Preparation method of lignin-based environmentally friendly stretchable photocurable resin

Through the preparation of lignin-based environmentally friendly stretchable photo-curable resin, the dual network structure of imidazole-modified-polysiloxane and acrylic acid-modified-lignin, combined with ZnCl2, solves the problem of light in flexible-stretchable electronic devices. The deformation performance and self-healing problem of cured glue enable efficient light curing and environmental protection.

CN118027310BActive Publication Date: 2024-10-29SUMII TECH (SHENZHEN) CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410227197.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2024-10-29
Estimated Expiration
2044-02-29

AI Technical Summary

Technical Problem

Existing photocurable adhesives lack excellent deformation properties and self-healing functions in flexible-stretchable electronic devices, making it difficult to meet the efficient curing needs of flexible displays, flexible lighting, and flexible sensing devices.

Method used

Using the preparation method of lignin-based environmentally friendly stretchable photo-curable resin, the dual network structure of imidazole-modified-polysiloxane and acrylic acid-modified-polysiloxane polymers and lignin is combined with ZnCl2 to form a dual reinforced structure. , to achieve UV curing.

Benefits of technology

It gives the light-cured resin excellent stretchability and self-healing functions, improving its breaking strength and elongation while ensuring environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118027310B_ABST
    Figure CN118027310B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a lignin-based environment-friendly stretchable photocurable resin, which specifically comprises the following steps: step 1, preparing an imidazole-modified polysiloxane polymer; step 2, preparing an acrylic acid-modified polysiloxane polymer; step 3, preparing an acrylic acid-modified lignin; step 4, preparing an imidazole-modified lignin; step 5, preparing a photocurable resin according to the products obtained from step 1 to step 4. The present invention constructs an acrylic acid-modified polysiloxane polymer and an acrylic acid-modified lignin as stretchable, ultraviolet light-curable active components, and imidazole-modified lignin and imidazole-modified polysiloxane polymer as stretchable, self-repairing active components. The photocurable resin prepared by the method has the functions of stretchability and self-repairing, and can be used in flexible stretchable electronic devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparing photocurable resins for flexible electronic devices, and relates to a method for preparing a lignin-based environment-friendly stretchable photocurable resin. Background Art

[0002] Photocuring adhesives have important applications in the fields of coatings, inks, paints, coating protection, adhesives, electronic devices, etc., involving many areas of people's livelihood. It is precisely because of the wide use of photocuring adhesives and as people have put forward higher requirements for the safety of photocuring adhesives, there is an urgent need to improve the environmental protection of photocuring adhesives. In addition, UV light-curing adhesives have always been mainly pursued for their waterproof, oil-proof, friction-resistant, efficient curing, adhesion, low V℃, low residue and other properties, and a series of photocuring materials have been developed around these performance requirements. With the development of flexible-stretchable electronic devices such as flexible displays, flexible lighting, and flexible sensor devices, photocurable functional resins also need to have compatibility in the selection process, giving them excellent deformation properties and achieving stretchability. Therefore, it is necessary to study a photocurable resin that can achieve stretchability. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a lignin-based environmentally friendly stretchable photocurable resin. The photocurable resin prepared by the method has stretchable and self-repairing functions and can be used in flexible-stretchable electronic devices.

[0004] The technical solution adopted by the present invention is a method for preparing a lignin-based environmentally friendly stretchable light-curable resin, which specifically comprises the following steps:

[0005] Step 1, preparing imidazole-modified polysiloxane polymer;

[0006] Step 2, preparing acrylic acid-modified polysiloxane polymer;

[0007] Step 3, preparing acrylic acid-modified lignin;

[0008] Step 4, preparing imidazole-modified lignin;

[0009] Step 5, preparing a photocurable resin according to the products obtained in steps 1 to 4.

[0010] The present invention is also characterized in that:

[0011] The specific process of step 1 is:

[0012] Take 10g-20g of bis(hydroxyalkyl)-terminated polydimethylsiloxane and 1mL-2mL of 3-(1H-imidazole-1-yl)propionic acid and dissolve them in 10mL-20mL of dimethyl sulfoxide solution, stir for 30min-60min, then add 1mL-2mL of concentrated sulfuric acid, heat the reaction system to 80℃-90℃ and continue stirring for 12h-15h, cool to room temperature after the reaction, pour the reaction solution into 200mL-400mL of deionized water, collect the solid precipitate, and obtain imidazole-modified polysiloxane polymer material.

