A kind of automobile original low-temperature stone-impact resistant water-based mid-coat coating and its preparation method and application

By using a water-based intermediate coating composed of aliphatic hydroxyl functional polycarbonate polyurethane, etc., the problems of insufficient low-temperature stone impact resistance and surface smoothness of the existing intermediate coatings are solved, and high adhesion, flexibility and surface smoothness are achieved. Fast drying effect, suitable for automobile painting process.

CN118222168BActive Publication Date: 2024-10-29GUANGDONG YATU CHEM
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410209843.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-26
Publication Date
2024-10-29
Estimated Expiration
2044-02-26

AI Technical Summary

Technical Problem

Existing automotive intermediate coatings have deficiencies in low-temperature stone impact resistance and surface smoothness, making it difficult to meet high adhesion, gloss and workability requirements at the same time.

Method used

A water-based intermediate coating composed of aliphatic hydroxyl functional polycarbonate polyurethane dispersion, water-based aliphatic polyurethane-urea dispersion, water-based blocked polyisocyanate cross-linking agent, amino resin, etc., prepared through a specific mixing and sanding process , forming a paint film with high adhesion, flexibility and impact resistance.

Benefits of technology

It achieves good stone impact resistance, adhesion and gloss under low temperature conditions, and has fast drying and excellent workability. It is suitable for coating processes with thin film thickness, ensuring the appearance and performance of automotive coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to a kind of automobile original factory low temperature stone impact resistant water-based mid-coat coating and its preparation method and application, the mid-coat coating composition includes aliphatic hydroxyl functional polycarbonate polyurethane dispersion, water-based aliphatic polyurethane-urea dispersion, water-based closed polyisocyanate crosslinking agent, amino resin, dispersant, defoamer, wetting agent, pigment, filler, fumed silica, cosolvent and water. The coating crosslinking density obtained by the modified polyurethane resin, amino resin and isocyanate crosslinking agent system adopted in the present invention is high, and the toughness is good, and the anti-stone impact performance is significantly improved, especially the anti-low temperature stone impact performance can reach level 1, and the mid-coat coating of the present invention is quick-drying, easy to construct, has higher gloss and fullness, leveling, good adhesion and water resistance, and is equipped with automobile original factory color paint and varnish, and can be widely used in electrophoretic coating or metal substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to an original automobile low-temperature stone-impact resistant water-based mid-coat and a preparation method and application thereof. Background Art

[0002] The midcoat is an important auxiliary function between the primer and the topcoat. On the one hand, it can cover the defects of the substrate and ensure the smoothness of the surface after the topcoat is applied. On the other hand, it can make the coating film resistant to stone impact and prevent stones from damaging the primer when impacting the coating film. Usually, the primer cannot be repaired. It can be seen that the existence of the midcoat is very important and critical to the coating process and coating performance. At present, there is also a coating technology without a midcoat in the existing technology, but the appearance and stone impact resistance of the paint after coating are far worse than those of the midcoat. It can be seen that the midcoat is still the mainstream technology in the current coating technology.

[0003] There are many types of mid-coat coatings for automobile bodies, such as phenolic resin, alkyd resin, epoxy resin, amino resin, etc. However, the mid-coat using traditional high-temperature baking varnish has poor stone impact resistance (especially low-temperature stone impact resistance), while the mid-coat prepared by epoxy resin and amino resin system has high adhesion and has become the most widely used resin system for mid-coat. Chinese patent CN107057537A discloses a water-based mid-coat for automobiles. The mid-coat is made of water-soluble polyester resin, emulsion polyester resin, and water-based epoxy resin system, and is obtained by adding additives and stirring. The stone impact resistance of the mid-coat reaches level 1~3, the impact strength is 295~310N·cm, and the water resistance reaches NO.10 of ASTMD714-87, but the surface of the mid-coat is smooth. Poor; CN105754463A discloses a water-based automotive mid-coat, which adopts a water-based polyester resin, a water-based epoxy resin, and a water-based methyl ether amino resin system, and is obtained by amino coupling in a closed water-based isocyanate-cured manner. The mid-coat has a smooth paint film and good adhesion, and the pencil hardness can reach F grade, but its stone impact resistance is insufficient; in addition, CN115074011A discloses a water-based automotive original mid-coat, which is prepared by a water-based acrylic ester polyurethane dispersion, a water-based hydroxy acrylic dispersion, a water-based polyester, an amino resin, and dimethylethanolamine or AMP-95. The mid-coat has good adhesion, but the hardness is HB, which is still slightly insufficient, and the mid-coat film has insufficient stone impact resistance and is difficult to protect the primer.

