Flame-retardant wear-resistant fiber fabric and preparation method thereof
By adding phosphorimide-containing polyester to polyester fibers and preparing flame-retardant and abrasion-resistant fibers using a specific process, the problem of insufficient flame retardancy and abrasion resistance of polyester fibers has been solved, and polyester fabrics with high strength and good flame retardant properties have been achieved.
Patent Information
- Application Number
- CN202411062280.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polyester fibers and their fabrics have poor flame retardancy and abrasion resistance.
Flame-retardant and abrasion-resistant fibers were prepared by adding phosphorimide-containing polyester to polyethylene terephthalate, and flame-retardant and abrasion-resistant polyester fabrics were prepared by using a melt spinning process with specific temperature and speed.
It improves the breaking strength and high temperature resistance of polyester fibers, enhances flame retardancy and abrasion resistance, and the limiting oxygen index of polyester fabrics reaches 26.5-29.8%, with a friction mass loss rate of less than 1.29%.
Smart Images

Figure BDA0004978296250000031 
Figure BDA0004978296250000041 
Figure BDA0004978296250000042
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyester fibers, and in particular relates to a flame-retardant and wear-resistant fiber fabric and a preparation method thereof. Background Art
[0002] Polyester fiber is made of polyethylene terephthalate as raw material through melt spinning, electrospinning and other processes. It is widely used in ropes, fabrics, textiles, etc. Improving the flame retardant, wear resistance, high temperature resistance and other properties of polyester fiber can expand the application range of polyester fiber, fabrics, etc. In the spinning process, adding functional additives to polyethylene terephthalate can give polyester fiber some unique properties.
[0003] Polyimide and its fiber products have high strength, high temperature resistance, and certain flame retardancy. They can be blended, modified, or blended with polyester, nylon and other fibers to obtain high-performance composite materials and fabric products. However, polyimide has poor compatibility with polyester. When blended with polyester, microphase separation is likely to occur between the two, resulting in structural defects in the fiber, which will affect the performance of polyester fibers and their fabric products. Summary of the invention
[0004] The invention solves the problem that the polyester fiber and the fabric thereof have poor flame retardancy and poor wear resistance.
[0005] The technical solution of the present invention is: a flame retardant and wear-resistant fiber, comprising 82-95 parts by weight of polyethylene terephthalate, 5-18 parts by weight of phosphorimide-containing polyester, and 0.2-0.5 parts by weight of antioxidant.
[0006] The preparation method of phosphorimide-containing polyester comprises the following steps: adding ethylene glycol, phosphorimide-containing benzoic acid monomer and p-toluenesulfonic acid into a reaction kettle, introducing nitrogen, carrying out polymerization reaction, cooling the material, filtering, washing with toluene and ethanol in sequence, and drying to obtain the phosphorimide-containing polyester.
[0007] Wherein, the molar ratio of ethylene glycol, phosphoramidite-containing benzoic acid monomer and p-toluenesulfonic acid is (1.4-1.6):1:(0.013-0.018).
[0008] The polymerization reaction temperature is 160-180°C and the reaction time is 5-10h.
[0009] Wherein, the preparation method of phosphorimide-containing benzoic acid monomer is:
[0010] (1) At 5-10° C., water, 4-acetaminophenol, sodium carbonate, and spirocyclic phosphate dichloride in a molar ratio of (1.9-2.1):(0.2-0.3):1 are added to a reaction flask, and the mixture is stirred for reaction for 4-8 hours. Then, sodium hydroxide is added, and the temperature is raised to 80-90° C., and the reaction is carried out for 10-18 hours. Ethyl acetate is added, and the mixture is extracted by oscillation. The mixture is allowed to stand for stratification, and the organic layer is collected. Anhydrous sodium sulfate is added to dry the mixture to remove water. After filtering, the filtrate is concentrated under reduced pressure, and the product is recrystallized from ethanol to obtain spirocyclic phosphate diphenylamine.