[0013] The specific process of step 2 is:

[0014] Take 10g-20g of bis(hydroxyalkyl)-terminated polydimethylsiloxane and 1mL-2mL of acrylic acid respectively, dissolve them in 10mL-20mL of dimethyl sulfoxide solution, stir for 30min-60min, then add 1mL-2mL of concentrated sulfuric acid, heat the reaction system to 80℃-90℃ and continue stirring for 12h-15h, cool to room temperature after the reaction is completed, pour the reaction solution into 200mL-400mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified polysiloxane polymer material.

[0015] The specific process of step 3 is:

[0016] Take 10g-20g of alkali lignin and 1mL-2mL of glycidyl acrylate, add them to 15mL-30mL of N,N-dimethylformamide solution, stir at room temperature for 5min-10min, put the reaction solution into a microwave reactor and heat it to 60℃-70℃ for reaction for 1h~2h, cool to room temperature after the reaction, pour the reaction solution into 100mL-200mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified lignin.

[0017] The specific process of step 4 is:

[0018] Step 4.1, add 1 mL-2 mL of 3-(1H-imidazol-1-yl)propionic acid to 1 mL-2 mL of thionyl chloride solution, stir at room temperature for 5 h-10 h, after the reaction is completed, remove excess thionyl chloride by rotary evaporation at 60° C.-120° C., and add the remaining solution after rotary evaporation to 10 mL-20 mL of dimethyl sulfoxide solution as a standby solution;

[0019] Step 4.2, take 10g-20g of alkali lignin and 0.1g-0.2g of sodium hydroxide and disperse them in 10mL-20mL of dimethyl sulfoxide solution, stir and disperse at room temperature for 30min-60min, then mix with the reserved solution in step 4.1, and continue stirring at 60℃-100℃ for 1h-2h to obtain.

[0020] The specific process of step 5 is:

[0021] Take 0.1g-0.2g of imidazole-modified polysiloxane polymer, 0.1g-0.2g of acrylic acid-modified polysiloxane polymer, 0.1g-0.2g of acrylic acid-modified lignin, 0.1g-0.2g of imidazole-modified lignin, 0.01g-0.05g of ZnCl2 and 5mL-10mL of vinyl tris(trimethylsiloxy)silane respectively, stir evenly at room temperature, pour the mixed solution into a polytetrafluoroethylene mold, use 365nm wavelength ultraviolet light, power 360mW / cm 2 -720mW / cm 2 The mixed solution is cured by a UV curing apparatus to obtain the product.

[0022] The beneficial effect of the present invention is that a double network of lignin and polysiloxane and a stretchable and self-repairing UV-curable resin with double reinforcement structure characteristics are constructed by using lignin as a raw material, which not only gives the light-curable resin a long stretchable length and strong fracture strength, but also gives it a self-repairing function. The main structure is formed by the polymerization of acrylic acid-modified-lignin and acrylic acid-modified-polysiloxane polymers, and the guest structure is formed by the polymerization of imidazole-modified-lignin and imidazole-modified-polysiloxane polymers, forming a double network structure, and the active sites of imidazole and acrylic acid are both in the main structure and the guest structure to form a double reinforcement structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 These are the tensile-strain test results of the photocured samples of Example 1, Comparative Example 1 and Comparative Example 3 and their self-repaired samples in the preparation method of the lignin-based environmentally friendly stretchable photocurable resin of the present invention. DETAILED DESCRIPTION

[0024] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0025] The method for preparing the lignin-based environment-friendly stretchable photocurable resin of the present invention specifically comprises the following steps:

[0026] Step 1, preparation of imidazole-modified polysiloxane polymer, specifically:

[0027] Take 10-20g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 2000-5600Da) and 1-2mL of 3-(1H-imidazole-1-yl) propionic acid and dissolve them in 10-20mL of dimethyl sulfoxide solution, and stir for 30-60min. Then add 1mL-2mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 80℃-90℃ and continue stirring for 12h-15h. After the reaction is completed, cool to room temperature, pour the reaction solution into 200mL-400mL of deionized water, collect the solid precipitate, and obtain imidazole-modified polysiloxane polymer material.

