A method for preparing samarium cobalt permanent magnetic material

By mixing element ratio and process of samarium-cobalt permanent magnet materials, the ABA three-layer structure green body is formed, which solves the problem of reduced coercive force of samarium-cobalt permanent magnet materials, and realizes the preparation and industrialization of high-performance samarium-cobalt permanent magnet materials. Hydrogen breaking improves the overall performance of magnetic materials.

CN114597042BActive Publication Date: 2024-11-26HANGZHOU ZHIYU MAGNETIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210128010.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-11
Publication Date
2024-11-26
Estimated Expiration
2042-02-11

AI Technical Summary

Technical Problem

When the existing samarium-cobalt permanent magnet material increases magnetic energy accumulation, after the iron content exceeds 17 wt%, the coercive force of the magnet is greatly deteriorated, and it cannot be used as a normal permanent magnet material, making it difficult to achieve the preparation of high-performance samarium-cobalt permanent magnet material.

Method used

By mixing the element ratios of the first alloy ingot and the second alloy ingot, high-performance samarium-cobalt permanent magnet material is prepared. The combination of mechanical crushing and hydrogen crushing is used to form a three-layer layered green body of ABA and perform Isostatic pressure, sintering solid solution and aging treatment, control iron content and composition to improve magnetic properties.

Benefits of technology

It realizes the high coercive force and residual magnetic properties of samarium-cobalt permanent magnet materials, is suitable for industrial applications, and improves the overall performance of magnetic materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDF0000033518200000061
    Figure GDF0000033518200000061
  • Figure GDF0000033518200000071
    Figure GDF0000033518200000071
Patent Text Reader

Abstract

The present invention belongs to the technical field of rare earth magnet materials and relates to a method for preparing a high-performance samarium-cobalt permanent magnet material, comprising the following steps: preparing a first alloy ingot and a second alloy ingot, wherein the chemical atomic formula of the first alloy ingot is Sm(Co 1‑a‑b‑ c Fe a Cu b Zr c ) z , 0.05≤a≤0.25, the chemical atomic formula of the second alloy ingot is Sm(Co 1‑d‑e‑f Fe d Cu e Zr f ) n , 0.25
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of rare earth magnet materials technology, and relates to a method for preparing samarium cobalt permanent magnet materials. Background Technology

[0002] In 1967, the United States successfully produced SmCo5 permanent magnets using a powder bonding method, marking the arrival of the rare-earth permanent magnet era. To date, rare-earth permanent magnet materials are the highest-performing permanent magnet materials known, boasting magnetic properties more than 100 times higher than the magnets used in the 19th century, significantly superior to ferrite and AlNiCo, and even twice as high as expensive platinum-cobalt alloys. The use of rare-earth permanent magnet materials has not only promoted the miniaturization of permanent magnet devices and improved product performance but has also spurred the development of certain specialized devices. Therefore, the emergence of rare-earth permanent magnet materials immediately attracted great attention from various countries. Rare-earth permanent magnets are divided into samarium cobalt (SmCo) permanent magnets and neodymium iron boron (NdFeB) permanent magnets. Samarium cobalt magnets are divided into two types: 1:5 (SmCo5) and 2:17 (Sm2Co17). Their main characteristics are high magnetic properties, good temperature performance, and a maximum operating temperature of 250–350 degrees Celsius. Compared to neodymium iron boron magnets, at operating temperatures above 180℃, its maximum magnetic energy product, temperature stability, and chemical stability all exceed those of neodymium iron boron permanent magnet materials, making it very suitable for manufacturing various high-performance permanent magnet motors and products used in applications with very complex operating environments.

[0003] Samarium cobalt rare earth permanent magnet materials are composed of samarium, cobalt, and other rare earth metallic materials in a specific ratio. The traditional preparation method is as follows: batching – melting and casting – powdering – magnetic field orientation molding – sintering and solution treatment – ​​aging. Controlling the raw material ratio and preparation method is essential for preparing high-performance samarium cobalt permanent magnet materials.

