A method for preparing silicon carbide material, application and silicon carbide material

By adjusting the process parameters of the chemical vapor deposition method, silicon carbide materials with high resistivity, high purity and high density are prepared, which solves the problems of short service life and easy contamination of silicon carbide materials in semiconductor production in the existing technology, and realizes Provides longer etching ring life and higher resistivity.

CN118064864BActive Publication Date: 2024-10-18湖南德智新材料股份有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410219496.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-27
Publication Date
2024-10-18
Estimated Expiration
2044-02-27

AI Technical Summary

Technical Problem

It is difficult to prepare silicon carbide materials with high resistivity, high purity and density with existing technology, which results in the etching ring having a short service life and being easily contaminated in semiconductor production.

Method used

Silicon carbide materials are prepared by chemical vapor deposition (CVD), adjusting the deposition temperature, pressure and the ratio of carbon silane and reducing gas, controlling the grain size and grain boundary structure, and obtaining high resistivity, high purity and high density. silicon carbide material.

Benefits of technology

It achieves high density, high purity and high resistivity of silicon carbide material, extends the service life of the etching ring, avoids contamination of the chip, and meets the needs of semiconductor etching rings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118064864B_ABST
    Figure CN118064864B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of semiconductor etching materials, and provides a method for preparing silicon carbide material, application and silicon carbide material, wherein the method for preparing silicon carbide material comprises: providing a substrate, placing the substrate in a vacuum chemical vapor deposition device for heating; introducing dilution gas and reaction gas into the chemical vapor deposition device, wherein the reaction gas comprises carbosilane and / or reducing gas, and setting the deposition process parameters: the deposition temperature is 1000°C-1500°C, the deposition pressure is 9000Pa-40,000Pa, and the flow ratio of carbosilane and reducing gas is 1:(1-40); after the chemical vapor deposition is completed, the introduction of dilution gas and reaction gas is stopped. The silicon carbide material obtained by the above method has excellent properties such as high resistivity, high purity and high density, and can be used in semiconductor production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor etching materials, and in particular to a method for preparing a silicon carbide material, an application thereof, and the silicon carbide material. Background Art

[0002] In semiconductor production, multiple procedures and components are involved, and each component is required to have its own unique properties to ensure that it can work well in the semiconductor production process. Etching is an extremely important link. In the etching process, it is necessary to select etching rings with different resistivities to assist in etching the wafer according to the different directions of the application.

[0003] Silicon carbide material has excellent properties such as wear resistance, strong oxidation resistance, acid and alkali resistance, and strong corrosion resistance. It is also a wide bandgap semiconductor material, so it is widely used in the production and processing of semiconductors. In the semiconductor etching process, etching rings are often used to assist in etching wafers. Etching rings can make the wafer surface evenly etched, and the edge of the wafer can also be evenly etched. However, during the etching process, the etching ring and the wafer are exposed to the etching environment at the same time, and the etching ring will also be etched by the plasma. Therefore, the purity and etching resistance of the etching ring are extremely important. The quality of the etching resistance directly affects the service life of the etching ring and the replacement frequency in production, thereby affecting the economic benefits of production. Etching rings with high purity and density will not contaminate the wafer during etching. At the same time, the high resistivity of the etching ring can reduce the degree of etching of the etching ring. The high resistivity can form a low sheath voltage on the surface of the etching ring, thereby reducing the etching rate of the etching ring and increasing the life of the etching ring. Therefore, the purity, density and high resistivity of the etching ring are extremely important to the performance of the etching ring.

[0004] However, in the related art, the silicon carbide material used to prepare the etching ring cannot have excellent properties such as high resistivity, high purity and density. Summary of the invention

[0005] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a method for preparing silicon carbide material, application and silicon carbide material. The silicon carbide material obtained by the preparation method of the present invention has excellent properties such as high resistivity, high purity and density.

[0006] Silicon carbide (SiC) material is an important structural material with the characteristics of high temperature resistance, high hardness, excellent oxidation resistance and chemical corrosion resistance, wear resistance, thermal shock resistance, etc. In addition, silicon carbide material also has advantages such as thermal expansion coefficient similar to Si, higher thermal conductivity, higher critical breakdown voltage, negative resistance temperature coefficient, etc., making it widely used in semiconductor components serving in high frequency, high temperature and high pressure environments.

[0007] The inventors of the present invention have found that the silicon carbide prepared by vacuum sintering has a high resistivity, but a low purity and a high porosity. The high porosity is easily etched in chip production, which makes the high-resistivity silicon carbide prepared by sintering rarely used in semiconductor production. The method of producing high-resistivity silicon carbide by CVD solves the porosity problem and can prepare silicon carbide with a high density, thereby obtaining a silicon carbide material with excellent etching resistance.

[0008] The inventors of the present invention have also found that the silicon carbide material prepared by the CVD method has a low porosity but a low resistivity. Although doping with impurity elements can increase the resistivity, the impurity elements doped in the etching ring will affect the purity of the etched chip. Therefore, how to obtain a silicon carbide material with high resistivity, high purity and high density is a problem that needs to be solved.