[0011] (2) Add N-methylpyrrolidone and toluene to the reaction flask, remove water by azeotropy, then add trimellitic anhydride and spirocyclic phosphate diphenylamine in a molar ratio of (2-2.2):1, carry out ring-opening reaction at 30-45°C for 4-6 hours, then increase the temperature to 135-150°C, carry out cyclization reaction for 5-8 hours, add water to the solution, precipitate, filter, wash with ethanol, and dry to obtain a phosphorimide benzoic acid monomer.
[0012] Among them, the preparation method of the flame retardant and wear-resistant fiber is: polyethylene terephthalate, phosphorimide polyester, and antioxidant are mixed in a mixer, and then spun in a melt spinning machine, the temperature of zones 1-4 of the melt spinning machine is 270-295°C, and the spinning speed is 1000-2000m / min; then stretching is carried out, the hot plate temperature is 80-85°C, the hot plate temperature is 165-185°C, the stretching speed is 200-500m / min, and the stretching multiple is 3-4 times; flame retardant and wear-resistant fiber is obtained.
[0013] Among them, flame retardant and wear-resistant fibers are used to prepare flame retardant and wear-resistant polyester fabrics.
[0014] The technical effect of the present invention is as follows: the present invention utilizes novel phosphorus-containing imide benzoic acid monomer to carry out polymerization reaction with ethylene glycol to obtain phosphorus-containing imide polyester, and then melt-spins with polyethylene terephthalate to obtain polyester fiber. The phosphorus-containing imide polyester contains a polyester molecular chain structure, and has good compatibility with the polyester molecular chain of polyethylene terephthalate. In the melt spinning process, the two are difficult to have microphase separation phenomenon, and the main chain of the phosphorus-containing imide polyester contains an imide rigid group, and has strong structural stability and large modulus, which is beneficial to improving the breaking strength of the polyester fiber. At the same time, the imide has strong heat resistance and is not easy to be thermally decomposed, which significantly improves the initial thermal decomposition temperature and high temperature resistance of the polyester fiber. The spirocyclic phosphate group in the molecular chain is thermally decomposed at high temperature to produce phosphoric acid substances, which can promote the dehydration of the polyester fiber into carbon, and is beneficial to improving the residual carbon content and flame retardant performance.
[0015] The limiting oxygen index of the polyester fabric made of polyester fiber of the present invention reaches 26.5-29.8%, which is attributed to the fact that the phosphorus imide polyester contains spirocyclic phosphate groups and nitrogen-containing imide rings, forming an expansion flame retardant system, which promotes the formation of an expansion carbon layer on the polyester fabric during combustion, showing good flame retardant performance. In addition, the friction mass loss rate is low and the wear resistance is excellent. DETAILED DESCRIPTION
[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] Example 1
[0018] (1) At 10°C, add 250 mL of water, 84 mmol of 4-acetaminophenol (CAS registration number 103-90-2), 8 mmol of sodium carbonate, and 40 mmol of spirocyclic phosphate dichloride (CAS registration number 714-87-4) to a reaction bottle, stir and react for 4 hours, then add 550 mmol of sodium hydroxide, heat to 85°C, hydrolyze for 18 hours, add ethyl acetate, shake and extract, stand and separate, collect the organic layer, add anhydrous sodium sulfate to dry and remove water, filter and concentrate the filtrate under reduced pressure, and recrystallize the product in ethanol to obtain spirocyclic phosphate diphenylamine. The reaction formula is:
[0019]
[0020] (2) Add 160 mL of N-methylpyrrolidone and 70 mL of toluene to the reaction flask, heat to 150°C to remove water by azeotropic reaction, then add 140 mmol of trimellitic anhydride (CAS registration number 552-30-7) and 70 mmol of spirocyclic phosphate diphenylamine, carry out ring-opening reaction at 30°C for 6 hours, then heat to 145°C and carry out cyclization reaction for 8 hours, add water to the solution, precipitate, filter, wash with ethanol, and dry to obtain phosphorimide-containing benzoic acid monomer. The reaction formula is:
[0021]
[0022] (3) Add 140mmol ethylene glycol, 100mmol phosphorimide benzoic acid monomer, and 1.3mmol p-toluenesulfonic acid to the reactor, introduce nitrogen, heat to 180°C for polymerization for 5h, cool the material, filter, wash with toluene and ethanol in turn, and dry to obtain phosphorimide polyester. The reaction formula is:
[0023]
[0024] (4) Mix 950 g of polyethylene terephthalate, 50 g of phosphorimide polyester and 5 g of antioxidant 168 in a mixer, and then spin them in a melt spinning machine. The temperatures of zones 1-4 of the melt spinning machine are 270°C, 290°C, 295°C and 295°C, and the spinning speed is 2000 m / min. Then stretch them. The temperature of the hot plate is 85°C, the temperature of the hot plate is 165°C, the stretching speed is 400 m / min, and the stretching multiple is 3 times. Flame-retardant and wear-resistant fibers are obtained.
