Preparation method and application of high-toughness wear-resistant polyethylene composite plastic
By using materials such as polyvinylpyrrolidone, water-soluble carboxymethyl chitosan and silicon carbide fiber in polyethylene film gloves, combined with a three-layer structure design and palm oil homogenization treatment, the leakage and cracking of polyethylene film gloves are solved problem, improves usage and durability, and reduces resource waste.
Patent Information
- Application Number
- CN202410816403.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polyethylene film gloves are prone to leakage and fingertip seam cracking during use, and need to be replaced after one-time use, resulting in a high waste rate and a waste of resources.
Polyvinylpyrrolidone and water-soluble carboxymethyl chitosan are used to improve the hot-pressing bonding and sealing properties, silicon carbide fiber enhances toughness and wear resistance, and the overall performance of the gloves is improved through a three-layer structure design and palm oil homogenization treatment. .
Significantly improves the hot-pressure bonding sealing and crack resistance of gloves, prolongs service life, doubles usage rate, reduces replacement frequency, and saves resources.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of plastic molding products, and in particular relates to a preparation method and application of a high-toughness wear-resistant polyethylene composite plastic. Background Art
[0002] Polyethylene (PE) film gloves are a type of transparent disposable film gloves, commonly used in the medical or food industry, such as disposable medical gloves and disposable dining gloves, and are consumables with huge usage.
[0003] The usual method for preparing polyethylene film gloves is to use a film blowing machine to blow the plastic raw material into a cylindrical film, and then use a glove machine to heat seal both sides and cut them into gloves. For example, CN103881178A discloses a disposable film glove and a preparation method thereof, and CN106977888A discloses a disposable film glove and a preparation method thereof.
[0004] However, polyethylene film gloves are still commonly leaking, especially at the heat-sealed seams on both sides of the gloves, which are prone to leakage and even cracking during use. For example, when wearing gloves to eat hand-held food (such as fried chicken), oil will still seep into the gloves through the seams of the edges and stain the hands. When preparing cold dishes, film gloves are often worn to mix vegetables. During the friction and squeezing process of mixing vegetables, the fingertips of the film gloves are easily punctured and cracked, and they cannot provide good protection.
[0005] Therefore, polyethylene film gloves are prone to leakage and the fingertip seams are prone to cracking, which has always been a difficult problem to solve. In addition, after leakage or cracking, disposable gloves need to be interrupted and replaced with new gloves. They cannot be reused, and the discard rate is very high, which is a great waste of resources. Summary of the invention
[0006] The existing polyethylene disposable film gloves are easy to leak, the fingertips are easy to crack, they cannot be reused, the discard rate is very high, and resources are wasted. The present invention provides a preparation method and application of high-toughness wear-resistant polyethylene composite plastics. Adding polyvinyl pyrrolidone and water-soluble carboxymethyl chitosan in the coating method can improve the hot pressing bonding and thermosetting sealing of the gloves; adding silicon carbide fiber can improve the toughness and tear resistance; adding silicon carbide in the coating method can improve the wear resistance and further improve the toughness; adding palm oil can improve the homogeneity and smoothness of the mixed film blowing, so that the quality of the plastic film film blowing is more uniform, less prone to weak parts, and less prone to cracking under stress. The three-layer structure of the film gloves is designed to isolate and form two glove cavities. Compared with disposable gloves, they can be used twice, and the utilization rate is doubled. In particular, during use, if one cavity of the glove leaks, it can be replaced by another cavity in time, and the gloves do not need to be discarded, saving replacement costs and resources. The specific technical scheme is as follows:
[0007] A method for preparing a high-toughness wear-resistant polyethylene composite plastic comprises the following steps:
[0008] S1, raw material preparation:
[0009] Solution A was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan = 100: (2-5): (3-8); and the mixture was uniformly mixed, dried, and dispersed at a mass ratio of polyethylene: solution A = 100: (40-80) to obtain a composite B;
[0010] Mixed solution C is prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan: silicon carbide = 100: (2-4): (2-4): (3-8); silicon carbide fiber and mixed solution C are sprayed on the surface of silicon carbide fiber by fluidized spraying method at a mass ratio of silicon carbide fiber: mixed solution C = 100: (20-30), dried, and dispersed to obtain a composite D;
[0011] S2, Mixing and Film Blowing:
[0012] According to the mass ratio of compound B:compound D:palm oil = (90-100): (3-8): (0.5-5), compound B, compound D and palm oil are mixed and blown to obtain a cylindrical film, i.e., a high-toughness and wear-resistant polyethylene composite plastic.