[0009] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a silicon carbide material, comprising the following steps:

[0010] (1) providing a substrate, and placing the substrate in a vacuum chemical vapor deposition device for heating;

[0011] (2) introducing a diluent gas and a reaction gas into a chemical vapor deposition device, wherein the reaction gas includes carbosilane and / or a reducing gas, and setting deposition process parameters: a deposition temperature of 1000° C. to 1500° C., a deposition pressure of 9000 Pa to 40,000 Pa, and a flow ratio of carbosilane to reducing gas of 1:(1-40);

[0012] (3) After chemical vapor deposition is completed, stop introducing dilution gas and reaction gas.

[0013] The inventors of the present invention have found that by adjusting the process parameters of temperature, pressure, and the ratio of carbosilane to reducing gas, a silicon carbide material with high resistivity, high purity, and high density can be obtained.

[0014] By regulating process parameters such as temperature and pressure within a certain range, silicon carbide crystals of different sizes and cubic structures can be obtained. The difference in grain size will affect the grain boundary barrier and carrier concentration, which are related to the resistivity. The effective barrier height at the grain boundary can be effectively regulated by changing the grain size.

[0015] The inventors of the present invention have found that a high resistivity silicon carbide material can be obtained by adjusting the ratio of carbon silane hydrocarbons and reducing gas used to prepare the silicon carbide material.

[0016] The second aspect of the present invention provides application of the above method in preparing high resistivity materials.

[0017] A third aspect of the present invention provides a silicon carbide material, wherein the purity of the silicon carbide material is greater than 99.9999%, the average particle size is 0.05 μm-3 μm, and the resistivity is 5 kΩ.cm-50 kΩ.cm.

[0018] The inventors of the present invention have found that the silicon carbide material obtained by the above preparation method has high purity, high resistivity and high density. The proportion of its grain boundaries with large angles greater than 10° is also high, which is 55%-85%, and the grain boundary barrier is 0.05ev-1ev; the average dislocation density is (50-140)×10 14 / m 2 , carrier concentration <10 15 (1 / cm 3 ), the difference in crystal structure makes silicon carbide material have higher resistivity and can be used in the preparation of high purity, high density, high hardness or high resistivity products.

[0019] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0020] (1) The method for preparing silicon carbide material provided by the present invention changes the microstructure of the silicon carbide material to a certain extent by changing the process parameters, thereby obtaining a silicon carbide material with high density, high purity and high resistivity.

[0021] (2) The silicon carbide material provided by the present invention has excellent properties of high density, high resistivity and high purity. When used for auxiliary etching of chips in semiconductors, it can reduce the degree of etching of the etching ring, increase the life of the etching ring, and will not contaminate the wafer.

[0022] (3) The silicon carbide material provided by the present invention does not incorporate impurity elements when increasing the resistivity, and thus will not pollute chips and important production components.

[0023] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Shown is a graph showing the particle size distribution of the silicon carbide material sample of the present invention.

[0025] Figure 2Shown is the XRD diffraction pattern of the silicon carbide material in the present invention.

[0026] Figure 3 Shown is a SEM image of the silicon carbide material sample of the present invention with an average particle size of <1 μm. DETAILED DESCRIPTION

[0027] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0028] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0029] A first aspect of the present invention provides a method for preparing a silicon carbide material, comprising the following steps:

[0030] (1) providing a substrate, and placing the substrate in a vacuum chemical vapor deposition device for heating;

[0031] (2) introducing a diluent gas and a reaction gas into a chemical vapor deposition device, wherein the reaction gas includes carbosilane and / or a reducing gas, and setting deposition process parameters: a deposition temperature of 1000° C. to 1500° C., a deposition pressure of 9000 Pa to 40,000 Pa, and a flow ratio of carbosilane to reducing gas of 1:(1-40);

[0032] (3) After chemical vapor deposition is completed, stop introducing dilution gas and reaction gas.

[0033] In some embodiments, in step (1), the substrate is a carbon-based material and / or a silicon-based material. Preferably, the substrate comprises at least one of graphite, silicon, quartz or silicon carbide. The substrate is preferably a graphite substrate, which is a material formed by stacking carbon atoms and has good electrical conductivity and thermal conductivity. Graphite substrates are mainly used as reactor materials in the preparation of silicon carbide, which can withstand high temperatures and chemical corrosion and have low chemical reaction activity.

[0034] The substrate is placed in a vacuum chemical vapor deposition device for heating because vacuuming can eliminate gas interference, improve reaction efficiency, avoid contamination of deposits, and avoid oxidation.

[0035] The chemical vapor deposition (CVD) is a process in which a gaseous or vaporous substance reacts in a gas phase or at a gas-solid interface to generate a solid deposit. Optional chemical vapor deposition equipment includes a high-temperature deposition furnace, a hot wall reactor, a low-pressure chemical vapor deposition equipment, a vapor phase epitaxy equipment, a metal organic chemical vapor deposition equipment, a plasma enhanced chemical vapor deposition equipment, etc. By adjusting the deposition parameters, the crystal structure, morphology, and density of the silicon carbide material deposited on the substrate can be effectively controlled. When the deposition reaction is carried out under high pressure, the collision probability between active atoms increases, which is conducive to the growth of crystal nuclei and is easy to grow into large grains. At this time, the grain boundaries become fewer and the resistivity becomes smaller. However, when the CVD deposition reaction pressure is too low, the density of the silicon carbide material generated is not high enough and cannot meet the etching requirements. Therefore, when the CVD deposition pressure is controlled within the above range, the requirements of high density and high resistivity of etching can be met at the same time.