[0028] Step 2, preparation of acrylic acid-modified polysiloxane polymer, specifically:

[0029] Take 10-20g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 2000-5600Da), and 1-2mL of acrylic acid, dissolve in 10-20mL of dimethyl sulfoxide solution, and stir for 30-60min. Then add 1mL-2mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 80℃-90℃ and continue stirring for 12h-15h. After the reaction is completed, cool to room temperature, pour the reaction solution into 200mL-400mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified polysiloxane polymer material.

[0030] Step 3, preparation of acrylic acid-modified lignin, specifically:

[0031] Take 10-20g of alkali lignin and 1-2mL of glycidyl acrylate, add them to 15-30mL of N,N-dimethylformamide solution, and stir at room temperature for 5-10min. Put the reaction solution into a microwave reactor and heat it to 60-70℃ for 1h-2h. After the reaction is completed, cool it to room temperature, pour the reaction solution into 100-200mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified lignin.

[0032] Step 4, preparation of imidazole-modified lignin, specifically:

[0033] Take 1-2mL of 3-(1H-imidazole-1-yl) propionic acid, add it to 1-2mL of dichlorothionyl solution, and stir at room temperature for 5-10h. After the reaction is completed, remove the excess dichlorothionyl by rotary evaporation at 60-120℃. Add the remaining solution after rotary evaporation to 10-20mL of dimethyl sulfoxide solution for standby use. Take 10-20g of alkali lignin and 0.1-0.2g of sodium hydroxide and disperse them in 10-20mL of dimethyl sulfoxide solution, stir and disperse at room temperature for 30-60min, then mix it with the standby solution, and continue stirring at 60-100℃ for 1-2h to obtain imidazole-modified lignin.

[0034] Step 5, preparation and curing of light-curable resin, specifically:

[0035] Take 0.1-0.2g of imidazole-modified-polysiloxane polymer, 0.1-0.2g of acrylic acid-modified-polysiloxane polymer, 0.1-0.2g of acrylic acid-modified-lignin, 0.1-0.2g of imidazole-modified-lignin, 0.01-0.05g of ZnCl2 and 5-10mL of vinyl tris(trimethylsiloxy)silane, stir evenly at room temperature, and pour the mixed solution into a polytetrafluoroethylene mold with a size of 5cm long, 2cm wide and 0.5cm high. Use 365nm wavelength ultraviolet light and 360-720mW / cm 2 The mixed solution is cured by a UV curing device.

[0036] Example 1

[0037] Step 1, preparation of imidazole-modified polysiloxane polymer, specifically:

[0038] Take 10g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 2000Da) and 1mL of 3-(1H-imidazole-1-yl)propionic acid and dissolve them in 10mL of dimethyl sulfoxide solution and stir for 30min. Then add 2mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 80℃ and continue stirring for 12h. After the reaction is completed, cool to room temperature, pour the reaction solution into 200mL of deionized water, collect the solid precipitate, and obtain imidazole-modified polysiloxane polymer material.

[0039] Step 2, preparation of acrylic acid-modified polysiloxane polymer, specifically:

[0040] Take 10g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 2000Da) and 1mL of acrylic acid and dissolve them in 10mL of dimethyl sulfoxide solution and stir for 30min. Then add 2mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 80℃ and continue stirring for 12h. After the reaction is completed, cool to room temperature, pour the reaction solution into 200mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified polysiloxane polymer material.

[0041] Step 3, preparation of acrylic acid-modified lignin, specifically:

[0042] Take 10g of alkali lignin and 1mL of glycidyl acrylate, add them to 15mL of N,N-dimethylformamide solution, and stir at room temperature for 5min. Put the reaction solution into a microwave reactor and heat it to 60℃ for 1h. After the reaction is completed, cool it to room temperature, pour the reaction mixture into 100mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified lignin.