[0013] In S1 of the above technical solution, the parameters of the fluidized spray are: the inlet temperature of the mixed liquid C is 20°C to 30°C, the spray speed is 0.5L / min to 0.8L / min; the atomization pressure is 0.6MPa to 0.8MPa; and the discharge temperature is 40°C to 50°C.
[0014] In S1 of the above technical solution, the drying temperature is 60°C to 80°C.
[0015] In S1 of the above technical solution, the particle size of the polyethylene is 50 μm to 300 μm.
[0016] In S1 of the above technical solution, the particle size of the silicon carbide is less than 500 nm.
[0017] In S1 of the above technical solution, the diameter of the silicon carbide fiber is 0.5 μm to 2 μm, and the length is less than 0.3 mm.
[0018] In the above technical scheme, the raw materials are all food grade or pharmaceutical grade.
[0019] The above-mentioned high-toughness wear-resistant polyethylene composite plastic is used to prepare film gloves. The method for preparing the film gloves comprises the following steps:
[0020] N1, slice superposition, choose one of the following three methods: N1.1, N1.2 and N1.3:
[0021] N1.1: Cutting the cylindrical film sideways to obtain a polyethylene composite plastic film sheet; stacking the polyethylene composite plastic film sheet into a three-layer structure to obtain a three-layer film, and winding the film into a roll;
[0022] N1.2: Cut the cylindrical film sideways to obtain a polyethylene composite plastic film sheet; stack the polyethylene film sheet-polyethylene composite plastic film sheet-polyethylene film sheet into a three-layer structure to obtain a three-layer film, and wind it into a roll;
[0023] N1.3: Cut the cylindrical film sideways to obtain a polyethylene composite plastic film sheet; stack the polyethylene composite plastic film sheet-polyethylene film sheet-polyethylene composite plastic film sheet into a three-layer structure to obtain a three-layer film, and wind it into a roll;
[0024] N2, heat sealing and cutting:
[0025] The three-layer film is transported to the glove machine for heat sealing and cutting into gloves.
[0026] In N2 of the above technical solution, there is a middle diaphragm between the front and back sides of the glove to separate and form two glove cavities.
[0027] In N1.2 and N1.3 of the above technical solutions, the polyethylene film single sheet is a polyethylene film single sheet prepared by conventional technology, and polyethylene film blowing is used to prepare a cylindrical film, which is then side-cut to obtain the polyethylene film single sheet.
[0028] Compared with the prior art, the preparation method and application of a high-toughness wear-resistant polyethylene composite plastic of the present invention have the following beneficial effects:
[0029] 1. The present invention adopts polyvinyl pyrrolidone and water-soluble carboxymethyl chitosan to dissolve in water, mix and coat the surface of polyethylene powder particles, improve the composite melting point and thermosetting firmness of the polyethylene powder surface, and after the plastic film is hot-pressed, the bonding thermosetting is better and it is difficult to crack or tear. The polyvinyl pyrrolidone and carboxymethyl chitosan after water dissolution are more evenly distributed, so that the quality of plastic film blowing is more uniform, and it is not easy to produce weak parts and is not easy to crack under stress.