[0004] It can be seen that multiple performance parameters of mid-coat coatings are still difficult to optimize with current existing technologies, which is an urgent problem to be solved. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention provides an original automobile water-based mid-coat paint with low-temperature stone impact resistance, and a preparation method and application thereof. The paint film prepared by the present invention has good adhesion and water resistance to electrophoretic coatings or metal substrates, high gloss and fullness, fast drying speed, and high workability. At the same time, because the mid-coat has good flexibility and impact resistance, it is particularly suitable for the current original automobile paint mid-coat spraying film thickness of a water-based B1B2 process + an oily high-solid 2K varnish matching system (the B1 mid-coat is generally only sprayed with 12~14um), which can ensure the appearance and construction, and at the same time, the stone impact resistance performance is still very excellent when the mid-coat is constructed with a low film thickness.

[0006] In the first aspect, the present invention provides an original automobile low-temperature stone-impact resistant water-based mid-coat, the raw material composition of the coating includes aliphatic hydroxyl-functional polycarbonate polyurethane dispersion, water-based aliphatic polyurethane-urea dispersion, water-based blocked polyisocyanate cross-linker, amino resin, dispersant, defoamer, wetting agent, pigment, filler, fumed silica, cosolvent and water.

[0007] Further, the co-solvent is selected from one or more of ethylene glycol butyl ether, isooctyl alcohol, and dimethylethanolamine (DMEA);

[0008] Furthermore, the mass ratio of ethylene glycol butyl ether, isooctyl alcohol and dimethylethanolamine in the co-solvent is 1-5:1-5:0.1;

[0009] Preferably, the mass ratio of ethylene glycol butyl ether, isooctyl alcohol and dimethylethanolamine in the co-solvent is 2:2.5:0.1.

[0010] Furthermore, the pigment is selected from one or more of titanium dioxide, black iron oxide, yellow iron oxide, and red iron oxide.

[0011] Furthermore, the filler is selected from one or more of superfine barium sulfate and superfine talc;

[0012] Preferably, the ultrafine talc powder is 3000 mesh, and the ultrafine barium sulfate is 2500 mesh.

[0013] Furthermore, the raw material composition of the coating includes, by weight, 10 to 30 parts of aliphatic hydroxyl-functional polycarbonate polyurethane dispersion, 10 to 30 parts of aqueous aliphatic polyurethane-urea dispersion, 3 to 8 parts of aqueous blocked polyisocyanate crosslinking agent, 2 to 6 parts of amino resin, 0.3 to 1 part of dispersant, 0.1 to 1 part of defoamer, 0.1 to 1 part of wetting agent, 20 to 35 parts of pigment / filler, 0.1 to 1 part of fumed silica, 1 to 10 parts of cosolvent and 2 to 30 parts of water.

[0014] Preferably, the raw material composition of the coating includes, by mass, 24.6 parts of aliphatic hydroxyl-functional polycarbonate polyurethane dispersion, 10 parts of aqueous aliphatic polyurethane-urea dispersion, 5.7 parts of aqueous blocked polyisocyanate crosslinker, 3 parts of amino resin, 0.6 parts of dispersant, 0.3 parts of defoamer, 0.3 parts of wetting agent, 21.5 parts of pigment, 10 parts of filler, 0.6 parts of fumed silica, 4.6 parts of cosolvent, and 18.8 parts of water.