[0043] Step 4, preparation of imidazole-modified lignin, specifically:

[0044] Take 1mL of 3-(1H-imidazole-1-yl)propionic acid, add it to 1mL of dichlorothionyl solution, and stir at room temperature for 5h. After the reaction is completed, remove the excess dichlorothionyl by rotary evaporation at 60℃. Add the remaining solution after rotary evaporation to 10mL of dimethyl sulfoxide solution for later use. Take 10g of alkali lignin and 0.1g of sodium hydroxide and disperse them in 10mL of dimethyl sulfoxide solution, stir and disperse at room temperature for 30min, then mix it with the reserved solution and continue stirring at 60℃ for 1h.

[0045] Step 5, preparation and curing of light-curable resin, specifically:

[0046] Take 0.1g of imidazole-modified-polysiloxane polymer, 0.1g of acrylic acid-modified-polysiloxane polymer, 0.1g of acrylic acid-modified-lignin, 0.1g of imidazole-modified-lignin, 0.01g of ZnCl2 and 5mL of vinyl tris(trimethylsiloxane)silane respectively, and stir evenly at room temperature. Pour the mixed solution into a polytetrafluoroethylene mold with a size of 5cm long, 2cm wide and 0.5cm high. Use ultraviolet light with a wavelength of 365nm and a power of 360mW / cm 2 The mixed solution is cured by a UV curing device.

[0047] Comparative Example 1 (imidazole-modified polysiloxane polymer was replaced with polysiloxane polymer, and the breaking strength and elongation of the photocurable adhesive were reduced)

[0048] 1. Preparation of acrylic acid-modified polysiloxane polymer

[0049] Take 10g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 2000Da) and 1mL of acrylic acid and dissolve them in 10mL of dimethyl sulfoxide solution and stir for 30min. Then add 2mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 80℃ and continue stirring for 12h. After the reaction is completed, cool to room temperature, pour the reaction solution into 200mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified polysiloxane polymer material.

[0050] 2. Preparation of acrylic acid-modified lignin

[0051] Take 10g of alkali lignin and 1mL of glycidyl acrylate, add them to 15mL of N,N-dimethylformamide solution, and stir at room temperature for 5min. Put the reaction solution into a microwave reactor and heat it to 60℃ for 1h. After the reaction is completed, cool it to room temperature, pour the reaction into 100mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified lignin.

[0052] 3. Preparation of Imidazole-modified Lignin

[0053] Take 1mL of 3-(1H-imidazole-1-yl)propionic acid, add it to 1mL of dichlorothionyl solution, and stir at room temperature for 5h. After the reaction is completed, remove the excess dichlorothionyl by rotary evaporation at 60℃. Add the remaining solution after rotary evaporation to 10mL of dimethyl sulfoxide solution for later use. Take 10g of alkali lignin and 0.1g of sodium hydroxide and disperse them in 10mL of dimethyl sulfoxide solution, stir and disperse at room temperature for 30min, then mix it with the reserved solution and continue stirring at 60℃ for 1-2h.

[0054] 4. Preparation and curing properties of light-curable resin

[0055] Take 0.1g polysiloxane polymer, 0.1g acrylic acid-modified polysiloxane polymer, 0.1g acrylic acid-modified lignin, 0.1g imidazole-modified lignin, 0.01g ZnCl2 and 5mL vinyl tris (trimethylsiloxy) silane, and stir evenly at room temperature. Pour the mixed solution into a polytetrafluoroethylene mold with a size of 5cm long x 2cm wide x 0.5cm high. Use a 365nm wavelength ultraviolet light with a power of 360mW / cm 2 The mixed solution is cured by a UV curing device.

[0056] Comparative Example 2 (When ZnCl2 is not added during the photocuring of the resin, the breaking strength and tensile elongation of the resin decrease after photocuring, and the resin cannot be self-repaired)

[0057] 1. Preparation of Imidazole-modified Polysiloxane Polymer

[0058] Take 10g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 2000Da) and 1mL of 3-(1H-imidazole-1-yl)propionic acid and dissolve them in 10mL of dimethyl sulfoxide solution and stir for 30min. Then add 2mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 80℃ and continue stirring for 12h. After the reaction is completed, cool to room temperature, pour the reaction solution into 200mL of deionized water, collect the solid precipitate, and obtain imidazole-modified polysiloxane polymer material.

