Sintered NdFeB magnet containing cerium and its anisostatic pressing preparation method

By introducing cerium elements and other metal elements into neodymium iron boron magnets, combined with unisostatic pressure forming process, the cost and performance problems when Ce replaces Nd and Pr are solved, and high-performance and low-cost neodymium iron boron magnet preparation is achieved. , simplifies the process flow and improves magnet performance.

CN118538496BActive Publication Date: 2024-11-22ARCFL TECH LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411014345.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-22
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

When Ce is used instead of Nd and Pr, the cost of existing neodymium iron boron magnets is difficult to reduce and the magnet performance is attenuated. The traditional isostatic pressing preparation process is cumbersome, which increases production costs.

Method used

Introduce cerium elements and add other metal elements into the neodymium iron boron magnet, and form auxiliary alloy phases through layering and stacking and smelting. Combined with unisostatic pressure forming process, simplify the preparation process, reduce manual operation and packaging steps, and adopt stage-type heating sintering and Third-level tempering treatment.

Benefits of technology

The remanent magnetism and intrinsic coercivity of neodymium iron boron cerium-containing magnets are improved, production costs are reduced, and the process flow is simplified. The magnetic blank cracking ratio and dimensional deformation are low, and it has excellent magnet performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of neodymium iron boron magnets, and specifically relates to a sintered neodymium iron boron cerium-containing magnet and a method for preparing the same by anisostatic pressing. The sintered neodymium iron boron cerium-containing magnet comprises the following raw materials by mass: 360-380 parts of iron, 25-30 parts of ferroboron, 40-45 parts of cerium, 14-18 parts of gadolinium iron alloy, 4-5 parts of dysprosium iron alloy, 130-140 parts of praseodymium-neodymium metal, 0.5-0.8 parts of gallium, 3-4 parts of cobalt, 0.5-1 parts of copper, 3-4 parts of aluminum, 1.5-2 parts of zirconium, and 0.5-0.8 parts of titanium; the above raw materials are sequentially smelted, hydrogen crushed, jet milled, anisostatically pressed, sintered, and heat treated to obtain the obtained material. The present invention adds cerium element to the NdFeB magnet and introduces multiple metal elements. By adjusting the magnet composition and structure, the remanence and coercive force of the NdFeB cerium-containing magnet are improved. The non-isostatic pressing preparation method is simpler than the traditional isostatic pressing preparation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of NdFeB magnets, and in particular relates to a sintered NdFeB cerium-containing magnet and a method for preparing the same by anisostatic pressing. Background Art

[0002] Neodymium iron boron magnet is a permanent magnetic material with high magnetic energy product and high coercivity. It occupies an important position in magnetic materials and is widely used in motors, generators, sensors and other fields. At present, due to the expansion of the application field of rare earth permanent magnetic materials and the surge in demand, Nd2Fe 14 Class B permanent magnet materials are highly dependent on precious rare earth resources such as Nd, Pr, Dy, and Tb. The usage of Nd and Pr accounts for more than 70% (mass fraction) of the total rare earth resources, and their consumption is huge. The high-abundance rare earth Ce, which has the most abundant reserves and relatively low prices, is a by-product in the extraction process of Nd and Pr, and its usage is relatively low. It has been in a state of market backlog for a long time.

[0003] Therefore, using Ce to replace part of Nd and Pr can reduce the cost of NdFeB magnets. However, the increase in Ce content will cause the magnetic performance of NdFeB magnets to decay. How to use Ce to replace part of Nd and Pr without losing the magnetic performance has become a hot topic of research.

[0004] Patent CN102842400A discloses a method for preparing low-cost sintered NdFeB by lanthanum-cerium doping. After NdFeB is made into powder, lanthanum-cerium alloy powder is added to replace part of the NdFeB rich phase with a lanthanum-cerium phase, which plays the role of a NdFeB rich phase. Compared with adding lanthanum-cerium alloy during smelting, the coercive force is slightly increased and the magnetic energy product is significantly improved. However, the amount of cerium added in the invention is relatively low, and the coercive force of the prepared NdFeB magnet is relatively low, which still needs to be further improved.

[0005] Furthermore, patent CN116092766A discloses a processing technology for high-cerium NdFeB magnets with improved intrinsic coercivity, in which high-cerium NdFeB magnets are prepared in the form of dual alloys, and the alloy composition with high cerium content is regulated, while degreasing and degassing treatment is added, thereby improving the intrinsic coercivity of NdFeB magnets. However, the particle size of the refined magnetic powder obtained by the invention during airflow grinding is relatively low. Reducing the particle size of the refined magnetic powder can improve the magnetic properties of the NdFeB magnet, but it will also greatly increase the difficulty of molding; in addition, the preparation process of the invention is relatively complicated. Although the introduction of cerium can reduce the cost of raw materials, the complexity of the production process will increase the production cost, resulting in a higher overall cost of the final product.