[0036] In some embodiments, the dilution gas in step (2) is an inert gas, preferably Ar. The volume fraction of the dilution gas is 30%-50%, where the volume fraction of the dilution gas is the percentage of the volume of the dilution gas to the volume of the total participating gas.

[0037] In some embodiments, the carbosilane hydrocarbon includes: at least one of monosilane, disilane, trisilane, methylchlorosilane, dimethylchlorosilane or trichloromethylsilane; preferably trichloromethylsilane.

[0038] In some embodiments, the reducing gas includes at least one of hydrogen, methane, ethylene or acetylene, preferably hydrogen.

[0039] By limiting and optimizing the deposition temperature, deposition pressure and ratio of carbosilane to reducing gas of the silicon carbide material, the resistivity and density of the silicon carbide material can be further improved.

[0040] In the present invention, the deposition temperature is 1000° C.-1500° C., and the deposition temperature refers to the temperature used when preparing silicon carbide material.

[0041] In some embodiments, the deposition temperature is 1100°C-1400°C, for example, 1100°C, 1200°C, 1300°C and 1400°C. In some more preferred embodiments, the deposition temperature is 1250°C-1350°C.

[0042] In the present invention, the deposition pressure is 9000-40,000Pa, and the deposition pressure refers to the gas pressure applied in the reaction chamber during the deposition process. The deposition pressure can affect the deposition rate, the film quality and the microstructure of the film. Within a certain range, a higher deposition pressure can increase the deposition rate, improve the quality and uniformity of the deposit, and also lead to a larger grain size and a lower dislocation density. This is because as the deposition pressure increases, the distance between gas molecules decreases, thereby enhancing the intermolecular force and promoting deposition.

[0043] In some embodiments, the deposition pressure is 15,000Pa-31,000Pa, for example, 15,000Pa, 20,000Pa, 22,000Pa, 25,000Pa, 26,000Pa, 29,000Pa, 30,000Pa and 31,000Pa. In some more preferred embodiments, the deposition pressure is 20,000-26,000Pa, for example, 20,000Pa, 22,000Pa, 23,000Pa, 24,000Pa, 25,000Pa and 26,000Pa.

[0044] In some embodiments, the flow ratio of the carbosilane and the reducing gas is 1:(1-40), for example, it can be 1:1, 1:5, 1:7, 1:9, 1:10, 1:13, 1:15, 1:18, 1:20, 1:25, 1:30, 1:35 and 1:40.

[0045] In some preferred embodiments, the flow ratio of the carbosilane to the reducing gas is 1:(10-30); in some more preferred embodiments, the flow ratio of the carbosilane to the reducing gas is 1:(15-25).

[0046] In some embodiments, the carbosilane is trichloromethylsilane, and the reducing gas is hydrogen, and the flow ratio is 1:(1-40). In some preferred embodiments, the flow ratio of trichloromethylsilane to hydrogen is 1:(10-30), and in some more preferred embodiments, the flow ratio of trichloromethylsilane to hydrogen is 1:(15-25).

[0047] In some embodiments, the resistivity of silicon carbide material will be relatively large only when the deposition temperature of silicon carbide material is 1000-1500°C, the deposition pressure is 9000-40,000Pa and the ratio of carbon silane to reducing gas is 1:(1-40). If any of the values ​​does not fall within its protection range, the resistivity will be relatively small.

[0048] Preferably, in some embodiments, the deposition temperature of the silicon carbide material is 1100-1400°C, the deposition pressure is 15,000-31,000Pa, and the ratio of carbosilane to reducing gas is 1:(10-30), that is, when all the deposition parameters of the silicon carbide material fall within the above protection range, the resistivity of silicon carbide will be larger.

[0049] More preferably, in some embodiments, the deposition temperature of the silicon carbide material is 1250°C-1350°C, the deposition pressure is 20,000Pa-26,000Pa, and the ratio of carbon silane to reducing gas is 1:(15-25), that is, when all the deposition parameters of the silicon carbide material fall within the above protection range, the resistivity of silicon carbide will be larger.

[0050] The second aspect of the present invention provides application of the above method in preparing high resistivity materials.

[0051] A third aspect of the present invention provides a silicon carbide material, the purity of the silicon carbide material is greater than 99.9999%, the average particle size of the silicon carbide material is 0.05 μm-3 μm, the porosity is less than 0.1%, and the resistivity is 5 kΩ.cm-50 kΩ.cm.

[0052] In some embodiments, the silicon carbide material has a porosity of 0.01%-0.1%.

[0053] Figure 3 This is a SEM image of a silicon carbide material sample with an average particle size of 1 μm, wherein the silicon carbide material has a relatively small porosity.