[0030] Second, the present invention designs polyvinyl pyrrolidone, water-soluble carboxymethyl chitosan and silicon carbide to be mixed in water, and spray is used to prevent adhesion and coating on the surface of silicon carbide fiber, wherein polyvinyl pyrrolidone and water-soluble carboxymethyl chitosan are used as binders and film-forming agents, which can firmly attach silicon carbide nanopowder to the surface of silicon carbide fiber, improve the wear resistance of the material, and have the function of assisting in improving the crack resistance of silicon carbide fiber, and the toughening effect is better, and a small amount of proportion can be added to achieve a good toughening and wear-resistant effect. In addition, spray coating can make the silicon carbide distribution more uniform, make the quality of plastic film blowing more uniform, and not easy to produce weak parts, and not easy to crack under stress.
[0031] 3. The present invention designs compound B, compound D and palm oil to be mixed and blown into film in a certain proportion. The addition of palm oil has a lubricating and homogenizing effect, so that the compound B with the film structure and the compound D with the coating structure can be mixed more smoothly, and are not easy to unite and destroy the composite structure of the particles, thereby ensuring the homogeneity of the mixed and blown film, and being less likely to produce weak parts and cracking under stress.
[0032] 4. The gloves designed by the present invention have a three-layer structure, which can be specifically divided into three forms: (1) three-layer polyethylene composite plastic film, which has the best hot pressing bonding sealing performance; (2) polyethylene film-polyethylene composite plastic film-polyethylene film, which has slightly poor hot pressing bonding sealing performance, but can appropriately save material costs; (3) polyethylene composite plastic film-polyethylene film-polyethylene composite plastic film, which has slightly poor hot pressing bonding sealing performance, but can appropriately save material costs;
[0033] The three-layer film gloves can be isolated to form two glove cavities. Compared with disposable gloves, they can be used twice, doubling the utilization rate. Especially during use, if one cavity of the glove leaks, it can be replaced with another cavity in time without discarding the gloves, saving replacement costs and resources. The gloves are more durable and not easy to crack or leak. They can also be reused repeatedly, extending their service life and reducing the frequency of replacement, and have good practical value. DETAILED DESCRIPTION
[0034] The present invention is further described below in conjunction with specific implementation cases, but the present invention is not limited to these embodiments.
[0035] Example 1
[0036] A method for preparing a high-toughness wear-resistant polyethylene composite plastic comprises the following steps:
[0037] S1, raw material preparation:
[0038] Solution A was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan = 100:3:5; polyethylene of 50 μm to 300 μm: solution A = 100:60, and the mixture was uniformly mixed, dried, and dispersed to obtain a composite B;
[0039] Mixed solution C was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan: silicon carbide of less than 500 nm = 100:3:3:5; silicon carbide fibers with a diameter of 0.5 μm to 2 μm and a length of less than 0.3 mm and mixed solution C were sprayed on the surface of silicon carbide fibers by fluidized spray method at a mass ratio of silicon carbide fibers: mixed solution C = 100:25, dried at 70°C, and dispersed to obtain composite D;
[0040] The parameters of fluidized spray are: the inlet temperature of mixed liquid C is 25°C, the spray speed is 0.6L / min; the atomization pressure is 0.7MPa; the discharge temperature is 45°C; the raw materials are all food grade;
[0041] S2, Mixing and Film Blowing:
[0042] According to the mass ratio of compound B:compound D:palm oil=95:5:3, compound B, compound D and palm oil are mixed and blown to obtain a cylindrical film, that is, a high-toughness wear-resistant polyethylene composite plastic.
[0043] The above-mentioned high-toughness wear-resistant polyethylene composite plastic is used to prepare film gloves. The method for preparing the film gloves comprises the following steps:
[0044] N1.1, slice overlap:
[0045] The cylindrical film is cut sideways to obtain a polyethylene composite plastic film single sheet; the polyethylene composite plastic film single sheet is stacked into a three-layer structure to obtain a three-layer film, and is wound into a roll;
[0046] N2, heat sealing and cutting:
[0047] The three-layer film is conveyed to the glove machine for heat sealing and cutting into gloves. There is a middle diaphragm between the front and back sides of the gloves to separate and form two glove cavities.