[0006] In addition, the above patents all use a process combining orientation molding and isostatic pressing to mold the magnetic powder, that is, the magnetic powder is pressed under the action of a molding magnetic field and pressure, and then isostatically pressed. This is also a commonly used molding process for industrial production. This molding process can prevent the magnetic blank from cracking during the molding process, and at the same time improve the structural uniformity of the magnetic blank. However, in actual production, after the pressing is completed, the magnetic blank needs to be coated and packaged in a glove box, and then a layer of protective bag is put on after the material is discharged, and then it is put into an outer packaging bag for outer packaging, and then isostatically pressed. After the isostatic pressing treatment, all the packaging materials must be removed before sintering. The entire molding process is relatively cumbersome, which increases labor costs and material costs.

[0007] Therefore, how to reduce the cost of raw materials and production process without reducing the performance of the magnet is of great significance to the industrial production and promotion of NdFeB magnets. Summary of the invention

[0008] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a sintered NdFeB cerium-containing magnet, by adding cerium element to the NdFeB magnet and introducing a variety of metal elements, thereby improving the remanence and coercive force of the NdFeB cerium-containing magnet through adjustment of the magnet composition and structure. The present invention also provides a non-isostatic pressing preparation method thereof, which is simpler than the traditional isostatic pressing preparation method.

[0009] The sintered NdFeB cerium-containing magnet of the present invention comprises the following raw materials in parts by mass: 360-380 parts of iron, 25-30 parts of ferroboron, 40-45 parts of cerium, 14-18 parts of gadolinium-iron alloy, 4-5 parts of dysprosium-iron alloy, 130-140 parts of praseodymium-neodymium metal, 0.5-0.8 parts of gallium, 3-4 parts of cobalt, 0.5-1 parts of copper, 3-4 parts of aluminum, 1.5-2 parts of zirconium, and 0.5-0.8 parts of titanium;

[0010] The raw materials are sequentially subjected to smelting, hydrogen crushing, air flow milling, isostatic pressing, sintering and heat treatment to obtain sintered NdFeB cerium-containing magnets.

[0011] The ferroboron is low-carbon ferroboron with a carbon content of no more than 0.1wt.%, and a boron content of 14-25wt.%, which complies with the national standard GB / T 5682-2015.

[0012] The total content of rare earth elements in the gadolinium-iron alloy is 69-75wt.%, and the content of gadolinium in the rare earth elements is not less than 99.5wt.%, which meets the rare earth industry standard XB / T 403-2012.

[0013] The total content of rare earth elements in the dysprosium-iron alloy is 75-85wt.%, and the content of dysprosium in the rare earth elements is not less than 99.5wt.%, which complies with the national standard GB / T 26415-2010.

[0014] The praseodymium-neodymium metal has a praseodymium content of 70-85wt.%, and a total rare earth element content of not less than 99wt.%, which complies with the national standard GB / T 20892-2007.

[0015] The anisostatic pressing method for preparing a sintered NdFeB cerium-containing magnet of the present invention comprises the following steps:

[0016] (1) Smelting: The raw materials are stacked in a vacuum belt-spinning furnace in order, with iron on the bottom layer, ferroboron, cerium, gadolinium-iron alloy, and dysprosium-iron alloy on the next bottom layer, praseodymium-neodymium metal on the middle layer, and gallium, cobalt, copper, aluminum, zirconium, and titanium on the top layer. The raw materials are melted, cast, and cooled in an argon atmosphere to obtain spinning sheets.

[0017] (2) Hydrogen crushing: The flakes are subjected to hydrogen absorption and dehydrogenation in sequence to obtain coarse powder;

[0018] (3) Jet mill pulverization: Add antioxidant and lubricant to the coarse powder, use jet mill to mix and grind until the average particle size is between 2.6-3.2 μm to obtain fine powder, add antioxidant, lubricant and compression molding aid to the fine powder, mix well and use as magnetic powder;

[0019] (4) Anisostatic pressing: The magnetic powder is pressed vertically, the oxygen content is controlled below 400ppm, the forming magnetic field is 1.7-1.8T, the pressing pressure is 25-28T, and the volume is reduced by 10-13%. The pressed magnetic blank is directly loaded into a graphite box, sealed and transported to a vacuum sintering furnace for sintering;

[0020] (5) Sintering: The magnetic blank is sintered under vacuum conditions, with the sintering end temperature at 1055-1060°C. After keeping at this temperature for 4-6 hours, it is cooled;

[0021] (6) Heat treatment: The sintered magnetic blank is subjected to three-stage tempering treatment, with the first-stage tempering temperature being 900-930°C, the second-stage tempering temperature being 600-700°C, and the third-stage tempering temperature being 400-450°C. After the treatment, a sintered NdFeB cerium-containing magnet is obtained.

[0022] In step (1), during smelting, the temperature is first raised to 1450-1480°C and kept for 10-15 minutes, and then the temperature is lowered to 1350-1400°C.