[0015] In a second aspect, the present invention further provides a method for preparing the original low-temperature stone-impact resistant water-based mid-coat for automobiles, the method comprising the following steps:

[0016] S1. Add aliphatic hydroxyl functional polycarbonate polyurethane dispersion and part of water into a container, and stir at a speed of 300-600 r / min for 5-45 min;

[0017] S2, adding part of the cosolvent, dispersant, defoamer, pigment, filler, and fumed silica to step S1 in sequence while stirring, and after the addition is completed, dispersing at 600-800 r / min for 5-60 min to obtain a mixed solution;

[0018] S3, sand-milling the mixed solution of step S2 in a horizontal sand mill, with the sand-milling temperature controlled below 40°C and the flow rate 10-15 L / min, sand-milling to a fineness of less than 10 μm, and cooling to room temperature for standby use;

[0019] S4, adding a polyester-based acrylic acid-modified high molecular weight polyurethane dispersion, a water-based blocked polyisocyanate crosslinking agent, an amino resin, and a wetting agent to step S3 while stirring, and after the addition is completed, dispersing at 600-800 r / min for 5-60 minutes;

[0020] S5. Add the remaining co-solvent and water to step S4 while stirring, adjust the pH value to 8.5±0.1, and the viscosity to 900±100 mPa.s / 3# rotor, 60RPM, 23°C (Brookfield RVDV2T viscometer), to obtain the original low-temperature stone-imping resistant water-based mid-coat coating for automobiles.

[0021] In a third aspect, the automobile original equipment low-temperature stone impact resistant water-based mid-coat described in the present invention can be used in, including but not limited to, automobile original equipment paint and automobile spare parts paint.

[0022] The coating composed of the aliphatic hydroxyl-functional polycarbonate polyurethane dispersion and the water-based blocked polyisocyanate crosslinker used in the present invention is supplied in the form of a single-component coating commonly used in the industry. During the use of the original coating, after being baked at a high temperature of 140°C, the hydroxyl groups of the aliphatic hydroxyl-functional polycarbonate polyurethane dispersion are cross-linked with the water-based blocked polyisocyanate crosslinker to form a paint film with high crosslinking density and good toughness, which greatly improves the stone chip resistance (especially low-temperature stone chip resistance) of traditional high-temperature baking paint using amino resin as a crosslinker.

[0023] The present invention also uses a water-based aliphatic polyurethane-urea dispersion with a particularly high molecular weight, quick drying, and high flexibility, which can provide a clear, crack-free, and highly flexible film. The aliphatic polyurethane-urea dispersion is applied to the formula to obtain a coating with a higher elongation, thereby making the coating have higher flexibility, thereby achieving the effect of further improving low-temperature stone impact resistance.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The automobile original low-temperature stone-impact resistant water-based mid-coat of the present invention is easy to apply, has good appearance and leveling properties, and is matched with automobile original color paint and varnish. The obtained paint film has a stone-impact resistance test result of level 1 under -40°C conditions, with almost no peeling, and has very good adhesion of level 0. The pendulum hardness (P pendulum) can reach 182, and has excellent water resistance, solvent resistance, acid and alkali resistance, chemical resistance, moisture and heat resistance, aging resistance and other properties.

[0026] (2) The original automobile low-temperature stone-impact resistant water-based mid-coat paint film prepared by the present invention has good adhesion and water resistance to the electrophoretic coating or metal substrate, high gloss and fullness, fast drying speed, and high workability. At the same time, because the mid-coat has good flexibility and impact resistance, it is particularly suitable for the current original automobile paint mid-coat spraying film thickness of the water-based B1B2 process + oil-based high-solid 2K varnish matching system (B1 mid-coat is generally only sprayed 12~14um), which can ensure the appearance and construction, and at the same time, the stone-impact resistance performance is still very excellent when the mid-coat is constructed with a low film thickness. DETAILED DESCRIPTION

[0027] The experimental methods in the following examples of the present invention, where no specific conditions are specified, are usually carried out under conventional conditions or under conditions recommended by the manufacturers. The various commonly used chemical reagents used in the examples are all commercially available products.

