extracted successively by P204 and P507 to obtain a cobalt chloride solution. Part of the cobalt chloride is electrolyzed to deposit cobalt, and the remaining cobalt chloride precipitates cobalt carbonate, which is then calcined to prepare cobalt powder. The heat from the calcination gas is used to heat the water leaching process, and sulfuric acid is prepared by reducing leaching using sulfur dioxide in the gas. The heat from the cobalt carbonate calcination heats ammonium chloride crystals to generate ammonia, hydrogen chloride, and water vapor. The water vapor is used to prepare sulfuric acid, the solvent water is used for recycling in the water leaching step, the ammonia is used for saponification of the lean organic phase and to produce ammonium bicarbonate with carbon dioxide generated during calcination, and the hydrogen chloride is used for back-extraction of the cobalt-containing organic phase. The hydrogen generated by electrolysis is used for reduction during the calcination of cobalt carbonate. The entire process fully utilizes the gas heat energy, and some byproducts are recycled, making it energy-saving and environmentally friendly.
[0005] Patent CN201510847679.2 discloses a method for co-roasting zinc concentrate and pyrite. Specifically, zinc concentrate and pyrite are mixed and subjected to fluidized bed roasting, followed by holding at 500-700℃ for 30-120 minutes. Oxygen or air is introduced during roasting and holding. The roasted ore is leached under low-acid conditions to obtain zinc sulfate leachate, which is then incorporated into the hydrometallurgical zinc smelting process. This invention utilizes pyrite in the fluidized bed roasting process of zinc concentrate to promote its oxidation through a synergistic reaction. The sulfur dioxide generated during the synergistic reaction is used to produce acid, and the associated valuable metals in the pyrite are recovered in the zinc smelting process. This method effectively improves the oxidation rate of zinc concentrate and effectively decomposes zinc ferrite. Neutral and weak acid leaching of the roasted ore results in minimal equipment corrosion, eliminates the iron slag produced in hydrometallurgical zinc smelting, and features a short process flow, simple operation, and environmental friendliness.
[0006] In summary, existing pyrite-type smelters employing oxidative roasting processes inevitably produce sulfur dioxide, thus necessitating the co-production of sulfuric acid. However, sulfuric acid is difficult to sell in many regions, and its storage and transportation pose significant challenges to the site selection of pyrite-type smelters. Furthermore, even after flue gas purification, a certain amount of SO2 is still emitted, making environmental protection a major obstacle for existing pyrite-type smelters. Summary of the Invention
[0007] The present invention aims to provide an apparatus and method for the clean utilization of multiple components of pyrite-type minerals.
[0008] A device for the clean utilization of multiple components of pyrite-type minerals includes: a multi-hearth furnace reactor, which consists of a multi-hearth furnace body, a spiral feed inlet, a gas inlet, a multi-layer material platform, a multi-hearth furnace central shaft, a multi-hearth furnace rake, a multi-hearth furnace spiral discharge outlet, and a flue gas outlet. The spiral feed / discharge inlet and gas inlet are respectively located at the top and bottom of the multi-hearth furnace reactor and symmetrically on both sides of the central axis. The spiral feed inlet, gas inlet, spiral discharge outlet, and flue gas outlet are connected to the multi-hearth furnace body through sealing flanges. Depending on the actual needs of the reaction process, 2-N material platforms are used, with a distance of 20-30mm between them. Multiple material platforms are connected to the central axis of the multi-hearth furnace via rotating bearings, with the included angle continuously adjustable within the range of 0° to 5°. The central axis of the multi-hearth furnace is located at the center of the furnace body. The multi-hearth furnace rake is connected to the central axis via rotating bearings. The rake arm of the rake is continuously adjustable within the range of 0° to 5°, with rake teeth evenly distributed on the rake arm. The length of the rake teeth gradually increases. When the included angle between the rake arm and the central axis is 5°, all rake teeth are on the same plane. The multi-hearth furnace rake rotates and moves the material layer under the drive of the central axis.