[0048] The polyethylene film single sheet used in this embodiment is a polyethylene film single sheet prepared by conventional technology. The polyethylene film is blown to prepare a cylindrical film, which is then cut sideways to obtain the polyethylene film single sheet.
[0049] Example 2
[0050] A method for preparing a high-toughness wear-resistant polyethylene composite plastic comprises the following steps:
[0051] S1, raw material preparation:
[0052] Solution A was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan = 100:2:3; polyethylene of 50 μm to 300 μm: solution A = 100:40, and the mixture was uniformly mixed, dried, and dispersed to obtain a composite B;
[0053] Mixed solution C was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan: silicon carbide of less than 500 nm = 100:2:2:3; silicon carbide fibers with a diameter of 0.5 μm to 2 μm and a length of less than 0.3 mm and mixed solution C were sprayed on the surface of silicon carbide fibers by fluidized spray method at a mass ratio of silicon carbide fibers: mixed solution C = 100:20, dried at 60°C, and dispersed to obtain composite D;
[0054] The parameters of fluidized spray are: the inlet temperature of mixed liquid C is 20°C, the spray speed is 0.5L / min; the atomization pressure is 0.6MPa; the discharge temperature is 40°C; the raw materials are all food grade;
[0055] S2, Mixing and Film Blowing:
[0056] According to the mass ratio of compound B:compound D:palm oil=90:3:0.5, compound B, compound D and palm oil are mixed and blown to obtain a cylindrical film, that is, a high-toughness and wear-resistant polyethylene composite plastic.
[0057] The above-mentioned high-toughness wear-resistant polyethylene composite plastic is used to prepare film gloves. The method for preparing the film gloves comprises the following steps:
[0058] N1.2, slice overlap:
[0059] The cylindrical film is cut sideways to obtain a polyethylene composite plastic film single sheet; the polyethylene film single sheet-polyethylene composite plastic film single sheet-polyethylene film single sheet are stacked into a three-layer structure to obtain a three-layer film, and the three-layer film is wound into a roll;
[0060] N2, heat sealing and cutting:
[0061] The three-layer film is conveyed to the glove machine for heat sealing and cutting into gloves. There is a middle diaphragm between the front and back sides of the gloves to separate and form two glove cavities.
[0062] The polyethylene film single sheet used in this embodiment is a polyethylene film single sheet prepared by conventional technology. The polyethylene film is blown to prepare a cylindrical film, which is then cut sideways to obtain the polyethylene film single sheet.
[0063] Example 3
[0064] A method for preparing a high-toughness wear-resistant polyethylene composite plastic comprises the following steps:
[0065] S1, raw material preparation:
[0066] Solution A was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan = 100:2:8; polyethylene of 50 μm to 300 μm: solution A = 100:40, and the mixture was uniformly mixed, dried, and dispersed to obtain a composite B;
[0067] Mixed solution C was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan: silicon carbide of less than 500 nm = 100:4:2:8; silicon carbide fibers with a diameter of 0.5 μm to 2 μm and a length of less than 0.3 mm and mixed solution C were sprayed on the surface of silicon carbide fibers by fluidized spray method at a mass ratio of silicon carbide fibers: mixed solution C = 100:20, dried at 80°C, and dispersed to obtain composite D;
[0068] The parameters of fluidized spray are: the inlet temperature of mixed liquid C is 20°C, the spray speed is 0.8L / min; the atomization pressure is 0.6MPa; the discharge temperature is 50°C; the raw materials are all food grade;
[0069] S2, Mixing and Film Blowing:
[0070] According to the mass ratio of compound B:compound D:palm oil=90:8:0.5, compound B, compound D and palm oil are mixed and blown to obtain a cylindrical film, that is, a high-toughness and wear-resistant polyethylene composite plastic.
