Thermally conductive and leak-proof polyethylene glycol composite phase change material and preparation method thereof

By using porous BN fibers to load PEG@SiO2 microencapsulated phase change materials in polyethylene glycol phase change materials and carrying out modification and vacuum melt infiltration technology, the thermal conductivity and leakage prevention deficiencies of polyethylene glycol phase change materials are solved. problem, achieving efficient thermal energy management and temperature control.

CN118580840BActive Publication Date: 2024-10-25XIAN UNIV OF TECH

Patent Information

Application Number
CN202411067843.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-25
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The thermal conductivity of polyethylene glycol phase change materials is low, resulting in inefficient thermal energy storage and temperature control, and it is prone to flow, diffusion and loss problems during the phase change process.

Method used

Porous BN fibers are used as the skeleton, and PEG@SiO2 microencapsulated phase change materials are loaded and modified by hydroxylation, combined with vacuum-assisted melt infiltration technology to form polyethylene glycol composite phase change materials with enhanced thermal conductivity and anti-leakage.

Benefits of technology

It significantly improves the thermal conductivity and leakage prevention performance of polyethylene glycol phase change materials, forms an efficient heat conduction path, and reduces the decline in phase change performance. It is suitable for thermal energy storage, temperature control, cold chain logistics and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention discloses a method for preparing a thermally conductive enhanced anti-leakage polyethylene glycol composite phase change material, which is specifically implemented according to the following steps: step 1, preparing porous BN fibers; step 2, preparing porous BN fibers loaded with PEG@SiO2 microencapsulated phase change materials; step 3, constructing aerogels and hydroxylation modification; step 4, vacuum-assisted melt infiltration. The present invention also discloses a phase change material prepared by a method for preparing a thermally conductive enhanced anti-leakage polyethylene glycol composite phase change material. The thermally conductive enhanced anti-leakage polyethylene glycol composite phase change material prepared by the present invention not only greatly improves the anti-leakage performance of the polyethylene glycol phase change material, but also the aerogel skeleton and the SiO2 shell microcapsules loaded thereon also cooperate to form an efficient heat conduction path, thereby enhancing the thermal conductivity of the polyethylene glycol phase change material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of phase change materials, and in particular relates to a thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material, and also relates to a preparation method of the phase change material. Background Art

[0002] In recent years, lithium-ion batteries have been used as the main energy source for electric vehicles due to their high energy density, no memory effect, and long cycle life. The performance and life of the battery system are limited by the operating temperature. If the heat generated by the battery is not dissipated in time, the battery's performance and service life will be damaged. At present, various cooling methods for battery modules have been widely studied. Generally speaking, active cooling requires additional auxiliary consumable equipment and space, which will increase the cost and weight accordingly. In contrast, the battery thermal management system based on phase change materials has attracted much attention due to its advantages such as simple structural design, high cooling efficiency, and low maintenance cost.

[0003] Polyethylene glycol (PEG) is a multi-purpose solid-liquid phase change material with the advantages of small phase change expansion coefficient, no supercooling and phase separation, no corrosion, direct processing and molding, and a wide phase change temperature. It has great potential value in thermal energy storage, temperature control, cold chain logistics, etc. However, when the external temperature reaches the initial melting temperature of the polyethylene glycol phase change material, the phase change material begins to absorb heat and changes from solid to liquid, resulting in problems such as flow, diffusion and loss, which affect the use of polyethylene glycol phase change materials. In addition, the thermal conductivity of polyethylene glycol phase change materials is low, which is not conducive to the rapid response of heat storage and release. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a thermally conductive and leak-proof polyethylene glycol composite phase change material, thereby solving the problem of low thermal conductivity of polyethylene glycol phase change materials in the prior art.

[0005] Another object of the present invention is to provide a phase change material prepared by a method for preparing a thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material.

[0006] The technical solution adopted by the present invention is a method for preparing a thermally conductive and leak-proof polyethylene glycol composite phase change material, which is specifically implemented according to the following steps:

[0007] Step 1, preparing porous BN fibers;

[0008] Step 2, preparing porous BN fiber loaded with PEG@SiO2 microencapsulated phase change material;

[0009] Step 3, constructing aerogel and modifying it by hydroxylation;

[0010] Step 4: vacuum-assisted melt infiltration.

[0011] The present invention is also characterized in that:

[0012] In step 1, specifically: pure SiO2 microspheres are used as templates, mixed with H3BO3 and C3H6N6, added with deionized water and stirred, then naturally cooled and filtered, dried and calcined in a nitrogen atmosphere, finally HF was used to remove SiO2, and porous BN fibers were obtained after washing and drying.

[0013] In step 2, specifically: prepare a polyethylene glycol solution and an ethanol solution of tetraethyl silicate, then mix the two, add the mixed solution to the porous BN fiber obtained in step 1 and add ammonia water dropwise, filter and wash with deionized water and anhydrous ethanol respectively and then dry, and after drying, obtain a porous BN fiber loaded with PEG@SiO2 microencapsulated phase change material.