[0009] In a multi-hearth furnace reactor, the solid and gas phases react in a countercurrent manner during heat exchange. Material enters the multi-hearth furnace through a spiral feed inlet at the top. Driven by a rotating multi-hearth furnace rake and downward-sloping multi-layered material platforms, the material moves from the upper platform to the lower platform and is finally discharged through a spiral outlet at the bottom of the furnace. Gas enters through the bottom gas inlet and exits through the top flue gas outlet. The countercurrent reaction between the solid and gas phases in the multi-hearth furnace, compared to conventional gas-solid reactors, achieves a heat utilization rate of over 80% and a hydrogen utilization efficiency of over 99%. The multi-layered material platforms and the rake arms of the multi-hearth furnace rake are detachable and can be added or removed according to the feeding conditions.
[0010] A method for the clean utilization of multiple components of pyrite-type minerals, implemented using the aforementioned apparatus, includes the following steps:
[0011] Step 1: Mixing ingredients
[0012] Mix the pyrite-type minerals and basic oxides evenly;
[0013] Step 2: Base hydrogen reduction
[0014] Pyrite-type minerals, basic oxides and hydrogen react in a multi-hearth furnace reactor, where the iron component in pyrite is reduced to elemental iron powder and the sulfur component is converted into basic sulfides.
[0015] Step 3: Solid-phase oxidation
[0016] The material obtained after the basic hydrogen reduction reaction is oxidized using its own residual heat.
[0017] Step 4: Magnetic separation
[0018] The material obtained after the reaction is separated by magnetic separation to recover elemental iron powder and basic sulfate.
[0019] In step 1, the pyrite is one of pyrite, marcasite, or pyrrhotite.
[0020] In step 1, the amount of alkaline oxide added is calculated as 1 to 3 times the stoichiometric coefficient of sulfur in the alkaline metal and pyrite-type minerals in the basic hydrogen reduction reaction, and is converted into the amount of alkaline oxide added.
[0021] In step 1, the alkaline oxide is one or more of calcium-based compounds, sodium-based compounds, and potassium-based compounds.
[0022] In step 2, the hydrogen reduction reaction is carried out at a temperature of 400℃ to 900℃ for 10 min to 120 min. The iron component in pyrite is reduced to elemental iron powder, and the sulfur component is converted into basic sulfides.
[0023] In step 3, the basic sulfides in the solid slag produced after the basic hydrogen reduction reaction are oxidized by their own residual heat to obtain basic sulfates. The temperature of the solid slag is maintained at 50℃~200℃, and the oxidation time is 10min~120min. The S in the solid slag... 2- Content ≤0.1%.
[0024] In step 4, the material obtained after the reaction is separated and the elemental iron powder is recovered by magnetic separation. The magnetic separation intensity is 0.1 to 1T, and the iron recovery rate is greater than 95%.
[0025] This invention discloses a method for the clean utilization of multiple components of pyrite-type minerals. Taking calcium oxide as an example, pyrite is reduced to metallic iron powder and calcium sulfide through a basic hydrogen reduction reaction. Elemental iron is recovered by magnetic separation, and calcium sulfide is oxidized at low temperature to prepare calcium sulfate. The chemical reaction formulas for the reaction process include:
[0026] Taking FeS2 as an example, the hydrogen reduction process:
[0027] FeS2+2CaO+2H2(g)=Fe+2CaS+2H2O(g)
[0028] Calcium sulfide conversion process
[0029] CaS + 2O₂(g) = CaSO₄
[0030] The apparatus and method for multi-element utilization by pyrite basic hydrogen reduction according to the present invention have the following advantages compared with the prior art:
[0031] (1) It eliminates SO2 flue gas pollution and sulfuric acid treatment problems. This invention uses a basic hydrogen reduction reaction. The reduction process does not produce SO2. Sulfur is converted into sulfides and enters the solid phase. After low-temperature oxidation, sulfate is generated, which achieves the purpose of sulfur fixation and solves the problems of flue gas pollution and sulfuric acid treatment in smelters.