[0028] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0029] The terms "including" and "having" and any variations thereof of the present invention are intended to cover non-exclusive inclusions. For example, a process, method, device, product or equipment comprising a series of steps is not limited to the listed steps or modules, but may optionally include steps not listed, or may optionally include other steps inherent to these processes, methods, products or equipment.

[0030] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0031] The present invention is further described in the following examples, but the examples are not intended to limit the scope of protection of the present invention.

[0032] The sources and types of the reagents, raw materials and other components used in the examples of the present invention are specifically shown in Table 1;

[0033] Table 1: Sources and models of some ingredients

[0034]

[0035] Example 1 Preparation of original low-temperature stone-impact resistant water-based mid-coat for automobiles

[0036] The formula of the original low-temperature stone-impact resistant water-based mid-coat paint prepared in this embodiment is shown in Table 2;

[0037] Table 2: Composition formula of automobile original low temperature stone impact resistant water-based mid-coat

[0038]

[0039] According to the formula composition in Table 2, the specific preparation steps of the original low-temperature stone-impact resistant water-based mid-coat coating for automobiles in this embodiment are as follows:

[0040] S1. Add aliphatic hydroxyl functional polycarbonate polyurethane dispersion and 1 / 2 mass part of water into a container, and stir at a speed of 300-600 r / min for 15 min;

[0041] S2, in step S1, adding ethylene glycol butyl ether, isooctyl alcohol, dispersant, defoamer, titanium dioxide, black iron oxide, yellow iron oxide, red iron oxide, ultrafine barium sulfate, ultrafine talc, and fumed silica in sequence while stirring, after the addition is completed, dispersing at 600-800 r / min for 30 min to obtain a mixed solution;

[0042] S3, after the dispersion is completed, the mixed solution of step S2 is put into a horizontal sand mill for sand grinding, the sand grinding temperature is controlled below 40°C, the flow rate is 10-15L / min, the sand grinding is performed to a fineness of less than 10μm, and the mixture is cooled to room temperature for standby use;

[0043] S4, adding aqueous aliphatic polyurethane-urea dispersion, aqueous blocked polyisocyanate crosslinking agent, amino resin and wetting agent to the step S3 with qualified grinding fineness while stirring, and after the addition is completed, dispersing at a medium speed of 600-800 r / min for 30 min;

[0044] S5. In the dispersed step S4, DMEA and the remaining water are added while stirring, and the pH value is adjusted to 8.5±0.1, and the viscosity is 900±100 mPa.s / 3# rotor, 60RPM, 23°C (Brookfield RVDV2T viscometer), to obtain the original low-temperature stone-impact resistant water-based mid-coat coating for automobiles.

[0045] Example 2 Preparation of original low-temperature stone-impact resistant water-based mid-coat for automobiles

[0046] The formula of the original low-temperature stone-impact resistant water-based mid-coat paint prepared in this embodiment is shown in Table 3;

[0047] Table 3: Composition formula of automobile original low temperature stone impact resistant water-based mid-coat

[0048]

[0049] According to the formula composition in Table 3, the specific preparation steps of the original low-temperature stone-impact resistant water-based mid-coat coating for automobiles in this embodiment are as follows:

[0050] S1. Add aliphatic hydroxyl functional polycarbonate polyurethane dispersion and 1 / 2 mass part of water into a container, and stir at a speed of 300-600 r / min for 15 min;

[0051] S2, in step S1, adding ethylene glycol butyl ether, isooctyl alcohol, dispersant, defoamer, titanium dioxide, black iron oxide, yellow iron oxide, red iron oxide, ultrafine barium sulfate, ultrafine talc, and fumed silica in sequence while stirring, after the addition is completed, dispersing at 600-800 r / min for 30 min to obtain a mixed solution;