[0014] In step 3, specifically: the porous BN fiber loaded with PEG@SiO2 microencapsulated phase change material obtained in step 2 is added with deionized water, and then placed in a mold for directional freeze-drying to obtain a porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material, and then placed in a NaOH solution for vacuum impregnation, and after drying, a hydroxylated-modified porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material is obtained.

[0015] In step 4, specifically: polyethylene glycol is placed in a beaker, a surfactant is added and stirred, and then the hydroxylated modified porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material obtained in step 3 is placed in polyethylene glycol, vacuum-assisted melt infiltration is performed, and the thermally conductive enhanced and leak-proof polyethylene glycol composite phase change material is taken out.

[0016] In step 1, the diameter of pure SiO2 microspheres is 20μm~50μm, the dosage is 4wt.%~10 wt.%, the molar ratio of H3BO3 and C3H6N6 is 3:1, the stirring temperature and time are 90℃ and 4h respectively, the drying temperature and time are 60℃ and 12h respectively, the calcination temperature is 1100℃, and the heat preservation is 2h.

[0017] In step 2, the polyethylene glycol is PEG6000, which is a polyethylene glycol aqueous solution with a mass fraction of 50wt.%, the tetraethyl silicate ethanol solution is a tetraethyl silicate ethanol solution with a mass fraction of 25wt.% to 40wt.%, the mixing temperature is 50°C, the time is 30min, the dropping rate of ammonia water is 0.2mol / min to 0.8mol / min, and the mixture is mixed at 50°C for 20h during the dropping of ammonia water. The product after suction filtration is washed 3 times with deionized water and 2 times with anhydrous ethanol. The drying time and temperature are 12h and 60°C, respectively.

[0018] In step 3, the directional freeze-drying parameters are: freezing at -45°C to -15°C for 2h to 3.5h, drying at 1Pa to 2Pa for 40h to 50h, NaOH solution concentration of 3.5mol / L, immersion for 3h, and drying time and temperature are 12h and 60°C respectively.

[0019] In step 4, the surfactant is hexadecyltrimethylammonium bromide, the stirring temperature is 70° C., the time is 2 h, the vacuum oven temperature is 75° C. to 90° C., and the penetration time is 65 min to 80 min.

[0020] Another technical solution adopted by the present invention is to prepare the thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material by adopting the preparation method of the thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material.

[0021] The beneficial effects of the present invention are:

[0022] The invention discloses a method for preparing a thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material. The prepared thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material has a fiber aerogel as a skeleton, and PEG@SiO2 microencapsulated phase change material is loaded on the pores and surface of the fiber, and polyethylene glycol is infiltrated into the fiber after modification to form a composite phase change material. The combination of the skeleton and the microencapsulated phase change material not only greatly improves the leakage-proof performance of the polyethylene glycol phase change material, but also the aerogel skeleton and the SiO2 shell microcapsules loaded thereon also synergistically form an efficient heat conduction path, thereby enhancing the thermal conductivity of the polyethylene glycol phase change material. The pore size on the BN fiber is regulated to make the loaded microcapsules larger, and more polyethylene glycol is adsorbed at the same time. Compared with the phase change performance of other polyethylene glycol composite phase change materials, the decline is also smaller. DETAILED DESCRIPTION

[0023] The present invention is described in detail below in conjunction with specific implementation modes.

[0024] The preparation method of the thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material of the present invention is specifically implemented according to the following steps:

[0025] Step 1, preparing porous BN fibers;

[0026] Pure silica (SiO2) microspheres were used as templates, mixed with boric acid (H3BO3) and melamine (C3H6N6), added with deionized water, stirred, then naturally cooled and filtered, dried, calcined in a nitrogen atmosphere, and finally SiO2 was removed with hydrofluoric acid (HF). After washing and drying, porous BN fibers were obtained.

[0027] In step 1, the diameter of the pure SiO2 microspheres is 20 μm to 50 μm, the dosage is 4 wt.% to 10 wt.%, the molar ratio of H3BO3 to C3H6N6 is 3:1, the stirring temperature and time are 90°C and 4 h, respectively, the drying temperature and time are 60°C and 12 h, respectively, the calcination temperature is 1100°C, and the heat preservation is 2 h;

[0028] Step 2, preparing porous BN fiber loaded with PEG@SiO2 microencapsulated phase change material;

[0029] Prepare a polyethylene glycol (PEG) solution and an ethanol solution of tetraethyl silicate (TEOS), then mix the two, add the porous BN fiber obtained in step 1 and drop ammonia (NH3·H2O), continue mixing, filter, wash with deionized water and anhydrous ethanol respectively, and then dry to obtain a porous BN fiber loaded with PEG@SiO2 microencapsulated phase change material;