[0032] (2) The metallic components in pyrite are effectively utilized. This invention uses a basic hydrogen reduction reaction to reduce the metallic components in pyrite to elemental metals, thereby increasing the utilization value of the iron component in pyrite;
[0033] (3) The present invention uses a multi-hearth furnace reactor, which has the following advantages: compared with conventional multi-hearth furnace reactors, it increases the running speed of solid materials by 50%, increases the reaction efficiency by 50%, achieves a system heat utilization rate of over 80%, and a hydrogen utilization efficiency of over 99%. Attached Figure Description
[0034] Figure 1 A schematic diagram of the process flow for a method of multi-element utilization by reducing pyrite with basic hydrogen;
[0035] Figure 2This is a schematic diagram of a multi-hearth furnace reactor; in the diagram, 1 - spiral feed inlet, 2 - flue gas outlet, 3 - multi-hearth furnace rake feeder, 4 - multi-layer material platform, 5 - gas inlet, 6 - multi-hearth furnace spiral discharge outlet, 7 - multi-hearth furnace central shaft, and 8 - multi-hearth furnace body. Detailed Implementation
[0036] The present invention will be further described in detail below with reference to the embodiments.
[0037] The pyrite-type mineral used in the embodiments of the present invention is pyrite, whose main components are Fe-46.75%, S-43.26%, and the balance being other components.
[0038] Example 1
[0039] An apparatus for the clean utilization of multiple components of pyrite-type minerals includes: a multi-hearth furnace reactor, such as... Figure 2 As shown, it consists of a multi-hearth furnace body 8, a spiral feed inlet 1, a gas inlet 5, a multi-layer material platform 4, a multi-hearth furnace central shaft 7, a multi-hearth furnace rake feeder 3, a multi-hearth furnace spiral discharge outlet 6, and a flue gas outlet 2. The spiral feed / discharge port and the gas inlet / outlet are respectively located at the top and bottom of the multi-hearth furnace reactor and symmetrically on both sides of the central axis. The spiral feed port 1, gas inlet 5, spiral discharge port 6, and flue gas outlet 2 are connected to the multi-hearth furnace body 8 through sealing flanges. According to the actual needs of the reaction process, 11 material platforms are used, with a distance of 25mm between the material platforms. The multi-layer material platform 4 is connected to the central axis 7 of the multi-hearth furnace through a rotating bearing, and the included angle is continuously adjustable within the range of 0° to 5°. The central axis 7 of the multi-hearth furnace is located at the center of the multi-hearth furnace body. The multi-hearth furnace rake 3 is connected to the central axis 7 of the multi-hearth furnace through a rotating bearing. The rake arm of the multi-hearth furnace rake 3 is continuously adjustable within the range of 0° to 5°. The rake teeth are evenly distributed on the rake arm, and the length of the rake teeth gradually increases. When the included angle between the rake arm of the multi-hearth furnace rake 3 and the central axis is 5°, all the rake teeth are on the same plane. The multi-hearth furnace rake 3 rotates and moves the material layer under the drive of the central axis.
[0040] In the multi-hearth furnace reactor, the solid and gas phases react in a countercurrent manner during the heat exchange process. The material enters the multi-hearth furnace through the spiral feed inlet 1 at the top of the furnace body. Under the action of the rotating multi-hearth furnace rake feeder 3 and the downwardly inclined multi-layer material platform 4, the material moves from the upper material platform to the lower material platform and is finally discharged from the spiral discharge outlet 6 at the bottom of the furnace body. The gas enters through the bottom gas inlet 5 and is discharged through the top flue gas outlet 2. The solid and gas phases react in the multi-hearth furnace in a countercurrent manner.
[0041] A method for the clean utilization of multiple components of pyrite-type minerals, implemented using the aforementioned apparatus, such as... Figure 1 As shown, the specific operation steps are as follows:
[0042] (1) Mix pyrite and calcium oxide in a certain proportion, and add calcium oxide in an amount equal to 1 times the stoichiometric coefficient of calcium and sulfur in the basic hydrogen reduction reaction of pyrite.
[0043] (2) Pyrite, basic oxides and hydrogen are carried out in a multi-hearth furnace to reduce the metal components in pyrite to metal elements and convert sulfur into calcium sulfide. The hydrogen reduction reaction temperature is 400℃ and the reaction time is 10min.