[0004] The theoretical magnetic energy product of samarium cobalt can reach over 50 MGOe, but in practice, achieving a magnetic energy product of over 32 MGOe is extremely difficult. One method to improve the magnetic energy product of samarium cobalt is to increase the iron content. However, when the iron content exceeds 17 wt%, the coercivity of the magnet begins to deteriorate significantly. Especially when the iron content exceeds 18 wt%, the coercivity of the magnet drops to almost below 5 kOe, rendering it unusable as a normal permanent magnet material. Summary of the Invention

[0005] This invention provides a method for preparing high-performance samarium cobalt permanent magnet materials. By adjusting the elemental ratio of the first alloy ingot and the second alloy ingot, and combining it with the preparation method, high-performance samarium cobalt permanent magnet materials can be obtained.

[0006] One objective of this invention is achieved through the following technical solution:

[0007] A method for preparing a high-performance samarium cobalt permanent magnet material includes the following steps:

[0008] (1) Prepare the first alloy ingot and the second alloy ingot separately in a melting furnace according to the element ratios. The chemical atomic formula of the first alloy ingot is Sm(Co z , Fe a Cu b Zr c ) z , 0.05 ≤ a ≤ 0.25, 0 ≤ b ≤ 0.15, 0 ≤ c ≤ 0.04, 6.5 ≤ z ≤ 8.3; The chemical atomic formula of the second alloy ingot is Sm(Co 1-d-e-f Fe d Cu e Zr f ) n , 0.25 < d ≤ <000005>0.5, 0 ≤ e ≤ 0.15, 0 ≤ f ≤ 0.04, 6.5 ≤ z ≤ 8.3; The first alloy ingot contains a lower iron content, which mainly provides a higher coercivity for the entire magnet after subsequent preparation; while the second alloy ingot contains more iron content, which provides a higher remanence for the entire magnet after subsequent preparation, and the presence of a higher iron content facilitates the industrial hydrogen decrepitation of the material.

[0009] (2) Mechanically crush the first alloy ingot to an average particle size of 100 - 300 μm, and then further crush it with a jet mill to obtain alloy powder A; Subject the second alloy ingot to hydrogen absorption at a hydrogen absorption temperature of 20 - 180 °C and a hydrogen pressure of 0.2 - 0.5 MPa for 1 - 5 h, and then dehydrogenate it by holding at 280 - 300 °C for 1 - 2 h to obtain hydrogen decrepitated powder B, and then further crush it with a jet mill to obtain alloy powder B.

[0010] [[ID=​​​​​​​​​​​​​​Preferably, the average particle size of alloy powder A and alloy powder B is 2.2–4.0 μm.

[0016] As a preferred option, the layer pressing step in step (3) includes: first pressing alloy powder A into a thin sheet A, then pouring in alloy powder B, pressing it into a two-layer structure of AB, and finally pouring alloy powder A into a mold to press it into a three-layer structure of ABA; the pressing process is carried out under inert protection and a magnetic field of 1.2 to 2T, and the pressing pressure is 4 to 10 MPa.

[0017] Alternatively, the layered pressing step in step (3) includes: dividing alloy powder A into two parts and pressing them into green blank A and green blank A' respectively; pressing alloy powder B into green blank B; then splicing green blank A, green blank B and green blank A' together, packing them into a plastic bag and vacuum fixing them to form a layered green blank with a three-layer ABA structure. All the pressing processes are carried out under inert protection and a magnetic field of 1.2 to 2T, with a pressing pressure of 4 to 10 MPa.

[0018] Samarium cobalt's coercivity mechanism is pinning. To improve the coercivity of a magnet, it is necessary to make it difficult for antimagnetic domains to form or for their walls to expand. Once antimagnetic domains form, it signifies the beginning of magnet demagnetization, which in turn causes surrounding magnetic domains to flip, ultimately demagnetizing the magnet. The externally observed magnetic parameter is low coercivity. Antimagnetic domains are most likely to form and expand on the magnet surface, therefore, a "hardening layer" with high coercivity needs to be added to the magnet surface. Alloy powder A contains a low iron content, which can provide high coercivity. Therefore, in the ABA three-layered layered green blank formed in this invention, alloy powder A is located on the surface of the green blank, which is beneficial to improving the performance of the magnetic material.