[0052] S3, after the dispersion is completed, the mixed solution of step S2 is put into a horizontal sand mill for sand grinding, the sand grinding temperature is controlled below 40°C, the flow rate is 10-15L / min, the sand grinding is performed to a fineness of less than 10μm, and the mixture is cooled to room temperature for standby use;

[0053] S4, adding water-based aliphatic polyurethane-urea dispersion, water-based blocked polyisocyanate crosslinking agent, amino resin and wetting agent to the step S3 with qualified grinding fineness while stirring, and after the addition is completed, dispersing at 600-800 r / min for 30 minutes;

[0054] S5. In the dispersed step S4, DMEA and the remaining water are added while stirring, and the pH value is adjusted to 8.5±0.1, and the viscosity is 900±100 mPa.s / 3# rotor, 60RPM, 23°C (Brookfield RVDV2T viscometer), to obtain the original low-temperature stone-impact resistant water-based mid-coat coating for automobiles.

[0055] Example 3 Preparation of original low-temperature stone-impact resistant water-based mid-coat for automobiles

[0056] The formula of the original low-temperature stone-impact resistant water-based mid-coat paint prepared in this embodiment is shown in Table 4;

[0057] Table 4: Composition formula of automobile original low temperature stone impact resistant water-based mid-coat

[0058]

[0059] According to the formula composition in Table 4, the specific preparation steps of the original low-temperature stone-impact resistant water-based mid-coat coating for automobiles in this embodiment are as follows:

[0060] S1. Add aliphatic hydroxyl functional polycarbonate polyurethane dispersion and 1 / 2 mass part of water into a container, and stir at a speed of 300-600 r / min for 15 min;

[0061] S2, in the stirred step S1, ethylene glycol butyl ether, isooctyl alcohol, dispersant, defoamer, titanium dioxide, black iron oxide, yellow iron oxide, red iron oxide, ultrafine barium sulfate, ultrafine talc, and fumed silica are added in sequence while stirring. After the addition is completed, disperse at 600-800 r / min for 30 minutes to obtain a mixed solution;

[0062] S3, after the dispersion is completed, the mixed solution of step S2 is put into a horizontal sand mill for sand grinding, the sand grinding temperature is controlled below 40°C, the flow rate is 10-15L / min, the sand grinding is performed to a fineness of less than 10μm, and the mixture is cooled to room temperature for standby use;

[0063] S4, adding water-based aliphatic polyurethane-urea dispersion, water-based blocked polyisocyanate crosslinking agent, amino resin and wetting agent to the step S3 with qualified grinding fineness while stirring, and after the addition is completed, dispersing at 600-800 r / min for 30 minutes;

[0064] S5. In the dispersed step S4, DMEA and the remaining water are added while stirring, and the pH value is adjusted to 8.5±0.1, and the viscosity is 900±100 mPa.s / 3# rotor, 60RPM, 23°C (Brookfield RVDV2T viscometer), to obtain the original low-temperature stone-impact resistant water-based mid-coat coating for automobiles.

[0065] Test Example 1: Performance test of automobile original low-temperature stone-impact resistant water-based midcoat

[0066] The performance of the original low-temperature stone-impact resistant water-based mid-coat prepared in Examples 1 to 3 was tested. The specific test methods and test results are shown in Tables 5 and 6, respectively.

[0067] Table 5: Performance test method of automobile original low temperature stone impact resistant water-based midcoat coating

[0068]

[0069] The specific steps of the low temperature stone impact test method in Table 5 are as follows:

[0070] Use MULTI GRIT TESTER 508VDA (manufactured by ERICHSEN) at 5kgf / cm 2 500 g of Chilled Iron Grit (G-9652-X) was applied to the composite coating of the sample cooled at -40°C from a distance of 35 cm at an angle of 45° under an air pressure of 100 °C. After washing and drying, the composite coating was peeled off with an industrial tape manufactured by 3M to remove the coating fragments. Then, the degree of peeling of the coating was visually evaluated. The peeling state of the coating was evaluated according to the following evaluation criteria:

[0071] Level 1: Almost no peeling

[0072] Level 2: Only a little peeling but no problem with appearance

[0073] Level 3: The peeling is slightly larger or more, and the appearance is problematic

[0074] Level 4: Large or more peeling

[0075] Level 5: The peeling is obviously larger or more

[0076] The original low-temperature stone-impact resistant water-based mid-coat coatings for automobiles prepared in Examples 1 to 3 were tested according to the performance test method in Table 5 above, and the results obtained are shown in Table 6;

[0077] Table 6: Performance test results of automobile original low temperature stone impact resistant water-based midcoat coating

[0078]

[0079] Conclusion: From the performance results in Table 6, it can be seen that the original low-temperature stone-impact resistant water-based mid-coat prepared in Examples 1 to 3 has a good paint film appearance, normal mechanical properties and chemical resistance, excellent low-temperature stone-impact resistance, and the low-temperature stone-impact resistance (-40°C) can reach level 1.

[0080] Comparative Example 1 Preparation of original low-temperature stone-impact resistant water-based mid-coat for automobiles

[0081] The formula of the original low-temperature stone-impact resistant water-based mid-coat prepared in this comparative example differs from the formula of Example 3 in the changes in the components and contents of the resin and the cross-linking agent, as shown in Table 7;

[0082] Table 7: Composition formula of automobile original low temperature stone impact resistant water-based midcoat

[0083]

[0084] According to the formula composition in Table 7, the specific preparation steps of the original automobile low-temperature stone impact resistant water-based mid-coat paint in this comparative example are consistent with those in Example 3.

[0085] Comparative Example 2 Preparation of original low-temperature stone-impact resistant water-based mid-coat for automobiles

[0086] The formula of the original low-temperature stone-impact resistant water-based mid-coat prepared in this comparative example differs from the formula of Example 3 in the changes in the components and contents of the resin and the cross-linking agent, as shown in Table 8 for details;

[0087] Table 8: Composition formula of automobile original low temperature stone impact resistant water-based mid-coat

[0088]

[0089] According to the formula composition in Table 8, the specific preparation steps of the original automobile low-temperature stone impact resistant water-based mid-coat paint in this comparative example are consistent with those in Example 3.

[0090] Comparative Example 3 Preparation of original low-temperature stone-impact resistant water-based mid-coat for automobiles

[0091] The formula of the original low-temperature stone-impact resistant water-based mid-coat prepared in this comparative example differs from the formula of Example 3 in the changes in the components and contents of the resin and the cross-linking agent, as shown in Table 9;

[0092] Table 9: Composition formula of automobile original low temperature stone impact resistant water-based mid-coat

[0093]

[0094] According to the formula composition in Table 9, the specific preparation steps of the original automobile low-temperature stone impact resistant water-based mid-coat paint in this comparative example are consistent with those in Example 3.

[0095] Comparative Example 4 Preparation of original low-temperature stone-impact resistant water-based mid-coat for automobiles

[0096] The formula of the original low-temperature stone-impact resistant water-based mid-coat prepared in this comparative example differs from that of Example 3 in the changes in the components and contents of the resin and the cross-linking agent, as shown in Table 10.

[0097] Table 10: Composition formula of automobile original low temperature stone impact resistant water-based midcoat

[0098]

[0099] According to the formula composition in Table 10, the specific preparation steps of the original automobile low-temperature stone impact resistant water-based mid-coat paint in this comparative example are consistent with those in Example 3.

[0100] Comparative Example 5 Preparation of original low-temperature stone-impact resistant water-based mid-coat for automobiles

[0101] The formula of the original low-temperature stone-impact resistant water-based mid-coat prepared in this comparative example differs from the formula of Example 3 in the changes in the components and contents of the resin and the cross-linking agent, as shown in Table 11;

[0102] Table 11: Composition formula of automobile original low temperature stone impact resistant water-based midcoat

[0103]

[0104] Comparative Example 6

[0105] The formula of the original low-temperature stone-impact resistant water-based mid-coat for automobiles prepared in this comparative example is different from the formula of Example 3 in that the co-solvent contains 3.2 g of ethylene glycol butyl ether, 0.8 g of isooctyl alcohol, and 0.6 g of DMEA, and the rest are the same.