[0054] In the present invention, the purity of the silicon carbide material is detected and analyzed by GDMS, and the purity of the silicon carbide material is greater than 99.9999%, that is, the purity of the silicon carbide material is very high, with almost no other impurities, and can be used in the semiconductor field.

[0055] In the present invention, the average particle size of the silicon carbide material is a volume particle size, which is tested by EBSD (electron backscatter diffraction), which is a test method used to study the crystal structure and crystal orientation of materials. It interacts with the crystals on the surface of the material through an electron beam, and obtains information such as the crystal orientation, crystal structure and grain morphology of the material by measuring the scattering pattern of the reflected electrons.

[0056] The average particle size of the silicon carbide material in the present invention is 0.05 μm-3 μm. The smaller the average particle size of the silicon carbide material, the more grain boundaries there are between the grains. When there are more grain boundaries, the flow of electrons will be hindered, resulting in a higher resistivity. In addition, the grain boundaries are defects in the material, which will cause electrons to scatter at the grain boundaries, thereby increasing the resistivity. Figure 1The figure shows the particle size distribution of the silicon carbide material sample. The average grain diameter in the figure is 0.1μm, and the area-weighted mean is 0.1μm, that is, the grain size of the silicon carbide material obtained by the above method is generally small, which means that under the same raw material conditions, the silicon carbide material obtained by the present invention has a high grain boundary barrier, a high proportion of large-angle grain boundaries, and a greater resistivity.

[0057] In this embodiment, the average grain size of the silicon carbide material may be 0.05 μm, 0.1 μm, 0.2 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, or 3 μm.

[0058] In the present invention, the porosity test method is a water drainage method. When the porosity of silicon carbide grains is large, there are more defects in the lattice, and electrons are not easily conducted in the lattice, and the resistivity will be relatively large. However, the higher porosity makes the etching ring easily etched during chip production, thereby reducing the life of the etching ring, and is therefore not suitable for use in the semiconductor industry. The silicon carbide material of the present invention must achieve an extremely high density to meet the etching requirements, so the porosity must be maintained within a very small range, which will inevitably lead to a relatively low resistivity. However, the present invention compensates for the shortcomings in resistivity by changing the preparation process and related parameters such as temperature, pressure, and the ratio of carbon silane to reducing gas, so that the silicon carbide material has both a higher density and resistivity.

[0059] In the present invention, the resistivity test method of the silicon carbide material is a four-probe test of the material resistivity.

[0060] In the present invention, taking the application of the silicon carbide material in the preparation of an etching ring as an example, by simultaneously limiting the resistivity, purity and porosity of the silicon carbide material, the etching ring can have a higher resistivity, so that a low sheath voltage is formed on the surface of the etching ring, thereby reducing the etching rate of the etching ring and increasing the life of the etching ring; the etching ring can also have a higher purity, and at this time the etching ring is not doped with any impurity elements, which can prevent the etching ring from contaminating the chip or other production parts during the production of the chip; the etching ring can also have a higher density, and its density will be relatively improved when the porosity is lower. At this time, the etching ring is not easily damaged when being etched, thereby extending the service life.

[0061] The grain size and porosity of the silicon carbide material are limited and optimized, and the density and resistivity of the silicon carbide material are further improved.

[0062] In some embodiments, the average particle size of the silicon carbide material may be 0.05 μm-1 μm. Preferably, the average particle size of the silicon carbide material is 0.05-0.8 μm; for example, it may be 0.05 μm, 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm and 0.8 μm. The smaller the particle size of the silicon carbide material, the larger the grain boundary barrier and the larger the resistivity.

[0063] Preferably, the porosity of the silicon carbide material is 0.01%-0.1%; for example, it may be 0.01%, 0.015%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, or 0.1%.

[0064] Preferably, the resistivity is 10 kΩ.cm-50 kΩ.cm, for example, 10 kΩ.cm, 15 kΩ.cm, 20 kΩ.cm, 25 kΩ.cm, 30 kΩ.cm, 40 kΩ.cm and 50 kΩ.cm.

[0065] Preferably, the resistivity is 20 kΩ.cm-50 kΩ.cm, for example, 20 kΩ.cm, 25 kΩ.cm, 30 kΩ.cm, 40 kΩ.cm and 50 kΩ.cm.

[0066] The grain boundary barriers, carrier concentration, average dislocation density and large-angle grain boundary ratio of the silicon carbide material are limited and optimized to further improve the density and resistivity of the silicon carbide material.

[0067] In one embodiment, the silicon carbide material satisfies at least one of the following:

[0068] The silicon carbide material satisfies at least one of the following:

[0069] (a) The grain boundary barrier of the silicon carbide material is 0.05 eV-1 eV;

[0070] (b) The carrier concentration of the silicon carbide material is less than 10 15 (1 / cm 3 );

[0071] (c) The average dislocation density of the silicon carbide material is (50-140)×10 14 / m 2 ;

[0072] (d) The proportion of high-angle grain boundaries of the silicon carbide material greater than 10° is 55-85%.