[0059] 2. Preparation of acrylic acid-modified polysiloxane polymer

[0060] Take 10g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 2000Da) and 1mL of acrylic acid and dissolve them in 10mL of dimethyl sulfoxide solution and stir for 30min. Then add 2mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 80℃ and continue stirring for 12h. After the reaction is completed, cool to room temperature, pour the reaction solution into 200mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified polysiloxane polymer material.

[0061] 3. Preparation of acrylic acid-modified lignin

[0062] Take 10g of alkali lignin and 1mL of glycidyl acrylate, add them to 15mL of N,N-dimethylformamide solution, and stir at room temperature for 5min. Put the reaction solution into a microwave reactor and heat it to 60℃ for 1h. After the reaction is completed, cool it to room temperature, pour the reaction into 100mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified lignin.

[0063] 4. Preparation of Imidazole-modified Lignin

[0064] Take 1 mL of 3-(1H-imidazole-1-yl) propionic acid, add it to 1 mL of thionyl chloride solution, and stir at room temperature for 5 hours. After the reaction is completed, remove the excess thionyl chloride by rotary evaporation at 60°C. Add the remaining solution after rotary evaporation to 10 mL of dimethyl sulfoxide solution for later use. Take 10 g of alkali lignin and 0.1 g of sodium hydroxide and disperse them in 10 mL of dimethyl sulfoxide solution, stir and disperse at room temperature for 30 minutes, then mix it with the reserved solution and stir at 60°C. ℃ Stirring was continued for 1 h.

[0065] 5. Preparation and curing of light-curable resin

[0066] Take 0.1g of imidazole-modified polysiloxane polymer, 0.1g of acrylic acid-modified polysiloxane polymer, 0.1g of acrylic acid-modified lignin, 0.1g of imidazole-modified lignin, and 5mL of vinyl tris(trimethylsiloxane)silane, and stir evenly at room temperature. Pour the mixed solution into a polytetrafluoroethylene mold with a size of 5cm long, 2cm wide, and 0.5cm high. Use a 365nm wavelength UV and a power of 360mW / cm 2 The mixed solution is cured by a UV curing device.

[0067] Comparative Example 3 (Acrylic acid-modified lignin was replaced with unmodified alkali lignin, and the breaking strength of the resin decreased after light curing)

[0068] 1. Preparation of Imidazole-modified Polysiloxane Polymer

[0069] Take 10g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 2000Da) and 1mL of 3-(1H-imidazole-1-yl)propionic acid and dissolve them in 10mL of dimethyl sulfoxide solution and stir for 30min. Then add 2mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 80℃ and continue stirring for 12h. After the reaction is completed, cool to room temperature, pour the reaction solution into 200mL of deionized water, collect the solid precipitate, and obtain imidazole-modified polysiloxane polymer material.

[0070] 2. Preparation of acrylic acid-modified polysiloxane polymer

[0071] Take 10g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 2000Da) and 1mL of acrylic acid and dissolve them in 10mL of dimethyl sulfoxide solution and stir for 30min. Then add 2mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 80℃ and continue stirring for 12h. After the reaction is completed, cool to room temperature, pour the reaction solution into 200mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified polysiloxane polymer material.

[0072] 3. Preparation of Imidazole-modified Lignin

[0073] Take 1 mL of 3-(1H-imidazole-1-yl) propionic acid, add it to 1 mL of thionyl chloride solution, and stir at room temperature for 5 hours. After the reaction is completed, remove the excess thionyl chloride by rotary evaporation at 60°C. Add the remaining solution after rotary evaporation to 10 mL of dimethyl sulfoxide solution for later use. Take 10 g of alkali lignin and 0.1 g of sodium hydroxide and disperse them in 10 mL of dimethyl sulfoxide solution, stir and disperse at room temperature for 30 minutes, then mix it with the reserved solution and stir at 60°C. ℃ Stirring was continued for 1 h.

[0074] 4. Preparation and curing properties of light-curable resin

[0075] Take 0.1g of imidazole-modified polysiloxane polymer, 0.1g of acrylic acid-modified polysiloxane polymer, 0.1g of alkali lignin, 0.1g of imidazole-modified lignin, 0.01g of ZnCl2 and 5mL of vinyl tris(trimethylsiloxane)silane, and stir evenly at room temperature. Pour the mixed solution into a polytetrafluoroethylene mold with a size of 5cm long, 2cm wide and 0.5cm high. Use a 365nm wavelength ultraviolet light with a power of 360mW / cm 2 The mixed solution is cured by a UV curing device.