[0019] Preferably, in the ABA three-layered green body, the thickness of the two A layers is 1-5 mm, and the thickness of the middle B layer is pressed into the corresponding size as needed. Preferably, the thickness of the B layer is 5-50 mm.

[0020] Preferably, the isostatic pressing in step (4) involves placing the green billet under a pressure of 100–300 MPa for cold isostatic pressing, holding the pressure for 1–10 minutes, and then releasing the pressure in two stages. The first stage releases the pressure from the highest value to 40–60 MPa, holding the pressure for 1–10 minutes, and then releasing the pressure to atmospheric pressure. Since the powder is pressed in batches, a large stress will be generated on the contact surface. This stress will be further released during the isostatic pressing process. The two-stage pressure release can effectively eliminate the pressing stress and prevent internal cracks in the green billet.

[0021] Preferably, the sintering and solution treatment in step (4) is performed by sintering the blank after isostatic pressing at 1180-1220°C for 30-240 min, followed by solution treatment at 1150-1195°C for 3-10 h, and finally air-cooling to room temperature.

[0022] As a preferred embodiment, the aging treatment in step (4) is as follows: the magnet after sintering and solution treatment is isothermally aged at 800-850℃ for 10-40h, then slowly cooled to 380-450℃ at a cooling rate of 0.5-1.5℃ / min, held for 2-10h, and finally air-cooled to room temperature to obtain samarium cobalt permanent magnet material.

[0023] Another objective of this invention is achieved through the following technical solution: a high-performance samarium cobalt permanent magnet material, which is prepared by the above-described preparation method.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The present invention regulates the composition of samarium cobalt permanent magnet material so that the first alloy ingot contains a low iron content, which mainly provides high coercivity for the entire magnet after subsequent preparation, while the second alloy ingot contains a higher iron content, which provides high remanence for the entire magnet after subsequent preparation. At the same time, the presence of high iron content can facilitate the industrial hydrogen pyrolysis of the material.

[0026] (2) In this invention, alloy powder A and alloy powder B are pressed in layers to form a layered structure green blank with three layers of ABA. Alloy powder A contains a low iron content, which can provide high coercivity. In the layered structure green blank with three layers of ABA, alloy powder A is located on the surface of the green blank, which is equivalent to adding a "hardening layer" with high coercivity to the surface of the magnet, which is beneficial to improving the performance of magnetic materials.

[0027] (3) Due to the special composition of the first alloy ingot and the second alloy ingot, the first alloy ingot is crushed by mechanical crushing + air jet milling, and the second alloy ingot is crushed by hydrogen crushing + air jet milling. This crushing mode is beneficial to improving the performance of permanent magnet materials.

[0028] (4) By controlling the composition and preparation method of samarium cobalt permanent magnets, this invention has successfully obtained samarium cobalt permanent magnet materials with excellent magnet performance. Detailed Implementation

[0029] The technical solution of the present invention will be further described and illustrated below through specific embodiments. It should be understood that the specific embodiments described herein are only for the purpose of helping to understand the present invention and are not intended to limit the present invention. Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.

[0030] Example 1

[0031] The samarium-cobalt permanent magnet material in this embodiment is prepared by the following steps:

[0032] (1) A first alloy ingot and a second alloy ingot are prepared in a furnace according to the proportions of each element, wherein the chemical atomic stoichiometry of the first alloy ingot is Sm(Co). 0.69 Fe 0.22 Cu 0.06 Zr 0.03 ) 7.85 The chemical atomic stoichiometry of the second alloy ingot is Sm(Co) 0.61 Fe 0.30 Cu 0.06 Zr 0.03 ) 7.85 .

[0033] (2) The first alloy ingot is first crushed into an average particle size of 150 μm by a medium crusher, and then further crushed by an air jet mill to obtain alloy powder A with an average particle size of 3.8 μm; the second alloy ingot is subjected to hydrogen absorption at a hydrogen absorption temperature of 100℃ and a hydrogen pressure of 0.3 MPa for 1 h, and then dehydrogenated at 280℃ for 2 h to obtain hydrogen-crushed powder B with an average particle size of 150 μm, and then further crushed by an air jet mill to obtain alloy powder B with an average particle size of 3.8 μm.