[0073] The silicon carbide material grain boundary barrier described in (a) is 0.05ev-1ev; The silicon carbide material grain boundary barrier is obtained by EBSD (electron backscatter diffraction) test. The silicon carbide material grain boundary barrier refers to the energy barrier existing in the grain boundary region of the silicon carbide film. The atomic arrangement in the grain boundary region will have certain distortions and defects. These defects and distortions will cause the energy barrier in the grain boundary region to be higher than the energy barrier inside the crystal. At this time, the difference between the energy barrier in the grain boundary region and the energy barrier inside the crystal is the grain boundary barrier. The grain boundary barrier will increase the resistance of the grain boundary region because electrons will be hindered by the energy barrier when crossing the grain boundary barrier. Therefore, when the grain boundary barrier is larger, the resistivity of the grain boundary region will also increase accordingly. The grain boundary barrier in this embodiment can be 0.05ev, 0.10ev, 0.12ev, 0.16ev, 0.19ev, 0.2ev, 0.3ev, 0.4ev, 0.5ev, 0.6ev, 0.7ev, 0.8ev, 0.9ev, 1.0ev.

[0074] The carrier concentration of the silicon carbide material in (b) is less than 10 15 (1 / cm 3 ); The carrier concentration is obtained through the Hall effect test. The lower the carrier concentration, the fewer free electrons and holes in the silicon carbide material, the less conductive it is, and the greater the resistivity.

[0075] The average dislocation density of the silicon carbide material in (c) is (50-140)×10 14 / m 2 The average dislocation density of silicon carbide material is obtained through EBSD (electron backscatter diffraction) test. The average dislocation density of silicon carbide material represents the number of defects per unit area, including surface defects, structural defects and interface defects. The larger the dislocation density, the less smooth the surface of the silicon carbide material is, and the corresponding resistivity is also greater.

[0076] The proportion of large-angle grain boundaries of silicon carbide materials described in (d)>10° is 55-85%. The large-angle grain boundaries of silicon carbide materials are obtained through EBSD (electron backscatter diffraction) testing. In silicon carbide materials, the grain boundary angles between most grains are greater than 10°, and the orientation differences between grains are large. At this time, due to the presence of some defects and impurities in the grain boundaries, these defects and impurities will scatter electrons, which hinder the transmission of electrons in the material, resulting in an increase in resistivity. When there are more large-angle grain boundaries, the electron transmission is also relatively hindered, and the resistivity is also relatively large at this time. At the same time, large-angle grain boundaries will also affect the crystallinity and grain size of the material, thereby affecting the resistivity of the material. The existence of grain boundaries will cause the distortion and fracture of the lattice, reduce the crystallinity of the crystal, and lead to irregular crystal structure, increased grain boundaries and defects; large-angle grain boundaries will also limit the growth and size of grains. These factors will lead to an increase in the resistivity of the material.

[0077] By limiting the cubic structure and orientation of the silicon carbide material grains, it is shown that the silicon carbide material in this solution has good uniformity and the grains are arranged in an orderly manner, making the silicon carbide material uniform and stable.

[0078] The silicon carbide material is 3C-SiC with a cubic structure and a single orientation of (111). Figure 2 As shown in the figure, the prepared silicon carbide material is determined to be a typical 3C-SiC crystal through XRD detection. <111> The high degree of single orientation can provide consistent crystal structure and performance, that is, the crystal structure in silicon carbide material has a high degree of order and symmetry, which makes silicon carbide material have better stability and reliability in application.

[0079] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0080] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0081] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.

[0082] Example 1

[0083] A silicon carbide material is prepared by the following method:

[0084] (1) placing a graphite substrate in a chemical vapor deposition device, evacuating the device, heating the graphite substrate to 1275° C., and keeping the temperature for 60 min;

[0085] (2) CH3SiCl3 gas and H2 are brought into the chemical vapor deposition equipment with dilution gas Ar, wherein the flow ratio of CH3SiCl3 gas to H2 is 1:25, the flow rate of dilution gas Ar is 42% of the mixed gas, the temperature is maintained at 1275°C, the pressure is set to 20,000 Pa, and the deposition time is 25 hours.

[0086] (3) After the chemical vapor deposition is completed, stop introducing CH3SiCl3, H2 and Ar and cool to room temperature.

[0087] Embodiment 2:

[0088] A silicon carbide material is prepared by the following method:

[0089] Embodiment 2a:

[0090] (1) placing a graphite substrate in a chemical vapor deposition device, evacuating the device, heating the graphite substrate to 1325° C., and keeping the temperature for 60 min;

[0091] (2) CH3SiCl3 gas and H2 are brought into the chemical vapor deposition equipment with the dilution gas Ar, wherein the flow ratio of CH3SiCl3 gas to H2 is 1:15, the flow rate of the dilution gas Ar is 42% of the mixed gas, the temperature is maintained at 1325°C, the pressure is set to 25,000 Pa, and the deposition time is 25 hours.

[0092] (3) After the chemical vapor deposition is completed, stop introducing CH3SiCl3, H2 and Ar and cool to room temperature.