[0076] Test Results and Discussion

[0077] Table 1. Test results of tensile strain of Example 1, Comparative Examples 1-3 and their self-repaired

[0078]

[0079] like Figure 1 As shown in Table 1, Example 1 has a high breaking strength of 160 MPa and a breaking elongation of 80%. The reason is that acrylic acid-modified lignin and acrylic acid-modified polysiloxane polymers are polymerized to form a main structure, and imidazole-modified lignin and imidazole-modified polysiloxane polymers are polymerized to form a guest structure, forming a double network structure. At the same time, the active sites of imidazole and acrylic acid are both in the main structure and the guest structure to form a double reinforcement structure, giving it excellent mechanical properties. Thanks to Zn 2+ The photocured sample in Example 1 can be self-repaired by hot pressing again after being cut by a blade, and the fracture strength of the self-repaired sample can reach 130MPa and the fracture elongation can reach 68%.

[0080] In Comparative Example 1, imidazole-modified-polysiloxane polymer was replaced with polysiloxane polymer, and the breaking strength and elongation of the photocured sample were 132MPa and 52%, respectively. Although imidazole-modified-lignin and Zn2+ can also form guest structures and can form a double network structure with the main structure, this result is reduced compared with Example 1. The possible reason is that only imidazole-modified-lignin guest structures can be formed in the system, and imidazole-modified-polysiloxane polymer guest structures cannot be formed, and ultimately dual reinforcement cannot be formed. At the same time, due to the lack of imidazole-modified-polysiloxane polymer components, the reversible coordination bond between the imidazole structural unit and Zn2+ cannot be formed, so its elongation at break is significantly reduced.

[0081] Comparative Example 2 lacks Zn2+ ions. Therefore, neither imidazole-modified-polysiloxane polymer nor imidazole-lignin can form a reversible coordination bond with Zn2+, resulting in the formation of a single main structure of acrylic acid-modified-lignin and acrylic acid-modified-polysiloxane polymer polymerization in the photocured sample, and it is impossible to construct a double network and double reinforcement structure. The fracture strength and elongation at break of Comparative Example 3 are significantly reduced, only 84MPa and 56% respectively. Since the entire structure cannot form a reversible coordination bond, there is no self-repairing function under the same treatment conditions, and the test of its fracture strength and elongation at break cannot be completed.

[0082] In comparative example 3, after the acrylic acid-modified lignin was replaced with unmodified alkali lignin, the photocured sample only had a single main structure of acrylic acid-modified polysiloxane polymer. The advantage of polysiloxane is its excellent tensile properties. The elongation at break of the comparative example 3 photocured sample and its self-repaired sample were as high as 120% and 110%, respectively. The lack of olefinic acid-modified lignin in the main structure resulted in a sharp decrease in the breaking strength, which was only 36MPa and 27MPa.

[0083] Example 2

[0084] Step 1, preparation of imidazole-modified polysiloxane polymer, specifically:

[0085] Take 20g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 5600Da) and 2mL of 3-(1H-imidazole-1-yl) propionic acid and dissolve them in 20mL of dimethyl sulfoxide solution and stir for 60min. Then add 1mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 90℃ and continue stirring for 15h. After the reaction is completed, cool to room temperature, pour the reaction solution into 400mL of deionized water, collect the solid precipitate, and obtain imidazole-modified polysiloxane polymer material.

[0086] Step 2, preparation of acrylic acid-modified polysiloxane polymer, specifically:

[0087] Take 20g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 5600Da) and 2mL of acrylic acid and dissolve them in 20mL of dimethyl sulfoxide solution and stir for 60min. Then add 1mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 90℃ and continue stirring for 15h. After the reaction is completed, cool to room temperature, pour the reaction solution into 400mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified polysiloxane polymer material.

[0088] Step 3, preparation of acrylic acid-modified lignin, specifically:

[0089] Take 20g of alkali lignin and 2mL of glycidyl acrylate, add them to 30mL of N,N-dimethylformamide solution, and stir at room temperature for 10min. Put the reaction solution into a microwave reactor and heat it to 70℃ for 2h. After the reaction is completed, cool it to room temperature, pour the reaction mixture into 200mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified lignin.