[0025] Example 2
[0026] (1) At 8°C, add 200 mL of water, 76 mmol of 4-acetaminophenol, 12 mmol of sodium carbonate, and 40 mmol of spirocyclic phosphate dichloride to a reaction flask, stir and react for 8 h, then add 620 mmol of sodium hydroxide, raise the temperature to 90°C, hydrolyze for 10 h, add ethyl acetate, shake and extract, stand and separate, collect the organic layer, add anhydrous sodium sulfate to dry and remove water, filter, and concentrate the filtrate under reduced pressure. The product is recrystallized in ethanol to obtain spirocyclic phosphate diphenylamine.
[0027] (2) Add 140 mL of N-methylpyrrolidone and 60 mL of toluene to the reaction flask, heat to 150° C. to remove water by azeotropic reaction, then add 140 mmol of trimellitic anhydride and 70 mmol of spirocyclic phosphate diphenylamine, carry out ring-opening reaction at 35° C. for 4 h, then heat to 150° C. to carry out cyclization reaction for 5 h, add water to the solution to precipitate, filter, wash with ethanol, and dry to obtain a phosphorimidate-containing benzoic acid monomer.
[0028] (3) Add 160 mmol of ethylene glycol, 100 mmol of phosphorimide benzoic acid monomer, and 1.5 mmol of p-toluenesulfonic acid into the reaction kettle, introduce nitrogen, raise the temperature to 160° C. to carry out polymerization reaction for 10 hours, cool the material, filter it, wash it with toluene and ethanol in turn, and dry it to obtain phosphorimide polyester.
[0029] (4) Mix 880 g of polyethylene terephthalate, 120 g of phosphorimide polyester and 2 g of antioxidant 168 in a mixer, and then spin them in a melt spinning machine. The temperatures of zones 1-4 of the melt spinning machine are 270°C, 290°C, 295°C and 295°C, and the spinning speed is 1000 m / min. Then stretch them. The temperature of the hot plate is 80°C, the temperature of the hot plate is 170°C, the stretching speed is 500 m / min, and the stretching multiple is 4 times. Flame-retardant and wear-resistant fibers are obtained.
[0030] Example 3
[0031] (1) At 5°C, add 200 mL of water, 80 mmol of 4-acetaminophenol, 12 mmol of sodium carbonate, and 40 mmol of spirocyclic phosphate dichloride to a reaction flask, stir and react for 6 h, then add 620 mmol of sodium hydroxide, raise the temperature to 80°C, and hydrolyze for 18 h. Add ethyl acetate, shake and extract, stand and separate, collect the organic layer, add anhydrous sodium sulfate to dry and remove water, filter, and concentrate the filtrate under reduced pressure. The product is recrystallized in ethanol to obtain spirocyclic phosphate diphenylamine.
[0032] (2) Add 180 mL of N-methylpyrrolidone and 70 mL of toluene to the reaction flask, heat to 150° C. to remove water by azeotropy, then add 154 mmol of trimellitic anhydride and 70 mmol of spirocyclic phosphate diphenylamine, carry out ring-opening reaction at 45° C. for 4 h, then heat to 135° C. and carry out cyclization reaction for 8 h, add water to the solution, precipitate, filter, wash with ethanol, and dry to obtain phosphorimidate-containing benzoic acid monomer.