[0034] (3) First, alloy powder A is pressed into a thin sheet A, then alloy powder B is poured in and pressed on the thin sheet A to form a thin sheet B, forming a two-layer structure of AB. Finally, alloy powder A is poured into a mold and pressed on the thin sheet B to form a thin sheet A, forming a three-layer structure green blank of ABA. In the three-layer structure green blank of ABA, the thickness of the A layer on both sides is 1mm, and the thickness of the B layer in the middle is 8mm. All the pressing processes are carried out under N2 protection and a magnetic field of 1.5T, and the pressing pressure is 8MPa.

[0035] (4) Place the green billet from step (3) under a pressure of 280 MPa for cold isostatic pressing. The pressure holding time is 3 min. Then, the pressure is released in two stages. The first stage of pressure release is from the highest value to 40 MPa, and the pressure is held for 8 min. Then, the pressure is released to atmospheric pressure.

[0036] (5) The isostatically pressed blank was sintered at 1210℃ for 180 min, then solution-treated at 1170℃ for 4 h, and finally air-cooled to room temperature. The sintered and solution-treated magnet was isothermally aged at 830℃ for 10 h, then slowly cooled to 400℃ at a cooling rate of 0.6℃ / min, held at that temperature for 3.5 h, and finally air-cooled to room temperature to obtain samarium cobalt permanent magnet material.

[0037] Example 2

[0038] The samarium-cobalt permanent magnet material in this embodiment is prepared by the following steps:

[0039] (1) A first alloy ingot and a second alloy ingot are prepared in a furnace according to the proportions of each element, wherein the chemical atomic stoichiometry of the first alloy ingot is Sm(Co). 0.71 Fe 0.20 Cu 0.06 Zr 0.03 ) 7.85 The chemical atomic stoichiometry of the second alloy ingot is Sm(Co) 0.6 Fe 0.32 Cu 0.06 Zr 0.02 ) 7.85 .

[0040] (2) The first alloy ingot is first crushed into an average particle size of 200 μm by a medium crusher, and then further crushed by an air jet mill to obtain alloy powder A with an average particle size of 3.5 μm; the second alloy ingot is subjected to hydrogen absorption at a hydrogen absorption temperature of 80℃ and a hydrogen pressure of 0.32 MPa for 2 h, and then dehydrogenated at 290℃ for 1.5 h to obtain hydrogen-crushed powder B with an average particle size of 180 μm, and then further crushed by an air jet mill to obtain alloy powder B with an average particle size of 3.5 μm.

[0041] (3) Divide alloy powder A into two parts and press them into green blank A and green blank A' respectively. Press alloy powder B into green blank B. Then, splice green blank A, green blank B and green blank A' together, put them into a plastic bag and vacuum fix them to form a layered structure green blank with three layers of ABA. In the layered structure green blank with three layers of ABA, the thickness of the A layer on both sides is 2mm and the thickness of the B layer in the middle is 10mm. All the pressing processes are carried out under N2 protection and a magnetic field of 1.5T, and the pressing pressure is 8MPa.

[0042] (4) Place the green billet from step (3) under a pressure of 250 MPa for cold isostatic pressing. The pressure holding time is 4 min. Then, the pressure is released in two stages. The first stage of pressure release is from the highest value to 45 MPa, and the pressure is held for 7 min. Then, the pressure is released to atmospheric pressure.

[0043] (5) The isostatically pressed blank was sintered at 1200℃ for 240 min, then solution-treated at 1160℃ for 5 h, and finally air-cooled to room temperature. The sintered and solution-treated magnet was isothermally aged at 820℃ for 11 h, then slowly cooled to 420℃ at a cooling rate of 0.7℃ / min, held at that temperature for 3 h, and finally air-cooled to room temperature to obtain samarium cobalt permanent magnet material.

[0044] Example 3

[0045] The samarium-cobalt permanent magnet material in this embodiment is prepared by the following steps:

[0046] (1) A first alloy ingot and a second alloy ingot are prepared in a furnace according to the proportions of each element, wherein the chemical atomic stoichiometry of the first alloy ingot is Sm(Co). 0.76 Fe 0.15 Cu 0.06 Zr 0.03 ) 7.75 The chemical atomic stoichiometry of the second alloy ingot is Sm(Co) 0.58 Fe 0.34 Cu 0.06 Zr 0.02 ) 7.85 .