[0071] The above-mentioned high-toughness wear-resistant polyethylene composite plastic is used to prepare film gloves. The method for preparing the film gloves comprises the following steps:
[0072] N1.3, slice overlap:
[0073] The cylindrical film is cut sideways to obtain a polyethylene composite plastic film single sheet; the polyethylene composite plastic film single sheet-polyethylene film single sheet-polyethylene composite plastic film single sheet are stacked into a three-layer structure to obtain a three-layer film, and the three-layer film is wound into a roll;
[0074] N2, heat sealing and cutting:
[0075] The three-layer film is conveyed to the glove machine for heat sealing and cutting into gloves. There is a middle diaphragm between the front and back sides of the gloves to separate and form two glove cavities.
[0076] The polyethylene film single sheet used in this embodiment is a polyethylene film single sheet prepared by conventional technology. The polyethylene film is blown to prepare a cylindrical film, which is then cut sideways to obtain the polyethylene film single sheet.
[0077] Example 4
[0078] A method for preparing a high-toughness wear-resistant polyethylene composite plastic comprises the following steps:
[0079] S1, raw material preparation:
[0080] Solution A was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan = 100:5:8; polyethylene of 50 μm to 300 μm: solution A = 100:80, and the mixture was uniformly mixed, dried, and dispersed to obtain a composite B;
[0081] Mixed solution C was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan: silicon carbide below 500 nm = 100:4:4:8; silicon carbide fibers with a diameter of 0.5 μm to 2 μm and a length of less than 0.3 mm and mixed solution C were sprayed on the surface of silicon carbide fibers by fluidized spraying method at a mass ratio of silicon carbide fibers: mixed solution C = 100:30, dried at 80°C, and dispersed to obtain a composite D;
[0082] The parameters of fluidized spray are: the inlet temperature of mixed liquid C is 30°C, the spray speed is 0.8L / min; the atomization pressure is 0.8MPa; the discharge temperature is 50°C; the raw materials are all pharmaceutical grade;
[0083] S2, Mixing and Film Blowing:
[0084] According to the mass ratio of compound B:compound D:palm oil=100:8:5, compound B, compound D and palm oil are mixed and blown to obtain a cylindrical film, that is, a high-toughness and wear-resistant polyethylene composite plastic.
[0085] The above-mentioned high-toughness wear-resistant polyethylene composite plastic is used to prepare film gloves. The method for preparing the film gloves comprises the following steps:
[0086] N1.1, slice overlap:
[0087] The cylindrical film is cut sideways to obtain a polyethylene composite plastic film single sheet; the polyethylene composite plastic film single sheet is stacked into a three-layer structure to obtain a three-layer film, and is wound into a roll;
[0088] N2, heat sealing and cutting:
[0089] The three-layer film is conveyed to the glove machine for heat sealing and cutting into gloves. There is a middle diaphragm between the front and back sides of the gloves to separate and form two glove cavities.
[0090] The polyethylene film single sheet used in this embodiment is a polyethylene film single sheet prepared by conventional technology. The polyethylene film is blown to prepare a cylindrical film, which is then cut sideways to obtain the polyethylene film single sheet.
[0091] Example 5
[0092] A method for preparing a high-toughness wear-resistant polyethylene composite plastic comprises the following steps:
[0093] S1, raw material preparation:
[0094] Solution A was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan = 100:5:3; polyethylene of 50 μm to 300 μm: solution A = 100:80, and the mixture was uniformly mixed, dried, and dispersed to obtain a composite B;
[0095] Mixed solution C was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan: silicon carbide of less than 500 nm = 100:2:4:3; silicon carbide fiber with a diameter of 0.5 μm to 2 μm and a length of less than 0.3 mm and mixed solution C were sprayed on the surface of silicon carbide fiber by fluidized spray method at a mass ratio of silicon carbide fiber: mixed solution C = 100:30), dried at 60°C, and dispersed to obtain composite D;
[0096] The parameters of fluidized spray are: the inlet temperature of mixed liquid C is 30°C, the spray speed is 0.5L / min; the atomization pressure is 0.8MPa; the discharge temperature is 40°C; the raw materials are all pharmaceutical grade;
[0097] S2, Mixing and Film Blowing:
[0098] According to the mass ratio of compound B:compound D:palm oil=100:3:5, compound B, compound D and palm oil are mixed and blown to obtain a cylindrical film, that is, a high-toughness wear-resistant polyethylene composite plastic.