[0033] (3) Add 160 mmol of ethylene glycol, 100 mmol of phosphorimide benzoic acid monomer, and 1.8 mmol of p-toluenesulfonic acid into the reaction kettle, introduce nitrogen, raise the temperature to 180° C. to carry out polymerization reaction for 6 hours, cool the material, filter it, wash it with toluene and ethanol in turn, and dry it to obtain phosphorimide polyester.
[0034] (4) Mix 820 g of polyethylene terephthalate, 180 g of phosphorimide polyester and 2 g of antioxidant 168 in a mixer, and then spin them in a melt spinning machine. The temperatures of zones 1-4 of the melt spinning machine are 270°C, 290°C, 295°C and 295°C, and the spinning speed is 2000 m / min. Then stretch them. The temperature of the hot plate is 85°C, the temperature of the hot plate is 185°C, the stretching speed is 200 m / min, and the stretching multiple is 4 times. Flame-retardant and wear-resistant fibers are obtained.
[0035] Comparative Example 1
[0036] (1) 950 g of polyethylene terephthalate and 5 g of antioxidant 168 are mixed in a mixer, and then spun in a melt spinning machine, the temperatures of zones 1-4 of the melt spinning machine are 270° C., 290° C., 295° C., and 295° C., and the spinning speed is 2000 m / min; then stretching is performed, the hot plate temperature is 85° C., the hot plate temperature is 165° C., the stretching speed is 400 m / min, and the stretching multiple is 3 times; polyester fiber is obtained.
[0037] Comparative Example 2
[0038] (1) 950 g of polyethylene terephthalate, 50 g of phosphorimidate-containing benzoic acid monomer (structural formula: ), 5g antioxidant 168 are mixed in a mixer, and then spun in a melt spinning machine, the temperatures of zones 1-4 of the melt spinning machine are 270°C, 290°C, 295°C, and 295°C, and the spinning speed is 2000m / min; then stretching is carried out, the hot plate temperature is 85°C, the hot plate temperature is 165°C, the stretching speed is 400m / min, and the stretching multiple is 3 times; polyester fiber is obtained.
[0039] Comparative Example 3
[0040] (1) Add 160 mL of N-methylpyrrolidone and 70 mL of toluene to a reaction flask, heat to 150°C to remove water by azeotropic azeotropy, then add 140 mmol of trimellitic anhydride and 70 mmol of 4,4-diaminodiphenylmethane, carry out a ring-opening reaction at 30°C for 6 hours, then heat to 145°C and carry out a cyclization reaction for 8 hours, add water to the solution, precipitate, filter, wash with ethanol, and dry to obtain an imidobenzoic acid monomer. The reaction formula is:
[0041]
[0042] (2) Add 140 mmol of ethylene glycol, 100 mmol of imidobenzoic acid monomer, and 1.3 mmol of p-toluenesulfonic acid into a reaction kettle, introduce nitrogen, raise the temperature to 180° C. to carry out polymerization reaction for 5 hours, cool the material, filter it, wash it with toluene and ethanol in turn, and dry it to obtain imido polyester.
[0043] (3) Mix 950 g of polyethylene terephthalate, 50 g of imide polyester and 5 g of antioxidant 168 in a mixer, and then spin them in a melt spinning machine. The temperatures of zones 1-4 of the melt spinning machine are 270°C, 290°C, 295°C and 295°C, and the spinning speed is 2000 m / min. Then stretch them. The temperature of the hot plate is 85°C, the temperature of the hot plate is 165°C, the stretching speed is 400 m / min, and the stretching multiple is 3 times. Polyester fiber is obtained.
[0044] The breaking properties of polyester fibers were tested using an electronic single fiber strength tester. The pre-tension was 150 cN, the clamping distance was 20 cm, and the stretching speed was 100 mm / min. Five samples were tested in each group and the average value was taken.