[0023] In step (1), the pouring temperature is 1450-1480°C, the pouring time is 10-12 minutes, and the pouring sheet thickness is 0.2-0.35 mm.

[0024] In step (1), the pellets are cooled to below 45° C. The cooled pellets are placed in a packaging bag and stored in an argon filled bag.

[0025] In step (2), the hydrogen absorption pressure is 100-120 kPa, the hydrogen absorption time is 90-120 min, and the dehydrogenation temperature is 550-560 °C.

[0026] In step (3), the antioxidant is at least one of 1-hexadecanol, triphenylmethanol, and calcium stearate; the amount of the antioxidant added to the coarse powder is 0.08-0.12% of the mass of the coarse powder; the amount of the antioxidant added to the fine powder is 0.08-0.12% of the mass of the fine powder.

[0027] In step (3), the lubricant is at least one of polyethylene glycol and 120# gasoline; the amount of lubricant added to the coarse powder is 0.03-0.05% of the mass of the coarse powder; the amount of lubricant added to the fine powder is 0.03-0.05% of the mass of the fine powder.

[0028] In step (3), the molding aid is at least one of glycerol and ethylene glycol; the amount of the molding aid added to the fine powder is 0.08-0.12% of the mass of the fine powder.

[0029] In step (3), the oxygen content of the air flow mill is less than 50 ppm, the grinding pressure is 0.5-0.6 MPa, the bottom spray pressure is 0.4-0.5 MPa, the sorting wheel speed is 3500-3800 rpm, and the grinding time is 4-5 h.

[0030] In step (4), the density of the pressed magnetic blank is 4.2-4.5 g / cm 3 When pressing vertically, the size is precisely controlled by mechanical limiters until the volume is reduced by 10-13%. After pressing to the set size, pressure demoulding is used. In order to make demoulding more convenient and reduce demoulding cracks, a release agent can be added.

[0031] The present invention directly loads the pressed magnetic blank into a graphite box through a mechanical arm, and then transports it to a vacuum sintering furnace through a sealed box. The entire pressing, boxing and stacking process is fully automatic, without manual operation, and the sealed box transportation allows the material to enter the sintering furnace in a sealed environment. Compared with the isostatic pressing process, there is no need for film sealing, packaging, and bag cutting operations.

[0032] In step (5), sintering is carried out in a vacuum sintering furnace, and the vacuum degree in the vacuum sintering furnace is maintained below 0.5 Pa, in order to remove harmful gases, additives and impurities in the magnetic blank.

[0033] In step (5), the temperature is raised in stages during sintering, the temperature is raised to 250-300°C and kept for 1.5-2h, the temperature is raised to 600-650°C and kept for 2-2.5h, the temperature is raised to 800-850°C and kept for 3-3.5h, the temperature is raised to 950-1000°C and kept for 20-30min, the temperature is raised to 1055-1060°C and kept for 4-6h, and then cooled to below 70°C.

[0034] In step (6), during the three-stage tempering treatment, the vacuum degree is maintained below 0.5 Pa, the first-stage tempering is heated to 900-930°C and kept warm for 2-4 hours, and then cooled to below 70°C; the second-stage tempering is heated to 600-700°C and kept warm for 3-5 hours, and then cooled to below 70°C; the third-stage tempering is heated to 400-450°C and kept warm for 1-2 hours, and then cooled to below 70°C.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] (1) The present invention not only introduces cerium into the NdFeB magnet, but also adds other metal auxiliary elements. Through layered stacking and smelting, various forms of auxiliary alloy phases can be formed between the auxiliary metal elements and the rare earth elements, thereby weakening the negative impact of the rare earth elements on the magnetic properties of the main alloy phase, and greatly improving the remanence and intrinsic coercive force of the NdFeB magnet containing cerium;

[0037] (2) The present invention adopts an isostatic pressing molding process. Compared with the isostatic pressing preparation method, there is no need to seal the film, encapsulate, and then cut the bag, which not only saves manpower and material resources, but also avoids the attenuation of the performance of the magnetic blank due to poor sealing during the transfer process;

[0038] (3) The present invention adds lubricants and antioxidants to the magnetic powder in batches, which can greatly increase the dispersibility and lubricity of the magnetic powder. At the same time, the addition of the compression molding aid forms a protective film on the surface of the magnetic powder, reducing the generation of magnet cracks during compression molding;

[0039] (4) The NdFeB cerium-containing magnet prepared by the present invention has a remanence greater than 13.5 kGs, an intrinsic coercive force greater than 20 kOe, a magnet blank cracking ratio not exceeding 2%, and a dimensional deformation less than 0.1 mm. It has excellent magnet performance, and the preparation method is simple and easy with low overall cost. DETAILED DESCRIPTION

[0040] The technical scheme of the present invention is further described below in conjunction with the examples. Unless otherwise specified, all raw materials used in the examples are commercially available.