[0044] (3) Calcium sulfide in the solid slag obtained from the multi-hearth furnace is oxidized by its own preheating to obtain calcium sulfate. The solid slag temperature is 50℃, and the oxidation time is 120 min. After the reaction is completed, the S in the separated material is... 2- The content is 0.1%;
[0045] (4) The material obtained after solid-phase oxidation is subjected to magnetic separation to recover the metal elements. The recovery rate of iron in pyrite is 96%.
[0046] Example 2
[0047] A method for the clean utilization of multiple components of pyrite-type minerals, implemented using the apparatus of claim 1, comprises the following specific steps:
[0048] (1) Mix pyrite and sodium oxide in a certain proportion, and add sodium oxide in an amount that is twice the stoichiometric coefficient of sodium and sulfur in the basic hydrogen reduction reaction of pyrite.
[0049] (2) Pyrite, basic oxides and hydrogen are carried out in a multi-hearth furnace to reduce the metal components in pyrite to metal elements and convert sulfur into sodium sulfide. The hydrogen reduction reaction temperature is 500℃ and the reaction time is 120min.
[0050] (3) Calcium sulfide in the solid slag obtained from the multi-hearth furnace is oxidized by its own preheating to obtain calcium sulfate. The solid slag temperature is 200℃, and the oxidation time is 10 min. After the reaction is completed, the S in the separated material is... 2- The content is 0.08%;
[0051] (4) The material obtained after solid-phase oxidation is subjected to magnetic separation to recover the metal elements. The recovery rate of iron in pyrite is 95%.
[0052] Example 3
[0053] A method for the clean utilization of multiple components of pyrite-type minerals, implemented using the apparatus of claim 1, comprises the following specific steps:
[0054] (1) Mix pyrite and potassium oxide in a certain proportion, and add potassium oxide in an amount that is 3 times the stoichiometric coefficient of calcium and sulfur in the basic hydrogen reduction reaction of pyrite.
[0055] (2) Pyrite, basic oxides and hydrogen are carried out in a multi-hearth furnace to reduce the metal components in pyrite to metal elements and convert sulfur into potassium sulfide. The hydrogen reduction reaction temperature is 900℃ and the reaction time is 50min.
[0056] (3) Calcium sulfide in the solid slag obtained from the multi-hearth furnace is oxidized by its own preheating to obtain calcium sulfate. The solid slag temperature is 100℃, and the oxidation time is 60 min. After the reaction is completed, the S in the separated material is... 2- The content is 0.07%;
[0057] (4) The material obtained after solid-phase oxidation is subjected to magnetic separation to recover the metal elements. The recovery rate of iron in pyrite is 96%.
[0058] Example 4
[0059] A method for the clean utilization of multiple components of pyrite-type minerals, implemented using the apparatus of claim 1, comprises the following specific steps:
[0060] (1) Mix pyrite and potassium oxide in a certain proportion, and add potassium oxide in an amount that is 1.5 times the stoichiometric coefficient of calcium and sulfur in the basic hydrogen reduction reaction of pyrite.
[0061] (2) Pyrite, basic oxides and hydrogen are carried out in a multi-hearth furnace to reduce the metal components in pyrite to metal elements and convert sulfur into potassium sulfide. The hydrogen reduction reaction temperature is 800℃ and the reaction time is 60min.
[0062] (3) Calcium sulfide in the solid slag obtained from the multi-hearth furnace is oxidized by its own preheating to obtain calcium sulfate. The solid slag temperature is 150℃, and the oxidation time is 100 min. After the reaction is completed, the S in the separated material is... 2- The content is 0.06%;
[0063] (4) The material obtained after solid-phase oxidation is subjected to magnetic separation to recover the metal elements. The recovery rate of iron in pyrite is 97%.