[0045] The thermogravimetric performance of polyester fiber was tested using a thermogravimetric analyzer in a nitrogen atmosphere, with a heating rate of 10°C / min from room temperature to 700°C. The test results are shown in the following table:
[0046]
[0047] As can be seen from the above table, in Examples 1-3, polyethylene terephthalate and phosphorimide-containing polyester are melt-spun, and the breaking strength of the obtained polyester fiber reaches 2.74-3.24 cN / dtex, the elongation at break reaches 74.0-98.5%, and the initial decomposition temperature reaches 408.8-413.9°C, and the residual carbon content reaches 20.6-26.7%, which are all higher than the polyester fiber of Comparative Example 1, showing good mechanical properties and high temperature resistance. This is attributed to the fact that the phosphorimide-containing polyester contains a polyester molecular chain structure, and has good compatibility with the polyester molecular chain of polyethylene terephthalate. During the melt spinning process, it is difficult for the two to undergo microphase separation. In addition, the main chain of the phosphorimide-containing polyester contains an imide rigid group, which has strong structural stability and large modulus, which is beneficial to improving the breaking strength of the polyester fiber. At the same time, the imide has strong heat resistance and is not easy to thermally decompose, which significantly improves the initial thermal decomposition temperature of the polyester fiber. The spirocyclic phosphate groups in the molecular chain High-temperature thermal decomposition produces phosphoric acid substances, which can promote the dehydration of polyester fibers into carbon, which is beneficial to increasing the residual carbon content and flame retardant properties.
[0048] Comparative Example 2: Phosphorus imidobenzoic acid monomer and polyethylene terephthalate were melt-spun. Due to the poor compatibility between the two, phase separation defects were easily generated after spinning, which reduced the breaking strength and elongation of the polyester fiber. In addition, the initial thermal decomposition temperature was slightly reduced.
[0049] In Comparative Example 3, trimellitic anhydride and 4,4-diaminodiphenylmethane are reacted to obtain an imidobenzoic acid monomer, which is then polymerized with ethylene glycol to obtain an imido polyester, which is finally melt-spun with polyethylene terephthalate. The imido polyester contains a polyester molecular chain structure and has good compatibility with the polyester molecular chain of polyethylene terephthalate. The main chain contains an imido rigid group, which significantly improves the breaking strength and initial thermal decomposition temperature of the polyester fiber. However, the imido polyester does not contain a spirocyclic phosphate group, and the charring property and mass residual rate of the polyester fiber are lower than those in Example 1.
[0050] A weft knitting machine was used. The polyester fibers of Examples 1-3 and Comparative Examples 1-3 were woven into polyester fabrics, respectively, with a warp density of 120 strands / 25.4 mm, a weft density of 75 strands / 25.4 mm, and a fabric thickness of 0.28 mm. The flame retardant properties of the polyester fabrics were tested using an oxygen index tester according to the GB / T 5454-1997 method.
[0051] The wear resistance of polyester fabric was tested using a disc-type fabric flat abrasion tester, with a pressure hammer of 250g, a friction revolution of 500 revolutions, and a rotation speed of 60r / min. The mass loss rate was calculated, W = (m0-m) / m0×100%, where m0 is the mass of the fabric before friction, and m is the mass of the fabric after friction. The smaller the mass loss rate, the better the wear resistance. The test results are as follows:
[0052] Limiting oxygen index (%) Mass loss rate (%) Example 1 26.5 1.29 Example 2 27.9 1.20 Example 3 29.8 1.18 Comparative Example 1 21.5 1.46 Comparative Example 2 27.3 1.49 Comparative Example 3 23.2 1.26
[0053] As can be seen from the above table, the limiting oxygen index of the polyester fabric made of polyester fibers in Examples 1-3 reaches 26.5-29.8%, which is higher than that in Comparative Example 1, and has good flame retardant properties. This is attributed to the fact that the phosphorus imide polyester contains spirocyclic phosphate groups and nitrogen-containing imide rings, forming an intumescent flame retardant system, which promotes the formation of an intumescent carbon layer on the polyester fabric during combustion, showing good flame retardant properties. In addition, the friction mass loss rate is only 1.18-1.29%, which is lower than that in Comparative Example 1, and has excellent wear resistance.