[0106] Comparative Example 7

[0107] This comparative example was prepared according to the formulation of Example 1 disclosed in CN115074011A.

[0108] Test Example 2: Performance test of the original low-temperature stone-impact resistant water-based midcoat coating for automobiles

[0109] The performance of the original low-temperature stone-impact resistant water-based mid-coat coatings prepared in Comparative Examples 1 to 7 was tested. The specific test method is the same as Table 5, and the test results are shown in Table 12;

[0110] Table 12: Performance test results of automobile original low temperature stone impact resistant water-based midcoat coating

[0111]

[0112] Conclusion: From the performance results in Table 12, it can be seen that the original low-temperature stone-impact resistant water-based mid-coat prepared in Comparative Example 1 does not use a water-based blocked polyisocyanate cross-linking agent, and the low-temperature stone-impact resistance of the paint film is significantly deteriorated; the original low-temperature stone-impact resistant water-based mid-coat prepared in Comparative Example 2 uses a water-based epoxy resin instead of a water-based aliphatic polyurethane-urea dispersion, and the pendulum hardness and gasoline resistance of the paint film are seriously reduced, and the low-temperature stone-impact resistance is also significantly deteriorated; the original low-temperature stone-impact resistant water-based mid-coat prepared in Comparative Example 3 does not use an amino resin in the formula, and the gasoline resistance of the paint film is reduced, and the low-temperature stone-impact resistance is also deteriorated; the original low-temperature stone-impact resistant water-based mid-coat prepared in Comparative Example 4 has a reduced content of water-based aliphatic polyurethane-urea dispersion and an increased content of cross-linking agent amino resin. The pendulum hardness of the paint film is significantly increased, but the mechanical properties such as impact resistance and bending resistance are very poor, and the low-temperature stone impact resistance is very poor; the original low-temperature stone impact resistant water-based mid-coat prepared in Example 5 uses water-based polyester resin to replace the aliphatic hydroxyl functional polycarbonate polyurethane dispersion, and the gasoline resistance of the paint film is significantly reduced, which does not meet the original paint use requirements; the original low-temperature stone impact resistant water-based mid-coat prepared in Example 6 has a changed co-solvent composition, poor paint film flatness, and reduced gasoline resistance and low-temperature stone impact resistance; the original low-temperature stone impact resistant water-based mid-coat prepared in Example 7 has a low pendulum hardness of the composite coating, and does not meet the low film thickness (generally 12~14um) construction requirements of the original new compact B1B2 process, and the low-temperature stone impact (-40℃) performance is far from sufficient.

[0113] It should be noted that the specific features, structures, materials or characteristics described in this specification can be combined arbitrarily. In order to make the description concise, not all possible combinations of the various technical features in the above embodiments are described. If there is no contradiction, technicians in this field can combine and combine the different embodiments and features of different embodiments described in this specification.

[0114] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A kind of original low temperature stone impact resistant water-based mid-coat paint for automobiles. It is characterized in that The raw material composition of the midcoat coating includes 10 to 30 parts of aliphatic hydroxyl functional polycarbonate polyurethane dispersion, 10 to 30 parts of aqueous aliphatic polyurethane-urea dispersion, 3 to 8 parts of aqueous blocked polyisocyanate crosslinker, 2 to 6 parts of amino resin, 0.3 to 1 part of dispersant, 0.1 to 1 part of defoamer, 0.1 to 1 part of wetting agent, 15 to 35 parts of pigment, 5 to 15 parts of filler, 0.1 to 1 part of fumed silica, 1 to 10 parts of cosolvent and 2 to 30 parts of water. The aliphatic hydroxyl functional polycarbonate polyurethane dispersion is Covestro resin. U XP 2757, the aqueous aliphatic polyurethane-urea dispersion is an allnex resin TW6431 / 45WA, the water-based blocked polyisocyanate crosslinker is HD-850 from Changzhou Houding Chemical, and the amino resin is Allnex amino resin 370.