Claims
1. A device for the clean utilization of multiple components of pyrite-type minerals, characterized in that, The reactor includes a multi-hearth furnace reactor, which consists of a multi-hearth furnace body (8), a spiral feed inlet (1), a gas inlet (5), a multi-layer material platform (4), a multi-hearth furnace central axis (7), a multi-hearth furnace rake (3), a multi-hearth furnace spiral discharge outlet (6), and a flue gas outlet (2); wherein, the spiral feed inlet / discharge inlet and the gas inlet / outlet are respectively located at the top and bottom of the multi-hearth furnace reactor and symmetrically on both sides of the central axis, and the spiral feed inlet (1), the gas inlet (5), and the multi-hearth furnace spiral discharge outlet (6) are located on both sides of the central axis. The flue gas outlet (2) is connected to the multi-hearth furnace body (8) through a sealing flange; according to the actual needs of the reaction process, two or more material platforms are used, and the multi-layer material platform (4) is connected to the multi-hearth furnace central shaft (7) through a rotating bearing; the multi-hearth furnace central shaft (7) is placed in the center of the multi-hearth furnace body (8), and the multi-hearth furnace rake (3) is connected to the multi-hearth furnace central shaft (7) through a rotating bearing. Rake teeth are evenly distributed on the rake arm, and the length of the rake teeth gradually increases. The multi-hearth furnace rake rotates and moves the material layer under the drive of the central shaft. The distance between material platforms is 20~30mm; the multi-layer material platform (4) is connected to the central shaft (7) of the multi-hearth furnace through a rotating bearing, and the included angle is continuously adjustable in the range of 0°~5°; the rake arm of the multi-hearth furnace rake is continuously adjustable in the range of 0°~5°, and when the included angle between the rake arm of the multi-hearth furnace rake and the central shaft is 5°, all rake teeth are on the same plane; In the multi-hearth furnace reactor, the solid phase and gas phase react in a countercurrent manner during the heat exchange process. The material enters the multi-hearth furnace through the spiral feed port (1) at the top of the furnace body. Under the action of the rotating multi-hearth furnace rake (3) and the downward-sloping multi-layer material platform (4), the material moves from the upper material platform to the lower material platform and is finally discharged from the spiral discharge port at the bottom of the furnace body. The gas enters through the bottom gas inlet (5) and is discharged through the top flue gas outlet (2). The solid phase and gas phase react in the multi-hearth furnace in a countercurrent manner. The rake arm of the multi-layer material platform (4) and the multi-hearth furnace rake can be disassembled and increased or decreased according to the feeding situation.
2. A method for the clean utilization of multiple components of pyrite-type minerals, implemented using the apparatus described in claim 1, characterized in that, Follow these steps: Step 1: Mixing ingredients Mix the pyrite-type minerals and basic oxides evenly; Step 2: Base hydrogen reduction Pyrite-type minerals, basic oxides, and hydrogen react in a multi-hearth furnace reactor. The iron component in pyrite is reduced to elemental iron powder, and the sulfur component is converted into basic sulfides. The hydrogen reduction reaction is carried out at a temperature of 400℃ to 900℃ and a reaction time of 10 min to 120 min. Step 3: Solid-phase oxidation The basic sulfides in the solid slag produced after the basic hydrogen reduction reaction are oxidized using their own residual heat to obtain basic sulfates; the temperature of the solid slag is 50℃~200℃, the oxidation reaction time is 10min~120min, and the sulfur content in the solid slag is... 2- Content ≤0.1%; Step 4: Magnetic separation The material obtained after the reaction is separated by magnetic separation to recover elemental iron powder and basic sulfate.
3. The method for clean utilization of multi-component pyrite-type minerals according to claim 2, characterized in that, In step 1, the pyrite is one of pyrite, marcasite, and pyrrhotite; the amount of alkaline oxide added is calculated as 1 to 3 times the stoichiometric coefficient of the alkaline metal and sulfur in the pyrite-type mineral in the basic hydrogen reduction reaction, and is converted into the amount of alkaline oxide added; the alkaline oxide is one or more of calcium-based compounds, sodium-based compounds, and potassium-based compounds.
Citation Information
Patent Citations
Cooperative roasting method for zinc concentrate and iron pyrite
CN105331801A
Method for producing sulfur-containing gas, calcium carbonate and iron ore concentrate from ardealite and pyrite
CN111118280A
A method for gas recycling and utilization in cobalt production process
CN115747478B
Method for utilizing comprehensive resource of sulfur-containing solid waste
CN101570341A
System and method for treating oil residue gasification filter cake and separating metal oxide
CN116146988A