[0090] Step 4, preparation of imidazole-modified lignin, specifically:

[0091] Take 2mL of 3-(1H-imidazole-1-yl)propionic acid, add it to 2mL of dichlorothionyl solution, and stir at room temperature for 10h. After the reaction is completed, remove the excess dichlorothionyl by rotary evaporation at 120℃. Add the remaining solution after rotary evaporation to 20mL of dimethyl sulfoxide solution for later use. Take 20g of alkali lignin and 0.2g of sodium hydroxide and disperse them in 20mL of dimethyl sulfoxide solution, stir and disperse at room temperature for 60min, then mix it with the reserve solution and continue stirring at 100℃ for 2h.

[0092] Step 5, preparation and curing of light-curable resin, specifically:

[0093] Take 0.2g of imidazole-modified-polysiloxane polymer, 0.2g of acrylic acid-modified-polysiloxane polymer, 0.2g of acrylic acid-modified-lignin, 0.2g of imidazole-modified-lignin, 0.05g of ZnCl2 and 10mL of vinyl tris(trimethylsiloxane)silane respectively, and stir evenly at room temperature. Pour the mixed solution into a polytetrafluoroethylene mold with a size of 5cm long, 2cm wide and 0.5cm high. Use a 365nm wavelength ultraviolet light with a power of 720mW / cm 2 The mixed solution is cured by a UV curing device.

[0094] Example 3

[0095] Step 1, preparation of imidazole-modified polysiloxane polymer, specifically:

[0096] Take 15g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 4000Da) and 1.5mL of 3-(1H-imidazole-1-yl) propionic acid and dissolve them in 15mL of dimethyl sulfoxide solution and stir for 50min. Then add 1.5mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 85℃ and continue stirring for 14h. After the reaction is completed, cool to room temperature, pour the reaction solution into 300mL of deionized water, collect the solid precipitate, and obtain imidazole-modified polysiloxane polymer material.

[0097] Step 2, preparation of acrylic acid-modified polysiloxane polymer, specifically:

[0098] Take 15g of bis(hydroxyalkyl)-terminated polydimethylsiloxane (molecular weight 4000Da) and 1.5mL of acrylic acid and dissolve them in 15mL of dimethyl sulfoxide solution and stir for 50min. Then add 1.5mL of concentrated sulfuric acid (98.3wt%) dropwise, heat the reaction system to 85℃ and continue stirring for 14h. After the reaction is completed, cool to room temperature, pour the reaction solution into 300mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified polysiloxane polymer material.

[0099] Step 3, preparation of acrylic acid-modified lignin, specifically:

[0100] Take 15g of alkali lignin and 1.5mL of glycidyl acrylate, add them to 20mL of N,N-dimethylformamide solution, and stir at room temperature for 8min. Put the reaction solution into a microwave reactor and heat it to 65℃ for 1.5h. After the reaction is completed, cool it to room temperature, pour the reaction mixture into 150mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified lignin.

[0101] Step 4, preparation of imidazole-modified lignin, specifically:

[0102] Take 1.5mL of 3-(1H-imidazole-1-yl)propionic acid, add it to 1.5mL of dichlorothionyl solution, and stir at room temperature for 8h. After the reaction is completed, remove the excess dichlorothionyl by rotary evaporation at 100℃. Add the remaining solution after rotary evaporation to 15mL of dimethyl sulfoxide solution for later use. Take 15g of alkali lignin and 0.15g of sodium hydroxide and disperse them in 15mL of dimethyl sulfoxide solution, stir and disperse at room temperature for 40min, then mix it with the standby solution and continue stirring at 80℃ for 1.5h.

[0103] Step 5, preparation and curing of light-curable resin, specifically:

[0104] Take 0.15g of imidazole-modified-polysiloxane polymer, 0.15g of acrylic acid-modified-polysiloxane polymer, 0.15g of acrylic acid-modified-lignin, 0.15g of imidazole-modified-lignin, 0.03g of ZnCl2 and 8mL of vinyl tris(trimethylsiloxane)silane respectively, and stir evenly at room temperature. Pour the mixed solution into a polytetrafluoroethylene mold with a size of 5cm long, 2cm wide and 0.5cm high. Use ultraviolet light with a wavelength of 365nm and a power of 480mW / cm 2 The mixed solution is cured by a UV curing device.