[0041] The ferroboron used in the embodiment is low-carbon ferroboron with a carbon content of no more than 0.1 wt.%, a boron content of 14-25 wt.%, and conforming to the national standard GB / T 5682-2015.

[0042] The gadolinium-iron alloy used in the embodiment has a total rare earth element content of 69-75wt.%, and the content of gadolinium in the rare earth elements is not less than 99.5wt.%, which complies with the rare earth industry standard XB / T 403-2012.

[0043] The dysprosium-iron alloy used in the embodiment has a total rare earth element content of 75-85wt.%, and the dysprosium content in the rare earth elements is not less than 99.5wt.%, which complies with the national standard GB / T 26415-2010.

[0044] The praseodymium-neodymium metal used in the embodiment has a praseodymium content of 70-85wt.%, and a total rare earth element content of not less than 99wt.%, which complies with the national standard GB / T 20892-2007.

[0045] The sizes of the NdFeB cerium-containing magnets prepared in the examples are all 47 mm×45 mm×31 mm.

[0046] Example 1

[0047] Sintered NdFeB cerium-containing magnets were prepared as follows:

[0048] (1) Smelting: prepare the following materials in parts by weight: 363 parts of iron, 28 parts of ferroboron (boron content 20wt.%, carbon content 0.05wt.%), 42 parts of cerium, 15 parts of gadolinium-iron alloy (total rare earth element content 72wt.%), 4.5 parts of dysprosium-iron alloy (total rare earth element content 80wt.%), 137 parts of praseodymium-neodymium metal (praseodymium content 80wt.%), 0.6 parts of gallium, 3.6 parts of cobalt, 0.9 parts of copper, 3.6 parts of aluminum, 1.8 parts of zirconium, and 0.6 parts of titanium;

[0049] The raw materials are stacked in the vacuum belt furnace in order, with iron on the bottom layer, ferroboron, cerium, gadolinium iron alloy, and dysprosium iron alloy on the next bottom layer, praseodymium-neodymium metal on the middle layer, and gallium, cobalt, copper, aluminum, zirconium, and titanium on the upper layer. After the furnace is loaded, smelting begins. The vacuum belt furnace is evacuated to below 4Pa, and argon gas is injected into the furnace body. The initial heating power is 180kW, which is increased to 250kW within 10min, and then increased to 450kw at a rate of 10kW / min. When all the raw materials are melted, the heating power is increased. The power is increased to 530kW. When the temperature of the raw material rises to 1460℃, the heating power is reduced to 120kW, and the temperature is kept for 12 minutes. Then the heating power is returned to zero until the temperature of the raw material drops to 1380℃, and the smelting is completed; the heating is turned on again until the temperature of the raw material rises to 1460℃, and the casting is carried out. The thickness of the casting sheet is 0.3mm, and the casting time is 12 minutes; after the casting is completed, the sheet is crushed and cooled until the temperature of the sheet drops below 45℃, and then it is packed in a packaging bag and filled with argon gas for storage;

[0050] (2) Hydrogen crushing: The slabs are subjected to hydrogen absorption and dehydrogenation in sequence, with a hydrogen absorption pressure of 100 kPa, a hydrogen absorption time of 120 min, and a dehydrogenation temperature of 550 °C to obtain coarse powder;

[0051] (3) Jet mill pulverization: add 0.1% calcium stearate and 0.1% 120# gasoline to the coarse powder, and grind them by jet mill until the average particle size is 3.0 μm to obtain fine powder. The oxygen content of the jet mill is less than 50 ppm, the grinding pressure is 0.55 MPa, the bottom spray pressure is 0.45 MPa, the classifying wheel speed is 3600 rpm, and the grinding time is 4.5 h. Add 0.04% calcium stearate, 0.04% 120# gasoline, and 0.1% glycerin to the fine powder, mix well and use as magnetic powder.

[0052] (4) Anisostatic pressing: The magnetic powder is pressed vertically, the oxygen content is controlled below 400ppm, the forming magnetic field is 1.8T, the pressing pressure is 25T, the size is accurately controlled by mechanical limit, the volume is reduced by 12%, and pressure demolding is used. The density of the pressed magnetic blank is 4.2g / cm 3 , the pressed magnetic blank is directly loaded into the graphite box through the robot arm, and then transferred by the sealed box to the vacuum sintering furnace for sintering;

[0053] (5) Sintering: After the magnetic blank is transferred to the vacuum sintering furnace, the vacuum degree in the vacuum sintering furnace is maintained below 0.5 Pa, and the sintering is carried out in a staged heating manner, heating to 250°C and keeping it for 2 hours, heating to 600°C and keeping it for 2.5 hours, heating to 800°C and keeping it for 3.5 hours, heating to 950°C and keeping it for 30 minutes, heating to 1050°C and keeping it for 6 hours, and then cooling to below 70°C;

[0054] (6) Heat treatment: The sintered magnetic blank is subjected to three-stage tempering treatment, maintaining the vacuum degree below 0.5Pa. The first-stage tempering is heated to 900℃ and kept at this temperature for 4h, and then cooled to below 70℃; the second-stage tempering is heated to 600℃ and kept at this temperature for 5h, and then cooled to below 70℃; the third-stage tempering is heated to 400℃ and kept at this temperature for 2h, and then cooled to below 70℃ to obtain a sintered NdFeB cerium-containing magnet.