2. The original low-temperature stone-impact resistant water-based mid-coat for automobiles according to claim 1, It is characterized in that The pigment is selected from one or more of titanium dioxide, black iron oxide, yellow iron oxide and red iron oxide.

3. The original low-temperature stone-impact resistant water-based mid-coat for automobiles according to claim 1, It is characterized in that The filler is selected from one or more of superfine barium sulfate and superfine talc.

4. The original low-temperature stone-impact resistant water-based mid-coat for automobiles according to claim 1, It is characterized in that The co-solvent is selected from one or more of ethylene glycol butyl ether, isooctyl alcohol, and dimethylethanolamine.

5. The original low-temperature stone-impact resistant water-based mid-coat for automobiles according to claim 4, It is characterized in that The cosolvent is composed of ethylene glycol butyl ether, isooctyl alcohol and dimethylethanolamine in a mass ratio of 1 to 5:1 to 5:0.

1.

6. The original low-temperature stone-impact resistant water-based mid-coat for automobiles according to claim 1, It is characterized in that Calculated by mass, the raw material composition of the mid-coat coating includes 24.6 parts of aliphatic hydroxyl-functional polycarbonate polyurethane dispersion, 10 parts of aqueous aliphatic polyurethane-urea dispersion, 5.7 parts of aqueous blocked polyisocyanate crosslinker, 3 parts of amino resin, 0.6 parts of dispersant, 0.3 parts of defoamer, 0.3 parts of wetting agent, 21.5 parts of pigment, 10 parts of filler, 0.6 parts of fumed silica, 4.6 parts of cosolvent, and 18.8 parts of water.

7. A method for preparing the original low-temperature stone-impact resistant water-based mid-coat for automobiles according to any one of claims 1 to 6, It is characterized in that The method comprises the following steps: S1. Add aliphatic hydroxyl functional polycarbonate polyurethane dispersion and part of water into a container, and stir at a speed of 300 to 600 r / min for 5 to 45 minutes; S2, adding part of the cosolvent, dispersant, defoamer, pigment, filler, and fumed silica to step S1 in sequence while stirring, and dispersing at 600-800 r / min for 5-60 min to obtain a mixed solution; S3, sand-grind the mixed solution of step S2, with the sand-grinding temperature controlled below 40°C and the flow rate 10-15 L / min, sand-grind to a fineness of less than 10 μm, and cool to room temperature for standby use; S4, adding the aqueous aliphatic polyurethane-urea dispersion, aqueous blocked polyisocyanate crosslinking agent, amino resin, and wetting agent to step S3 while stirring, and after the addition is completed, dispersing at 600-800 r / min for 5-60 min; S5. In step S4, the remaining co-solvent and the remaining water are added while stirring, and the pH value and viscosity are adjusted to obtain the original automobile low-temperature stone-impact resistant water-based mid-coat.

8. The method for preparing the original low-temperature stone-impact resistant water-based mid-coat for automobiles according to claim 7, It is characterized in that The pH in step S5 is 8.5±0.

1.

9. The method for preparing the original low-temperature stone-impact resistant water-based mid-coat for automobiles according to claim 7, It is characterized in that The viscosity in step S5 is 900±100 mPa.s.

10. Use of the automobile original low-temperature stone-impact resistant water-based mid-coat according to any one of claims 1 to 6 in electrophoretic coatings and metal substrates.

Citation Information

Patent Citations

  • Automotive waterborne floating-coat coating and preparation method thereof

    CN105754463A

  • Water-based middle coating for automobile and preparation method thereof

    CN107057537A

  • Water-based automobile original factory floating coating and preparation method thereof

    CN115074011A

  • A waterborne automobile coating composition and a preparing method and applications thereof

    CN107099238A