[0099] The above-mentioned high-toughness wear-resistant polyethylene composite plastic is used to prepare film gloves. The method for preparing the film gloves comprises the following steps:
[0100] N1.2, slice overlap:
[0101] The cylindrical film is cut sideways to obtain a polyethylene composite plastic film single sheet; the polyethylene film single sheet-polyethylene composite plastic film single sheet-polyethylene film single sheet are stacked into a three-layer structure to obtain a three-layer film, and the three-layer film is wound into a roll;
[0102] N2, heat sealing and cutting:
[0103] The three-layer film is conveyed to the glove machine for heat sealing and cutting into gloves. There is a middle diaphragm between the front and back sides of the gloves to separate and form two glove cavities.
[0104] The polyethylene film single sheet used in this embodiment is a polyethylene film single sheet prepared by conventional technology. The polyethylene film is blown to prepare a cylindrical film, which is then cut sideways to obtain the polyethylene film single sheet.
[0105] Example 6
[0106] A method for preparing a high-toughness wear-resistant polyethylene composite plastic comprises the following steps:
[0107] S1, raw material preparation:
[0108] Solution A was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan = 100:4:4; polyethylene of 50 μm to 300 μm: solution A = 100:60, and the mixture was uniformly mixed, dried, and dispersed to obtain a composite B;
[0109] Mixed solution C was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan: silicon carbide of less than 500 nm = 100:2:4:6; silicon carbide fibers with a diameter of 0.5 μm to 2 μm and a length of less than 0.3 mm and mixed solution C were sprayed on the surface of silicon carbide fibers by fluidized spraying method at a mass ratio of silicon carbide fibers: mixed solution C = 100:28, dried at 75°C, and dispersed to obtain composite D;
[0110] The parameters of fluidized spray are: the inlet temperature of mixed liquid C is 26°C, the spray speed is 0.7L / min; the atomization pressure is 0.65MPa; the discharge temperature is 46°C; the raw materials are all pharmaceutical grade;
[0111] S2, Mixing and Film Blowing:
[0112] According to the mass ratio of compound B:compound D:palm oil=92:6:4, compound B, compound D and palm oil are mixed and blown to obtain a cylindrical film, that is, a high-toughness wear-resistant polyethylene composite plastic.
[0113] The above-mentioned high-toughness wear-resistant polyethylene composite plastic is used to prepare film gloves. The method for preparing the film gloves comprises the following steps:
[0114] N1.3, slice overlap:
[0115] The cylindrical film is cut sideways to obtain a polyethylene composite plastic film single sheet; the polyethylene composite plastic film single sheet-polyethylene film single sheet-polyethylene composite plastic film single sheet are stacked into a three-layer structure to obtain a three-layer film, and the three-layer film is wound into a roll;
[0116] N2, heat sealing and cutting:
[0117] The three-layer film is conveyed to the glove machine for heat sealing and cutting into gloves. There is a middle diaphragm between the front and back sides of the gloves to separate and form two glove cavities.
[0118] The polyethylene film single sheet used in this embodiment is a polyethylene film single sheet prepared by conventional technology. The polyethylene film is blown to prepare a cylindrical film, which is then cut sideways to obtain the polyethylene film single sheet.
[0119] Preparation of gloves of Comparative Example 1:
[0120] The conventional preparation method in the prior art adopts polyethylene film blowing to prepare a cylindrical film, and then adopts a glove machine to heat-seal and press-cut the film on both sides into gloves.