[0055] Example 2

[0056] Sintered NdFeB cerium-containing magnets were prepared as follows:

[0057] (1) Smelting: Prepare the following materials in the following proportions by weight: 380 parts of iron, 25 parts of ferroboron (boron content 25wt.%, carbon content 0.05wt.%), 45 parts of cerium, 18 parts of gadolinium iron alloy (total rare earth element content 69wt.%), 4 parts of dysprosium iron alloy (total rare earth element content 85wt.%), 130 parts of praseodymium-neodymium metal (praseodymium content 70wt.%), 0.5 parts of gallium, 3 parts of cobalt, 0.5 parts of copper, 4 parts of aluminum, 1.5 parts of zirconium, and 0.8 parts of titanium; stack the raw materials in a vacuum belt-spinning furnace in order, with iron on the bottom layer, ferroboron, cerium, gadolinium iron alloy, and dysprosium iron alloy on the next bottom layer, praseodymium-neodymium metal on the middle layer, and gallium, cobalt, copper, aluminum, zirconium, and titanium on the top layer; after the furnace is loaded, start smelting, and the vacuum belt-spinning furnace is vacuumed. The furnace is evacuated to below 4Pa, and argon is injected into the furnace. The initial heating power is 180kW, which is increased to 250kW within 10min, and then increased to 450kw at a rate of 10kW / min. When all the raw materials are melted, the heating power is increased to 530kW. When the raw material temperature rises to 1450℃, the heating power is reduced to 120kW, and the temperature is kept for 15min. Then the heating power is returned to zero until the raw material temperature drops to 1350℃, and the smelting is completed; the heating is turned on again until the raw material temperature rises to 1450℃, and pouring is carried out. The thickness of the poured sheet is 0.35mm, and the pouring time is 11min; after pouring, the sheet is crushed and cooled until the sheet temperature drops below 45℃, and then it is packed in a packaging bag and filled with argon for storage;

[0058] (2) Hydrogen crushing: The flakes are subjected to hydrogen absorption and dehydrogenation in sequence, with a hydrogen absorption pressure of 120 kPa, a hydrogen absorption time of 90 min, and a dehydrogenation temperature of 560 °C to obtain a coarse powder;

[0059] (3) Jet mill pulverization: add 0.08% of triphenylmethanol and 0.08% of 120# gasoline to the coarse powder, and grind them by jet mill until the average particle size is 3.2μm to obtain fine powder. The oxygen content of the jet mill is less than 50ppm, the grinding pressure is 0.6MPa, the bottom spray pressure is 0.5MPa, the classifying wheel speed is 3800rpm, and the grinding time is 4h; add 0.05% of triphenylmethanol, 0.05% of 120# gasoline, and 0.08% of ethylene glycol to the fine powder, mix them evenly and use them as magnetic powder;

[0060] (4) Anisostatic pressing: The magnetic powder is pressed vertically, the oxygen content is controlled below 400ppm, the forming magnetic field is 1.7T, the pressing pressure is 26T, the size is accurately controlled by mechanical limit, the volume is reduced by 10%, and pressure demolding is used. The density of the pressed magnetic blank is 4.3g / cm 3 , the pressed magnetic blank is directly loaded into the graphite box through the robot arm, and then transferred by the sealed box to the vacuum sintering furnace for sintering;

[0061] (5) Sintering: After the magnetic blank is transferred to the vacuum sintering furnace, the vacuum degree in the vacuum sintering furnace is maintained below 0.5 Pa, and the sintering is carried out by step-by-step heating. The temperature is raised to 300°C and kept for 1.5 hours, then raised to 650°C and kept for 2.5 hours, then raised to 850°C and kept for 3 hours, then raised to 1000°C and kept for 20 minutes, then raised to 1060°C and kept for 4 hours, and then cooled to below 70°C;

[0062] (6) Heat treatment: The sintered magnetic blank is subjected to three-stage tempering treatment, maintaining the vacuum degree below 0.5Pa. The first-stage tempering is heated to 930℃ and kept at this temperature for 2h, and then cooled to below 70℃; the second-stage tempering is heated to 700℃ and kept at this temperature for 3h, and then cooled to below 70℃; the third-stage tempering is heated to 450℃ and kept at this temperature for 1h, and then cooled to below 70℃ to obtain a sintered NdFeB cerium-containing magnet.