[0093] Embodiment 2b:

[0094] (1) placing a graphite substrate in a chemical vapor deposition device, evacuating the device, heating the graphite substrate to 1200° C., and keeping the temperature for 60 min;

[0095] (2) CH3SiCl3 gas and H2 are brought into the chemical vapor deposition equipment with dilution gas Ar, wherein the flow ratio of CH3SiCl3 gas to H2 is 1:12, the flow rate of dilution gas Ar is 42% of the mixed gas, the temperature is maintained at 1200°C, the pressure is set to 16,000 Pa, and the deposition time is 25 hours.

[0096] (3) After the chemical vapor deposition is completed, stop introducing CH3SiCl3, H2 and Ar and cool to room temperature.

[0097] Embodiment 2c:

[0098] (1) placing a graphite substrate in a chemical vapor deposition device, evacuating the device, heating the graphite substrate to 1380° C., and keeping the temperature for 60 min;

[0099] (2) CH3SiCl3 gas and H2 are brought into the chemical vapor deposition equipment with the dilution gas Ar, wherein the flow ratio of CH3SiCl3 gas to H2 is 1:28, the flow rate of the dilution gas Ar is 42% of the mixed gas, the temperature is maintained at 1380°C, the pressure is set to 30,000 Pa, and the deposition time is 25 hours.

[0100] (3) After the chemical vapor deposition is completed, stop introducing CH3SiCl3, H2 and Ar and cool to room temperature.

[0101] Embodiment 2d:

[0102] (1) placing a graphite substrate in a chemical vapor deposition device, evacuating the device, heating the graphite substrate to 1075° C., and keeping the temperature for 60 min;

[0103] (2) CH3SiCl3 gas and H2 are brought into the chemical vapor deposition equipment with the dilution gas Ar, wherein the flow ratio of CH3SiCl3 gas to H2 is 1:35, the flow rate of the dilution gas Ar is 42% of the mixed gas, the temperature is maintained at 1075°C, the pressure is set to 14,000 Pa, and the deposition time is 25 hours.

[0104] (3) After the chemical vapor deposition is completed, stop introducing CH3SiCl3, H2 and Ar and cool to room temperature.

[0105] Embodiment 2e:

[0106] (1) placing a graphite substrate in a chemical vapor deposition device, evacuating the device, heating the graphite substrate to 1450° C., and keeping the temperature for 60 min;

[0107] (2) CH3SiCl3 gas and H2 are brought into the chemical vapor deposition equipment with dilution gas Ar, wherein the flow ratio of CH3SiCl3 gas to H2 is 1:8, the flow rate of dilution gas Ar is 42% of the mixed gas, the temperature is maintained at 1450°C, the pressure is set to 36,000 Pa, and the deposition time is 25 hours.

[0108] (3) After the chemical vapor deposition is completed, stop introducing CH3SiCl3, H2 and Ar and cool to room temperature.

[0109] Example 3

[0110] This group of embodiments is used to illustrate the influence of changes in the deposition temperature of silicon carbide material on various performance parameters of silicon carbide.

[0111] Example 3a: The difference from Example 1 is that the temperature in step 1 and step 2 is 1300°C.

[0112] Example 3b: The difference from Example 1 is that the temperature in step 1 and step 2 is 1200°C.

[0113] Example 3c: The difference from Example 1 is that the temperature in step 1 and step 2 is 1075°C.

[0114] Example 3d: The difference from Example 1 is that the temperature in step 1 and step 2 is 1450°C.

[0115] Example 3e: The difference from Example 2b is that the temperature in step 1 and step 2 is 1450°C.

[0116] Example 4

[0117] This group of embodiments is used to illustrate the influence of changes in the deposition pressure of silicon carbide material on various performance parameters of silicon carbide.

[0118] Example 4a: The difference from Example 1 is that the pressure in step 2 is 25000 Pa.

[0119] Example 4b: The difference from Example 1 is that the silicon carbide deposition pressure in step 2 is 30,000 Pa.

[0120] Example 4c: The difference from Example 1 is that the silicon carbide deposition pressure in step 2 is 36,000 Pa.

[0121] Example 4d: The difference from Example 1 is that the silicon carbide deposition pressure in step 2 is 14,000 Pa.

[0122] Example 4e: The difference from Example 2b is that the silicon carbide deposition pressure in step 2 is 36,000 Pa.

[0123] Example 5

[0124] This group of examples is used to illustrate the influence of different MTS:H2 ratios of the silicon carbide material reaction raw materials on various performance parameters of silicon carbide.

[0125] Example 5a: The difference from Example 1 is that in step 2, the flow ratio of CH3SiCl3 gas and H2 is 1:15.

[0126] Example 5b: The difference from Example 1 is that in step 2, the flow ratio of CH3SiCl3 gas and H2 is 1:28.

[0127] Example 5c: The difference from Example 1 is that in step 2, the flow ratio of CH3SiCl3 gas and H2 is 1:12.

[0128] Example 5d: The difference from Example 1 is that in step 2, the flow ratio of CH3SiCl3 gas and H2 is 1:35.

[0129] Example 5e: The difference from Example 1 is that in step 2, the flow ratio of CH3SiCl3 gas and H2 is 1:8.