[0047] (2) The first alloy ingot is first crushed into an average particle size of 120 μm by a medium crusher, and then further crushed by an air jet mill to obtain alloy powder A with an average particle size of 3.0 μm; the second alloy ingot is subjected to hydrogen absorption at a hydrogen absorption temperature of 120℃ and a hydrogen pressure of 0.35 MPa for 1 h, and then dehydrogenated at 300℃ for 1 h to obtain hydrogen-crushed powder B with an average particle size of 120 μm, and then further crushed by an air jet mill to obtain alloy powder B with an average particle size of 3.0 μm.

[0048] (3) First, alloy powder A is pressed into a thin sheet A, then alloy powder B is poured in and pressed on the thin sheet A to form a thin sheet B, forming an AB two-layer structure. Finally, alloy powder A is poured into a mold and pressed on the thin sheet B to form a thin sheet A, forming an ABA three-layer structure green blank. In the ABA three-layer structure green blank, the thickness of the A layer on both sides is 2mm, and the thickness of the B layer in the middle is 6mm. All the pressing processes are carried out under N2 protection and a 2T magnetic field, and the pressing pressure is 6MPa.

[0049] (4) Place the green billet from step (3) under a pressure of 220 MPa for cold isostatic pressing. Hold the pressure for 5 minutes. Then depressurize in two stages. In the first stage, depressurize from the highest value to 50 MPa and hold the pressure for 8 minutes. Then depressurize to atmospheric pressure.

[0050] (5) The isostatically pressed blank was sintered at 1220℃ for 180 min, then solution-treated at 1170℃ for 5 h, and finally air-cooled to room temperature. The sintered and solution-treated magnet was isothermally aged at 830℃ for 10 h, then slowly cooled to 390℃ at a cooling rate of 0.8℃ / min, held at that temperature for 4 h, and finally air-cooled to room temperature to obtain samarium cobalt permanent magnet material.

[0051] Comparative Example 1

[0052] The difference between Comparative Example 1 and Example 1 is that the first alloy ingot of Comparative Example 1 has the chemical atomic stoichiometry of Sm(Co). 0.63 Fe 0.28 Cu 0.06 Zr0.03 ) 7.75 The chemical atomic stoichiometry of the second alloy ingot is Sm(Co) 0.58 Fe 0.34 Cu 0.06 Zr 0.02 ) 7.85 Everything else is the same as in Example 3.

[0053] Comparative Example 2

[0054] The difference between Comparative Example 2 and Example 3 is that the first alloy ingot of Comparative Example 1 has the chemical atomic stoichiometry Sm(Co) 0.58 Fe 0.34 Cu 0.06 Zr 0.02 ) 7.85 The chemical atomic stoichiometry of the second alloy ingot is Sm(Co) 0.76 Fe 0.15 Cu 0.06 Zr 0.03 ) 7.75 Everything else is the same as in Example 3.

[0055] Sm(Co 0.76 Fe 0.15 Cu 0.06 Zr 0.03 ) 7.75 The chemical atomic stoichiometry of the second alloy ingot is Sm(Co) 0.58 Fe 0.34 Cu 0.06 Zr 0.02 ) 7.85 .

[0056] Comparative Example 3

[0057] The difference between Comparative Example 3 and Example 3 is that in Comparative Example 3, alloy powder A and alloy powder B of the same mass as those in the three-layered ABA structure green blank of Example 3 were mixed and pressed together to a thickness of 10 mm. Otherwise, they were the same as in Example 3.

[0058] Comparative Example 4

[0059] The difference between Comparative Example 4 and Example 3 is that in Comparative Example 4, alloy powder A of the same mass as in the three-layered ABA structure green blank of Example 3 is pressed into a thin sheet A, and then alloy powder B is poured in and pressed on the thin sheet A to form a thin sheet B, forming a two-layered AB structure with a thickness of 10 mm. Everything else is the same as in Example 3.