[0121] Preparation of gloves of Comparative Example 2:
[0122] Without preparing solution A, polyethylene was directly mixed with compound D and palm oil for film blowing. Other step parameters were the same as those in Example 1.
[0123] Preparation of gloves of Comparative Example 3:
[0124] Without preparing mixed solution C, silicon carbide fiber is directly mixed with composite B and palm oil for film blowing. Other step parameters are the same as those in Example 1.
[0125] Preparation of gloves of Comparative Example 4:
[0126] Solution A and mixed solution C are not prepared, and palm oil is not added; polyethylene is directly mixed with silicon carbide fiber and silicon carbide for film blowing. Other step parameters are the same as those in Example 1.
[0127] 30 pairs (60 pieces) of gloves from the above embodiments and comparative examples were randomly selected for use test. The test method was as follows:
[0128] Experiment 1: Wear gloves and immerse them in soybean oil. Let it stand for 5 minutes, take them out and check whether there is oil on the fingers. If there is oil, it is considered a leak and observe the cracking.
[0129] Experiment 2: Wear gloves and immerse them in soybean oil. Rub your hands gently for 5 minutes, take them out, and check whether there is oil on your fingers. If there is oil, it is considered a leak and observe the cracking.
[0130] Experiment 3: Wear gloves and perform mixing and kneading operations. The mixture is cold dishes (containing oil and water). Mix for 10 minutes, take out and check whether there is oil and water on the fingers. If there is oil and water, it is judged as leakage and the cracking is observed.
[0131] The trial results are shown in Table 1 below:
[0132]
[0133] From the above trial results, it can be seen that the gloves of Examples 1 to 5 have good hot pressing sealing and are not easy to crack, and the film surface toughness is high and is not easy to crack; compared with the results of the comparative example, it can be seen that the addition of polyvinyl pyrrolidone and water-soluble carboxymethyl chitosan can improve the hot pressing sealing of the gloves, improve the composite melting point and thermosetting firmness, and are difficult to crack; adding silicon carbide fiber can improve toughness and tear resistance; adding silicon carbide can improve wear resistance; adding palm oil can improve the homogeneity of the mixed blown film, thereby preventing cracking at weak points.
[0134] In addition, a total of 6 leaking gloves in the test gloves of Examples 1 to 6 were replaced with another cavity of the gloves after slight leakage, and Experiments 1 and 2 were repeated. There was no leakage, and Experiment 3 was continued. There were 5 no leakage and 1 slight leakage. The non-leaking gloves in the test gloves of Examples 1 to 6 were replaced with another cavity of the gloves, and Experiments 1 and 2 were repeated. There was no leakage, and Experiment 3 was continued. There were 6 slight leakages, no obvious cracks were observed, and 2 serious leakages, and obvious cracks were found at the compression seal. The results show that the gloves of Examples 1 to 6 can be used interchangeably with double cavities, and the leakage rate is also low after changing cavities and wearing, and have a good reuse effect.
[0135] Five pairs of gloves from the above embodiments and comparative examples were randomly selected for tearing test. The test method was: tearing along the seams on the front and back sides of the gloves to evaluate the tearing difficulty. The results are shown in Table 2 below:
[0136]
[0137] The tearing difficulty index is divided into: 1-easy to tear; 2-can be torn with little force; 3-can be torn with greater force.
[0138] From the above evaluation results, it can be seen that the gloves of Examples 1 to 6 have good hot pressing and thermosetting properties, good toughness at the seams, and are more difficult to tear apart than the gloves of Comparative Example 1. In Comparative Example 2, the polyethylene surface is not coated with polyvinyl pyrrolidone and water-soluble carboxymethyl chitosan, and the hot pressing and thermosetting properties are slightly poor; in Comparative Example 3, the silicon carbide fiber is not coated with polyvinyl pyrrolidone, water-soluble carboxymethyl chitosan and silicon carbide, and the hot pressing and thermosetting properties are slightly poor; in Comparative Example 4, there is no polyvinyl pyrrolidone and water-soluble carboxymethyl chitosan at all, and the hot pressing and thermosetting properties are equivalent to those of Comparative Example 1, and it is easy to crack and leak.