[0130] Example 5f: The difference from Example 2b is that in step 2, the flow ratio of CH3SiCl3 gas and H2 is 1:38.

[0131] Comparative Example 1

[0132] This group of embodiments is used to illustrate the influence of changes in the deposition temperature of silicon carbide material on various performance parameters of silicon carbide.

[0133] Comparative Example 1a: The difference from Example 1 is that the temperature in step 1 and step 2 is different, both being 1800°C.

[0134] Comparative Example 1b: The difference from Example 2d is that the temperature in step 1 and step 2 is different, both being 1800°C.

[0135] Comparative Example 2

[0136] This group of embodiments is used to illustrate the influence of changes in the deposition pressure of silicon carbide material on various performance parameters of silicon carbide.

[0137] Comparative Example 2a: The difference from Example 1 is that the pressure in step 2 is different, which is 55,000 Pa.

[0138] Comparative Example 2b: The difference from Example 2d is that the pressure in step 2 is different, which is 55,000 Pa.

[0139] Comparative Example 3

[0140] This group of examples is used to illustrate the influence of different MTS:H2 ratios of the silicon carbide material reaction raw materials on various performance parameters of silicon carbide.

[0141] Comparative Example 3a: The difference from Example 1 is that the MTS:H2 ratio in step 2 is different, which is 1:50.

[0142] Comparative Example 3b: The difference from Example 2d is that the MTS:H2 ratio in step 2 is different, which is 1:50.

[0143] Table 1

[0144]

[0145]

[0146] The silicon carbide materials obtained in the above examples and comparative examples were respectively subjected to the following tests:

[0147] (1) Test average grain size

[0148] The test method is: electron backscatter diffraction.

[0149] (2) Resistivity

[0150] The test method is as follows:

[0151] The measurement is performed using a four-probe test method. Refer to the following test steps:

[0152] Prepare the sample: Prepare a suitable sample from the silicon carbide material. Usually mechanical methods such as cutting, grinding or cutting can be used to obtain the sample of the required shape and size.

[0153] Connect the four probes: Connect the four probes to the test instrument. Two probes are used as current source and the other two probes are used to measure voltage.

[0154] Place the sample: Place the sample on the test instrument and make sure the sample has good contact with the probe.

[0155] Apply Current: Apply a known current through the two current source probes. Typically a DC current is used.

[0156] Measure voltage: Use the other two voltage probes to measure the voltage across the sample. Make sure the probes make good contact with the sample.

[0157] Calculate resistivity: Use the measured current and voltage values ​​to calculate the resistivity of the sample according to Ohm's law. Resistivity can be calculated using the following formula: Resistivity (ρ) = resistance (R) × cross-sectional area (A) / length (L).

[0158] Record and analyze data: Record the measured resistivity data and analyze and compare them.

[0159] (3) Carrier concentration

[0160] Test method: Hall effect test

[0161] (4) Average dislocation density

[0162] Testing method: Electron backscatter diffraction (EBSD), by measuring the electron backscatter diffraction pattern generated on the sample surface to obtain information about crystal defects, and then infer the average dislocation density.

[0163] (5) The proportion of high-angle grain boundaries is greater than 10°

[0164] Test method: EBSD test

[0165] Sample preparation: Select the material samples to be tested and perform necessary preprocessing, such as cutting, grinding and polishing, to ensure that the sample surface is smooth and has no obvious defects.

[0166] EBSD test device setup: Mount the sample on the EBSD test device, ensuring that the distance between the sample and the detector is appropriate to obtain a clear image.

[0167] Initial settings: According to the characteristics of the sample and the test requirements, set appropriate parameters such as acceleration voltage, current, detector angle and step size.

[0168] Image acquisition: EBSD images are acquired by scanning the sample surface. A combined system of SEM (scanning electron microscope) and EBSD testing device can be used to observe the image scanning process in real time and ensure image quality.

[0169] Data processing: EBSD software is used to process the images, including grain boundary identification, crystal orientation measurement, and grain boundary angle analysis.

[0170] High-angle grain boundary screening: For each grain boundary, screening is performed by comparing the grain boundary angle with the set threshold (>10°), and the number of high-angle grain boundaries is recorded.

[0171] Statistical analysis: Based on the screening results, the proportion of high-angle grain boundaries was calculated, that is, the ratio of the number of high-angle grain boundaries to the total number of grain boundaries.

[0172] Result analysis: Data analysis is performed based on the test results to evaluate the grain boundary structure characteristics of the material and further study its impact on material properties.

[0173] (6) Grain boundary barrier (ev)

[0174] The test method is: CV instrument test (semiconductor analyzer)

[0175] The test data of the embodiments and comparative examples are shown in Table 2.