[0060] Comparative Example 5

[0061] The difference between Comparative Example 5 and Example 3 is that in Comparative Example 5, the second alloy ingot was first crushed into an average particle size of 120 μm using a medium crusher, and then further crushed into alloy powder B with an average particle size of 3.0 μm using an air jet mill. Otherwise, it was the same as in Example 3.

[0062] The performance of the samarium cobalt permanent magnet materials of Examples 1-3 and Comparative Examples 1-5 was tested, and the results are shown in Table 1.

[0063] Table 1 Performance data of samarium cobalt permanent magnet materials in Examples 1-3 and Comparative Examples 1-5

[0064]

[0065]

[0066] As can be seen from Table 1, when the Fe content of the first alloy ingot and the second alloy ingot is not appropriate, the coercivity of the samarium cobalt permanent magnet material is significantly affected and greatly reduced, and the magnetic energy product BHm also shows a decrease. Since alloy powder A and alloy powder B are not pressed into a layered structure of ABA three layers, a "hardened layer" with high coercivity is not formed on the magnet surface, resulting in a significant reduction in the coercivity of the samarium cobalt permanent magnet material. After the second alloy ingot adopts the hydrogen-breaking process, the remanence is significantly improved compared with the one without the hydrogen-breaking process.

[0067] Finally, it should be noted that the specific embodiments described herein are merely illustrative of the spirit of the invention and are not intended to limit the implementation of the invention. Those skilled in the art can make various modifications or additions to the described embodiments or use similar methods to replace them; it is neither necessary nor possible to exemplify all embodiments here. However, these obvious variations or modifications derived from the essential spirit of the invention still fall within the scope of protection of the invention, and interpreting them as any additional limitation would contradict the spirit of the invention.

Claims

1. A method for preparing a samarium cobalt permanent magnet material, characterized in that: The following steps are involved: (1) A first alloy ingot and a second alloy ingot are prepared in a furnace according to the ratio of each element, wherein the chemical atomic formula of the first alloy ingot is Sm(Co 0.69 Fe 0.22 Cu 0.06 Zr 0.03 ) 7.85 The chemical atomic formula of the second alloy ingot is Sm(Co 0.61 Fe 0.30 Cu 0.06 Zr 0.03 ) 7.85 ; (2) The first alloy ingot is first crushed into an average particle size of 150 μm by a medium crusher, and then further crushed by a jet mill to obtain alloy powder A with an average particle size of 3.8 μm; the second alloy ingot is hydrogenated for 1 hour at a hydrogen absorption temperature of 100°C and a hydrogen pressure of 0.3 MPa, and then dehydrogenated at 280°C for 2 hours to obtain hydrogen-broken powder B with an average particle size of 150 μm, and then further crushed by a jet mill to obtain alloy powder B with an average particle size of 3.8 μm; (3) Alloy powder A is first pressed into thin sheet A, then alloy powder B is poured in, and thin sheet B is pressed on thin sheet A to form an AB two-layer structure. Finally, alloy powder A is poured into a mold and pressed on thin sheet B to form thin sheet A to form an ABA three-layer layered structure green body. In the ABA three-layer layered structure green body, the thickness of the A layer on both sides is 1 mm, and the thickness of the B layer in the middle is 8 mm. The above pressing process is carried out under N2 protection and a 1.5T magnetic field, and the pressing pressure is 8 MPa. (4) placing the green body of step (3) under a pressure of 280 MPa for cold isostatic pressing, holding the pressure for 3 min, and then releasing the pressure in two stages, wherein the first stage of pressure release is from the maximum value to 40 MPa, holding the pressure for 8 min, and then releasing the pressure to atmospheric pressure; (5) The isostatically pressed blank was sintered at 1210°C for 180 min, then solution treated at 1170°C for 4 h, and finally air-cooled to room temperature; the sintered solution treated magnet was isothermally aged at 830°C for 10 h, then slowly cooled to 400°C at a cooling rate of 0.6°C / min, kept at this temperature for 3.5 h, and finally air-cooled to room temperature to obtain the samarium cobalt permanent magnet material.

2. A samarium cobalt permanent magnet material, characterized in that: It is prepared by the preparation method described in claim 1.