[0063] Example 3

[0064] Sintered NdFeB cerium-containing magnets were prepared as follows:

[0065] (1) Smelting: prepare the following materials in the following proportions by weight: 360 parts of iron, 30 parts of ferroboron (boron content 14wt.%, carbon content 0.1wt.%), 40 parts of cerium, 14 parts of gadolinium-iron alloy (total rare earth element content 75wt.%), 5 parts of dysprosium-iron alloy (total rare earth element content 75wt.%), 140 parts of praseodymium-neodymium metal (praseodymium content 85wt.%), 0.8 parts of gallium, 4 parts of cobalt, 1 part of copper, 3 parts of aluminum, 2 parts of zirconium, and 0.5 parts of titanium;

[0066] The raw materials are stacked in the vacuum belt furnace in order, with iron on the bottom layer, ferroboron, cerium, gadolinium iron alloy, and dysprosium iron alloy on the next bottom layer, praseodymium-neodymium metal on the middle layer, and gallium, cobalt, copper, aluminum, zirconium, and titanium on the upper layer. After the furnace is loaded, smelting begins. The vacuum belt furnace is evacuated to below 4Pa, and argon gas is injected into the furnace body. The initial heating power is 180kW, which is increased to 250kW within 10min, and then increased to 450kw at a rate of 10kW / min. When all the raw materials are melted, the heating power is increased. The power is increased to 530kW. When the temperature of the raw material rises to 1480℃, the heating power is reduced to 120kW, and the temperature is kept for 10 minutes. Then the heating power is returned to zero until the temperature of the raw material drops to 1400℃, and the smelting is completed; the heating is turned on again until the temperature of the raw material rises to 1480℃, and pouring is carried out. The thickness of the poured sheet is 0.2mm, and the pouring time is 10 minutes; after the pouring is completed, the sheet is crushed and cooled until the temperature of the sheet drops below 45℃, and then it is packed in a packaging bag and filled with argon for storage;

[0067] (2) Hydrogen crushing: The slabs are subjected to hydrogen absorption and dehydrogenation in sequence, with a hydrogen absorption pressure of 110 kPa, a hydrogen absorption time of 100 min, and a dehydrogenation temperature of 550 °C to obtain a coarse powder;

[0068] (3) Jet mill pulverization: add 0.12% of 1-hexadecanol and 0.12% of polyethylene glycol to the coarse powder, and grind them by jet mill until the average particle size is 2.6 μm to obtain fine powder. The oxygen content of the jet mill is less than 50 ppm, the grinding pressure is 0.5 MPa, the bottom spray pressure is 0.4 MPa, the classifying wheel speed is 3500 rpm, and the grinding time is 5 h; add 0.03% of 1-hexadecanol, 0.03% of polyethylene glycol, and 0.12% of glycerol to the fine powder, and mix them evenly to obtain magnetic powder;

[0069] (4) Anisostatic pressing: The magnetic powder is pressed vertically, the oxygen content is controlled below 400ppm, the forming magnetic field is 1.8T, the pressing pressure is 28T, the size is accurately controlled by mechanical limit, the volume is reduced by 13%, and pressure demolding is used. The density of the pressed magnetic blank is 4.5g / cm 3 , the pressed magnetic blank is directly loaded into the graphite box through the robot arm, and then transferred by the sealed box to the vacuum sintering furnace for sintering;

[0070] (5) Sintering: After the magnetic blank is transferred to the vacuum sintering furnace, the vacuum degree in the vacuum sintering furnace is maintained below 0.5 Pa, and the sintering is carried out by step-by-step heating. The temperature is raised to 300°C and kept for 1.5 hours, then raised to 650°C and kept for 2.5 hours, then raised to 850°C and kept for 3 hours, then raised to 1000°C and kept for 20 minutes, then raised to 1060°C and kept for 4 hours, and then cooled to below 70°C;

[0071] (6) Heat treatment: The sintered magnetic blank is subjected to three-stage tempering treatment, maintaining the vacuum degree below 0.5Pa. The first-stage tempering is heated to 920℃ and kept at this temperature for 3h, and then cooled to below 70℃; the second-stage tempering is heated to 650℃ and kept at this temperature for 4h, and then cooled to below 70℃; the third-stage tempering is heated to 420℃ and kept at this temperature for 1.5h, and then cooled to below 70℃ to obtain a sintered NdFeB cerium-containing magnet.

[0072] Comparative Example 1

[0073] The difference between this comparative example and Example 1 is that the process of combining orientation molding and isostatic pressing treatment is adopted in step (4), which is as follows:

[0074] The magnetic powder is vertically pressed, the oxygen content is controlled below 400ppm, the molding magnetic field is 1.8T, the pressing pressure is 20T, the size is precisely controlled by mechanical limit, and the volume is reduced by 5%. The pressed magnetic blank is coated and packaged in the glove box, and then put into a protective bag after discharge, and put into an outer packaging bag for outer packaging, and then isostatic pressing is performed with an isostatic pressure of 230Mpa. After isostatic pressing, it is transferred to the sintering furnace glove box for bag cutting, material stripping, and box placement, and then placed in a vacuum sintering furnace for sintering.