Claims
1. A method for preparing a high-toughness wear-resistant polyethylene composite plastic, characterized in that: The steps include: S1, raw material preparation: Solution A was prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan = 100: (2-5): (3-8); and the mixture was uniformly mixed, dried, and dispersed at a mass ratio of polyethylene: solution A = 100: (40-80) to obtain a composite B; Mixed solution C is prepared at a mass ratio of water: polyvinyl pyrrolidone: water-soluble carboxymethyl chitosan: silicon carbide = 100: (2-4): (2-4): (3-8); silicon carbide fiber and mixed solution C are sprayed on the surface of silicon carbide fiber by fluidized spraying method at a mass ratio of silicon carbide fiber: mixed solution C = 100: (20-30), dried, and dispersed to obtain a composite D; The particle size of the polyethylene is 50 μm to 300 μm; the particle size of the silicon carbide is less than 500 nm; the diameter of the silicon carbide fiber is 0.5 μm to 2 μm, and the length is less than 0.3 mm; S2, Mixing and Film Blowing: According to the mass ratio of compound B:compound D:palm oil = (90-100): (3-8): (0.5-5), compound B, compound D and palm oil are mixed and blown to obtain a cylindrical film, i.e., a high-toughness and wear-resistant polyethylene composite plastic.
2. The method for preparing a high-toughness wear-resistant polyethylene composite plastic according to claim 1, characterized in that: In S1, the parameters of the fluidized spray are: the inlet temperature of the mixed liquid C is 20°C to 30°C, the spray speed is 0.5L / min to 0.8L / min; the atomization pressure is 0.6MPa to 0.8MPa; and the discharge temperature is 40°C to 50°C.
3. The method for preparing a high-toughness wear-resistant polyethylene composite plastic according to claim 1, characterized in that: In S1, the drying temperature is 60°C to 80°C.
4. Application of a high-toughness wear-resistant polyethylene composite plastic, the high-toughness wear-resistant polyethylene composite plastic prepared by the preparation method of a high-toughness wear-resistant polyethylene composite plastic according to claim 1, characterized in that: The plastic is used to prepare film gloves. The method for preparing the film gloves comprises the following steps: N1, slice superposition, choose one of the following three methods: N1.1, N1.2 and N1.3: N1.1: Cutting the cylindrical film sideways to obtain a polyethylene composite plastic film sheet; stacking the polyethylene composite plastic film sheet into a three-layer structure to obtain a three-layer film, and winding the film into a roll; N1.2: Cut the cylindrical film sideways to obtain a polyethylene composite plastic film sheet; stack the polyethylene film sheet-polyethylene composite plastic film sheet-polyethylene film sheet into a three-layer structure to obtain a three-layer film, and wind it into a roll; N1.3: Cut the cylindrical film sideways to obtain a polyethylene composite plastic film sheet; stack the polyethylene composite plastic film sheet-polyethylene film sheet-polyethylene composite plastic film sheet into a three-layer structure to obtain a three-layer film, and wind it into a roll; N2, heat sealing and cutting: The three-layer film is transported to the glove machine for heat sealing and cutting into gloves.
5. The use of a high-toughness wear-resistant polyethylene composite plastic according to claim 4, characterized in that: In N2, there is a middle diaphragm between the front and back sides of the glove to separate and form two glove cavities.
Citation Information
Patent Citations
Disposable film gloves and preparation method thereof
CN103881178A
Disposable film glove and making method thereof
CN106977888A
Polymer composite membrane, preparation method thereof, polymer composite membrane prepared by method, gel electrolyte and lithium ion battery
CN106159173A
Oil-resistant antiskid protective glove and preparation method thereof
CN117322695A
Cited By
Preparation method of wear-resistant polyethylene composite plastic
CN120504867A