Claims

1. Preparation method of lignin-based environmentally friendly stretchable photocurable resin, Features: The specific steps include: Step 1, preparing imidazole-modified polysiloxane polymer; The specific process of step 1 is as follows: Take 10g-20g of bis(hydroxyalkyl)-terminated polydimethylsiloxane and 1mL-2mL of 3-(1H-imidazole-1-yl)propionic acid and dissolve them in 10mL-20mL of dimethyl sulfoxide solution, stir for 30min-60min, then add 1mL~2mL of concentrated sulfuric acid dropwise, heat the reaction system to 80℃~90℃ and continue stirring for 12h~15h, cool to room temperature after the reaction is completed, pour the reaction solution into 200mL-400mL of deionized water, collect the solid precipitate, and obtain imidazole-modified polysiloxane polymer material; Step 2, preparing acrylic acid-modified polysiloxane polymer; The specific process of step 2 is: 10g-20g of bis(hydroxyalkyl)-terminated polydimethylsiloxane and 1mL-2mL of acrylic acid are dissolved in 10mL-20mL of dimethyl sulfoxide solution, stirred for 30min-60min, and then 1mL-2mL of concentrated sulfuric acid is added dropwise, the reaction system is heated to 80℃~90℃ and stirred for 12h~15h, and after the reaction is completed, the temperature is cooled to room temperature, and the reaction solution is poured into 200mL-400mL of deionized water, and the solid precipitate is collected to obtain an acrylic acid-modified polysiloxane polymer material; Step 3, preparing acrylic acid-modified lignin; The specific process of step 3 is as follows: Take 10g-20g of alkali lignin and 1mL-2mL of glycidyl acrylate, add them to 15mL-30mL of N,N-dimethylformamide solution, stir at room temperature for 5 min-10 min, put the reaction solution into a microwave reactor and heat it to 60℃-70℃ for 1h~2h, cool to room temperature after the reaction, pour the reaction solution into 100mL-200mL of deionized water, collect the solid precipitate, and obtain acrylic acid-modified lignin; Step 4, preparing imidazole-modified lignin; The specific process of step 4 is as follows: Step 4.1, add 1 mL-2 mL of 3-(1H-imidazole-1-yl)propionic acid to 1 mL-2 mL of thionyl chloride solution, stir at room temperature for 5 h-10 h, after the reaction is completed, remove excess thionyl chloride by rotary evaporation at 60°C-120°C, and add the remaining solution after rotary evaporation to 10 mL-20 mL of dimethyl sulfoxide solution as a standby solution; Step 4.2, take 10g-20g of alkali lignin and 0.1g-0.2g of sodium hydroxide and disperse them in 10mL-20mL of dimethyl sulfoxide solution, stir and disperse at room temperature for 30min-60min, then mix with the reserved solution in step 4.1, and continue stirring at 60℃-100℃ for 1h-2h to obtain; Step 5, preparing a photocurable resin according to the products obtained from steps 1 to 4; The specific process of step 5 is as follows: Take 0.1g-0.2g of imidazole-modified polysiloxane polymer, 0.1g-0.2g of acrylic acid-modified polysiloxane polymer, 0.1g-0.2g of acrylic acid-modified lignin, 0.1g-0.2g of imidazole-modified lignin, 0.01g-0.05g of ZnCl 2 and 5mL-10mL of vinyl tris(trimethylsiloxy)silane, stir evenly at room temperature, pour the mixed solution into a polytetrafluoroethylene mold, and use a 365nm wavelength ultraviolet light with a power of 360mW / cm 2 -720mW / cm 2 The mixed solution is cured by a UV curing apparatus to obtain the product.

Citation Information

Patent Citations

  • Self-repairing polysiloxane elastomer based on strong and weak hydrogen bond interaction and preparation method thereof

    CN115819776A

  • Anti-ultraviolet UV adhesive and preparation method thereof

    CN117210193A

  • Method of making synthetic resin from lignin and an epoxide and resulting product

    US3149085A