[0075] Comparative Example 2

[0076] The difference between this comparative example and Example 1 is that during the smelting in step (1), all raw materials are mixed and then placed in a vacuum belt furnace for smelting.

[0077] Comparative Example 3

[0078] The only difference between this comparative example and Example 1 is that during the jet mill pulverization in step (3), no molding aid glycerin is added to the fine powder.

[0079] Since no molding aid is added to the fine powder, when a vertical molding is used in step (4) for one-step molding, the magnetic blank is prone to cracking under a large pressing pressure, and the molding qualification rate is low.

[0080] Comparative Example 4

[0081] The only difference between this comparative example and Example 1 is that during the air flow milling in step (3), the antioxidant calcium stearate and the lubricant 120# gasoline originally added to the coarse powder are added to the fine powder instead.

[0082] Comparative Example 5

[0083] The difference between this comparative example and Example 1 is that titanium, zirconium and gallium are not added during the material preparation in step (1).

[0084] The NdFeB cerium-containing magnets prepared in each embodiment and comparative example were subjected to performance tests, wherein: the remanence (Br) and intrinsic coercive force (Hcj) were tested in accordance with the standard GB / T 3217-2013; the occurrence of cracks in the magnet blank during the molding process was recorded as cracking, and the magnet blank cracking ratio = the number of magnet blank cracks / the total number of magnet blanks × 100%, and the number of samples was not less than 50; the dimensional deformation was the absolute value of the difference between the final product size and the size of the magnet blank after molding, and was measured by the maximum deformation of the three side lengths. The test results are shown in Table 1.

[0085]

[0086] As can be seen from Table 1, the present invention not only introduces cerium element into the NdFeB magnet, but also adds other metal auxiliary elements. Through layered stacking and smelting, various forms of auxiliary alloy phases can be formed between the auxiliary metal elements and the rare earth elements, thereby weakening the negative impact of the rare earth elements on the magnetic properties of the main alloy phase, and greatly improving the remanence and intrinsic coercive force of the NdFeB containing cerium magnet. The remanence is greater than 13.5kGs, and the intrinsic coercive force is greater than 20kOe. In addition, the present invention adds lubricants and antioxidants to the magnetic powder in batches, which can greatly increase the dispersibility and lubricity of the magnetic powder. At the same time, the addition of the die-casting aid forms a protective film on the surface of the magnet, which reduces the generation of cracks in the magnet during die-casting. The cracking ratio of the magnetic blank does not exceed 2%, and the dimensional deformation is less than 0.1mm.

[0087] Comparative Example 1 adopts a process that combines orientation molding and isostatic pressing. Compared with the non-isostatic pressing preparation method of the present invention, the remanence is slightly lower, the coercive force is slightly higher, the magnet performance is roughly the same, the cracking ratio and dimensional deformation of the magnetic blank are also similar, but the isostatic pressing process is relatively cumbersome and the production efficiency is low.

[0088] In Comparative Example 2, all raw materials are mixed and then smelted, which is not conducive to the formation of various forms of auxiliary alloy phases between the auxiliary metal elements and the rare earth elements. The remanence and intrinsic coercive force of the obtained NdFeB cerium-containing magnet are both reduced.

[0089] In Comparative Example 3, no molding aid is added to the magnetic powder. During the one-step molding by vertical molding, the larger pressing pressure will cause the magnetic blank to crack, and the molding qualification rate is low.

[0090] In Comparative Example 4, antioxidant and lubricant are added to the magnetic powder at one time, which reduces the dispersion uniformity, resulting in an increase in the cracking ratio of the magnetic blank formed in one step by vertical die pressing and an increase in the product size deformation; at the same time, the uneven distribution of the magnetic powder during molding also leads to a decrease in the remanence and intrinsic coercive force of the NdFeB cerium-containing magnet.

[0091] In comparative example 5, titanium, zirconium and gallium are not added to the raw materials, so that the rare earth elements cannot form various forms of auxiliary alloy phases, which will have a negative impact on the magnetic properties of the main alloy phase, thereby reducing the remanence and intrinsic coercive force of the NdFeB cerium-containing magnet.