[0054] Comparative Example 2 adds a phosphorus-containing imide benzoic acid monomer, which contains a spirocyclic phosphate group and a nitrogen-containing imide ring, and can form an intumescent flame retardant system. The limiting oxygen index of the polyester fabric reaches 27.3%, and the flame retardant performance is good.
[0055] The imide polyester added in Comparative Example 3 does not contain spirocyclic phosphate groups and has poor flame retardant properties for polyester fabrics.
[0056] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A flame retardant and wear resistant fiber, characterized in that: The flame retardant and wear resistant fiber comprises 82-95 parts by weight of polyethylene terephthalate, 5-18 parts by weight of phosphorimide polyester, and 0.2-0.5 parts by weight of antioxidant; The preparation method of the phosphorimide-containing polyester comprises the following steps: adding ethylene glycol, phosphorimide-containing benzoic acid monomer and p-toluenesulfonic acid into a reaction kettle, introducing nitrogen, carrying out polymerization reaction, cooling the material, filtering, washing with toluene and ethanol in sequence, and drying to obtain the phosphorimide-containing polyester.
2. The flame retardant and wear resistant fiber according to claim 1, characterized in that: The molar ratio of the ethylene glycol, the phosphorimidate-containing benzoic acid monomer, and p-toluenesulfonic acid is (1.4-1.6):1:(0.013-0.018).
3. The flame retardant and wear resistant fiber according to claim 1, characterized in that: The polymerization reaction temperature is 160-180° C., and the reaction time is 5-10 hours.
4. The flame retardant and wear resistant fiber according to claim 1, characterized in that: The preparation method of the phosphorimide-containing benzoic acid monomer is as follows: (1) Add water, 4-acetaminophenol, sodium carbonate, and spirocyclic phosphate dichloride to a reaction flask at 5-10° C., stir and react for 4-8 hours, then add sodium hydroxide, raise the temperature to 80-90° C., react for 10-18 hours, add ethyl acetate, extract, and recrystallize to obtain spirocyclic phosphate diphenylamine; (2) Add N-methylpyrrolidone and toluene to the reaction flask, remove water by azeotropic method, then add trimellitic anhydride and spirocyclic phosphate diphenylamine to carry out ring-opening reaction, and then carry out cyclization reaction, add water to the solution, precipitate, filter, wash and dry the precipitate to obtain phosphorimide-containing benzoic acid monomer.
5. The flame retardant and wear resistant fiber according to claim 4, characterized in that: In the method (1), the molar ratio of 4-acetaminophenol, sodium carbonate and spirocyclic phosphate dichloride is (1.9-2.1):(0.2-0.3):
1.
6. The flame retardant and wear resistant fiber according to claim 4, characterized in that: In the above (2), the molar ratio of trimellitic anhydride to spirocyclic phosphate diphenylamine is (2-2.2):
1.
7. The flame retardant and wear resistant fiber according to claim 4, characterized in that: In the above (1), the temperature of the ring-opening reaction is 30-45°C, and the reaction time is 4-6 hours; the temperature of the cyclization reaction is 135-150°C, and the reaction time is 5-8 hours.
8. A method for preparing the flame retardant and wear resistant fiber according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: uniformly mixing polyethylene terephthalate, phosphorimide-containing polyester and an antioxidant in a mixer, and then spinning and drawing the fibers in a melt spinning machine to obtain flame-retardant and wear-resistant fibers.
9. The method for preparing the flame retardant and wear resistant fiber according to claim 8, characterized in that: The temperature of zones 1-4 of the melt spinning machine is 270-295° C., and the spinning speed is 1000-2000 m / min; the temperature of the hot plate during drawing is 80-85° C., the temperature of the hot plate is 165-185° C., the drawing speed is 200-500 m / min, and the drawing multiple is 3-4 times.
10. A flame-retardant and wear-resistant polyester fabric made of the flame-retardant and wear-resistant fiber obtained by the preparation method according to claim 9.
Citation Information
Cited By
Preparation method and application of high-temperature-resistant flame-retardant fireproof blanket