[0176] Table 2

[0177] Resistivity / kΩ.cm Average grain size / μm <![CDATA[Carrier concentration (1 / cm 3 )]]> Example 1 45.7 0.05 <![CDATA[9.57×10 12 ]]> Example 2a 38.5 0.07 <![CDATA[1.94×10 13 ]]> Example 2b 23.6 0.48 <![CDATA[9.13×10 13 ]]> Example 2c 25.3 0.41 <![CDATA[8.62×10 13 ]]> Example 2d 11.6 0.82 <![CDATA[7.69×10 14 ]]> Example 2e 10.7 0.85 <![CDATA[8.41×10 14 ]]> Example 3a 39.9 0.08 <![CDATA[1.85×10 13 <!-- 10 -->]]> Example 3b 26.7 0.41 <![CDATA[8.49××10 13 ]]> Example 3c 14.4 0.66 <![CDATA[6.19×10 14 ]]> Example 3d 12.7 0.81 <![CDATA[7.19×10 14 ]]> Example 3e 11.8 0.86 <![CDATA[7.67×10 14 ]]> Example 4a 40.3 0.07 <![CDATA[1.01×10 13 ]]> Example 4b 27.3 0.39 <![CDATA[8.07×10 13 ]]> Example 4c 18.6 0.59 <![CDATA[2.40×10 14 ]]> Example 4d 17.5 0.6 <![CDATA[3.76×10 14 ]]> Example 4e 14.1 0.71 <![CDATA[6.79×10 14 ]]> Example 5a 40.7 0.07 <![CDATA[1.09×10 13 ]]> Example 5b 28.7 0.35 <![CDATA[5.52×10 13 ]]> Example 5c 28.1 0.38 <![CDATA[5.67×10 13 ]]> Example 5d 16.9 0.62 <![CDATA[4.27×10 14 ]]> Example 5e 15.3 0.63 <![CDATA[5.94×10 14 ]]> Example 5f 13.7 0.79 <![CDATA[7.13×10 14 ]]> Comparative Example 1a 0.86 6.27 <![CDATA[4.86×10 17 ]]> Comparative Example 1b 0.34 7.46 <![CDATA[7.06×10 17 ]]> Comparative Example 2a 1.37 5.41 <![CDATA[8.34×10 16 ]]> Comparative Example 2b 0.73 6.73 <![CDATA[5.29×10 17 ]]> Comparative Example 3a 1.74 4.28 <![CDATA[7.81×10 16 ]]> Comparative Example 3b 1.61 4.79 <![CDATA[7.93×10 16 ]]>

[0178] The results in Table 2 show that when the present invention adopts the CVD method to prepare silicon carbide material, and sets the deposition temperature to 1000-1500°C, the deposition pressure to 9000-40,000Pa, and the flow ratio of carbon silane to reducing gas to 1:(1-40), the prepared silicon carbide material has high purity, high density and high resistivity, and can meet the requirements of semiconductor etching materials.

[0179] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0180] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing silicon carbide material, It is characterized in that The following steps are involved: (1) providing a substrate, and placing the substrate in a vacuum chemical vapor deposition device for heating; (2) introducing a dilution gas and a reaction gas into a chemical vapor deposition device, wherein the reaction gas includes carbosilane and a reducing gas, the dilution gas is argon, and the volume fraction of the dilution gas is 42%-50%. The deposition process parameters are set as follows: the deposition temperature is 1275° C.-1350° C., the deposition pressure is 20000 Pa-25000 Pa, and the flow ratio of carbosilane to reducing gas is 1:(15-25); (3) After the chemical vapor deposition is completed, the dilution gas and the reaction gas are stopped to obtain silicon carbide; the purity of the silicon carbide material is greater than 99.9999%, the average particle size of the silicon carbide material is 0.05 μm-0.8 μm, the proportion of high-angle grain boundaries of the silicon carbide material greater than 10° is greater than or equal to 55% and less than 85%, and the average dislocation density of the silicon carbide material is (50-140)×10 14 / m 2 The resistivity of the silicon carbide material is 20kΩ.cm-50kΩ.cm.

2. The method for preparing silicon carbide material according to claim 1, It is characterized in that The carbosilane hydrocarbon includes at least one of monosilane, disilane, trisilane, methylchlorosilane, dimethylchlorosilane or trichloromethylsilane; and / or, the reducing gas comprises: at least one of hydrogen, methane, ethylene or acetylene; And / or, the substrate is a carbon-based material and / or a silicon-based material.

3. The method for preparing silicon carbide material according to claim 2, It is characterized in that The carbosilane includes trichloromethylsilane.

4. Use of the method according to any one of claims 1 to 3 in preparing high resistivity materials.

5. The silicon carbide material prepared by the method according to any one of claims 1 to 3, wherein the porosity of the silicon carbide material is 0.01% to 0.1%.

6. The silicon carbide material according to claim 5, It is characterized in that The silicon carbide material satisfies at least one of the following: (a) The grain boundary barrier of the silicon carbide material is 0.05ev-1ev; (b) The carrier concentration of the silicon carbide material is less than 10 15 (1 / cm 3 ).

7. The silicon carbide material according to claim 5 or 6, It is characterized in that The silicon carbide material is 3C-SiC with a cubic structure and a (111) single orientation.

Citation Information

Patent Citations

  • High-purity silicon carbide ceramic manufacturing method and ceramic base material

    CN105732044A

  • Method for preparing silicon carbide ceramic material, application and silicon carbide ceramic material