Claims

1. A method for preparing sintered NdFeB cerium-containing magnets by anisostatic pressing, characterized in that: The following steps are involved: (1) Smelting: The raw materials are stacked in a vacuum belt-spinning furnace in order, with iron on the bottom layer, ferroboron, cerium, gadolinium-iron alloy, and dysprosium-iron alloy on the next bottom layer, praseodymium-neodymium metal on the middle layer, and gallium, cobalt, copper, aluminum, zirconium, and titanium on the top layer. The raw materials are melted, cast, and cooled in an argon atmosphere to obtain spinning sheets. (2) Hydrogen crushing: The flakes are subjected to hydrogen absorption and dehydrogenation in sequence to obtain coarse powder; (3) Jet mill pulverization: Add antioxidant and lubricant to the coarse powder, use jet mill to mix and grind until the average particle size is between 2.6-3.2 μm to obtain fine powder, add antioxidant, lubricant and compression molding aid to the fine powder, mix well and use as magnetic powder; (4) Anisostatic pressing: The magnetic powder is pressed vertically, the oxygen content is controlled below 400ppm, the forming magnetic field is 1.7-1.8T, the pressing pressure is 25-28T, and the volume is reduced by 10-13%. The pressed magnetic blank is directly loaded into a graphite box, sealed and transported to a vacuum sintering furnace for sintering; (5) Sintering: The magnetic blank is sintered under vacuum conditions, with the sintering end temperature at 1050-1060°C. After keeping at this temperature for 4-6 hours, it is cooled; (6) Heat treatment: subjecting the sintered magnetic blank to three-stage tempering treatment, wherein the first-stage tempering temperature is 900-930°C, the second-stage tempering temperature is 600-700°C, and the third-stage tempering temperature is 400-450°C, and a sintered NdFeB cerium-containing magnet is obtained after the treatment; In step (1), the weight proportions of the raw materials are: 360-380 parts of iron, 25-30 parts of ferroboron, 40-45 parts of cerium, 14-18 parts of gadolinium-iron alloy, 4-5 parts of dysprosium-iron alloy, 130-140 parts of praseodymium-neodymium metal, 0.5-0.8 parts of gallium, 3-4 parts of cobalt, 0.5-1 parts of copper, 3-4 parts of aluminum, 1.5-2 parts of zirconium, and 0.5-0.8 parts of titanium.

2. The method for preparing sintered NdFeB cerium-containing magnets by anisostatic pressing according to claim 1, characterized in that: In step (1), during smelting, the temperature is first raised to 1450-1480°C and kept for 10-15 minutes, and then the temperature is lowered to 1350-1400°C.

3. The method for preparing sintered NdFeB cerium-containing magnets by anisostatic pressing according to claim 1, characterized in that: In step (1), the pouring temperature is 1450-1480°C, the pouring time is 10-12 minutes, and the pouring sheet thickness is 0.2-0.35 mm.

4. The method for preparing sintered NdFeB cerium-containing magnets by anisostatic pressing according to claim 1, characterized in that: In step (2), the hydrogen absorption pressure is 100-120 kPa, the hydrogen absorption time is 90-120 min, and the dehydrogenation temperature is 550-560 °C.

5. The method for preparing sintered NdFeB cerium-containing magnets by anisostatic pressing according to claim 1, characterized in that: In step (3), the antioxidant is at least one of 1-hexadecanol, triphenylmethanol, and calcium stearate; the amount of the antioxidant added to the coarse powder is 0.08-0.12% of the mass of the coarse powder; the amount of the antioxidant added to the fine powder is 0.08-0.12% of the mass of the fine powder; The lubricant is at least one of polyethylene glycol and 120# gasoline; the amount of the lubricant added to the coarse powder is 0.03-0.05% of the mass of the coarse powder; the amount of the lubricant added to the fine powder is 0.03-0.05% of the mass of the fine powder.

6. The method for preparing sintered NdFeB cerium-containing magnets by anisostatic pressing according to claim 1, characterized in that: In step (3), the molding aid is at least one of glycerol and ethylene glycol; the amount of the molding aid added to the fine powder is 0.08-0.12% of the mass of the fine powder.

7. The method for preparing sintered NdFeB cerium-containing magnets by anisostatic pressing according to claim 1, characterized in that: In step (3), the oxygen content of the air flow mill is less than 50 ppm, the grinding pressure is 0.5-0.6 MPa, the bottom spray pressure is 0.4-0.5 MPa, the sorting wheel speed is 3500-3800 rpm, and the grinding time is 4-5 h.

8. The method for preparing sintered NdFeB cerium-containing magnets by anisostatic pressing according to claim 1, characterized in that: In step (5), the temperature is raised in stages during sintering, the temperature is raised to 250-300°C and kept for 1.5-2h, the temperature is raised to 600-650°C and kept for 2-2.5h, the temperature is raised to 800-850°C and kept for 3-3.5h, the temperature is raised to 950-1000°C and kept for 20-30min, the temperature is raised to 1050-1060°C and kept for 4-6h, and then cooled to below 70°C.

9. The method for preparing sintered NdFeB cerium-containing magnets by anisostatic pressing according to claim 1, characterized in that: In step (6), during the three-stage tempering treatment, the vacuum degree is maintained below 0.5 Pa, the first-stage tempering is heated to 900-930°C and kept warm for 2-4 hours, and then cooled to below 70°C; the second-stage tempering is heated to 600-700°C and kept warm for 3-5 hours, and then cooled to below 70°C; the third-stage tempering is heated to 400-450°C and kept warm for 1-2 hours, and then cooled to below 70°C.