[0030] In step 2, the polyethylene glycol is PEG6000, which is a polyethylene glycol aqueous solution with a mass fraction of 50wt.%, the tetraethyl silicate ethanol solution is a tetraethyl silicate ethanol solution with a mass fraction of 25wt.% to 40wt.%, the mixing temperature is 50°C, the time is 30min, the dropping rate of ammonia water is 0.2mol / min to 0.8mol / min, and the ammonia water is added dropwise at 50°C for 20h. The product after suction filtration is washed 3 times with deionized water and 2 times with anhydrous ethanol, and the drying time and temperature are 12h and 60°C, respectively;

[0031] Step 3, constructing aerogel and modifying it by hydroxylation;

[0032] The porous BN fiber loaded with PEG@SiO2 microencapsulated phase change material obtained in step 2 is added with deionized water, and then placed in a mold for directional freeze drying to obtain a porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material, which is then placed in a NaOH solution for vacuum impregnation, and after drying, a hydroxylated-modified porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material is obtained;

[0033] In step 3, the directional freeze-drying parameters are: freezing at -45°C to -15°C for 2h to 3.5h, drying at 1Pa to 2Pa for 40h to 50h, NaOH solution concentration of 3.5mol / L, immersion for 3h, drying time and temperature of 12h and 60°C respectively;

[0034] Step 4, vacuum-assisted melt infiltration;

[0035] Put polyethylene glycol (PEG) into a beaker, add a surfactant, stir, then put the hydroxylated modified porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material obtained in step 3 into the polyethylene glycol, perform vacuum-assisted melt infiltration, take it out after infiltration, and obtain a thermally conductive enhanced and leak-proof polyethylene glycol composite phase change material;

[0036] In step 4, the surfactant is hexadecyltrimethylammonium bromide (CTAB), the stirring temperature is 70° C., the time is 2 h, the vacuum oven temperature is 75° C. to 90° C., and the penetration time is 65 min to 80 min.

[0037] The invention adopts a hard template method to prepare porous BN fibers, adopts a sol-gel method to load the prepared PEG@SiO2 microencapsulated phase change material inside and outside the pores of the fibers, controls the size of the pores on the fibers by adjusting the diameter of SiO2 microspheres, and makes the formed microcapsules larger and adsorbs more PEG; controls the proportion of TEOS in an ethanol solution and the dropping rate of NH3·H2O to control the microscopic morphology of the microcapsules; assembles the porous BN fibers loaded with the PEG@SiO2 microencapsulated phase change material into aerogels by directional freeze drying, and the aerogels not only serve as the skeleton of the composite phase change material, greatly improving its anti-leakage performance, but also the aerogel skeleton and the loaded SiO2 shell microcapsules also cooperate to form an efficient heat conduction path, so that the thermal conductivity of the polyethylene glycol phase change material is enhanced; and controls the PEG adsorption amount by adjusting the temperature and time of vacuum melting adsorption, so as to obtain a thermally conductive and anti-leakage polyethylene glycol composite phase change material.

[0038] The thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material prepared by the present invention has a porous BN fiber as a skeleton, and PEG@SiO2 microencapsulated phase change material is loaded on the pores and surface of the fiber. After modification, the polyethylene glycol phase change material is infiltrated into it to form a composite phase change material. Through the combination of the skeleton and the microencapsulated phase change material, not only the leakage-proof performance of the polyethylene glycol phase change material is greatly improved, but also the BN fiber skeleton and the SiO2 shell microcapsules loaded thereon also synergistically form an efficient heat conduction path, thereby enhancing the thermal conductivity of the polyethylene glycol phase change material. The pore size on the BN fiber is regulated to make the loaded microcapsules larger and to adsorb more polyethylene glycol. Compared with the phase change performance of other polyethylene glycol composite phase change materials, the decrease is also smaller. Therefore, the obtained composite phase change material will have broad application prospects in the fields of thermal energy storage, temperature control, cold chain logistics, etc.

[0039] Example 1

[0040] The preparation method of the thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material of the present invention is specifically as follows:

[0041] Firstly, pure SiO2 microspheres with a diameter of 20 μm were used as templates in an amount of 4 wt.%, and mixed with a mixture of H3BO3 and C3H6N6 with a molar ratio of 3:1, deionized water was added, and stirred at 90 ° C for 4 h, then cooled and filtered, and then dried at 60 ° C for 12 h, and then calcined in a nitrogen atmosphere at a calcination temperature of 1100 ° C for 2 h, and finally HF was used to remove SiO2, and porous BN fibers were obtained after washing and drying;

[0042] A 50wt.% PEG6000 solution and a 25wt.% tetraethyl silicate ethanol solution were prepared, and then the two were mixed at 50°C for 30 minutes, and then porous BN fibers were added and ammonia water was added dropwise at a rate of 0.2mol / min. During the addition of ammonia water, the mixture was mixed at 50°C for 20 hours. After filtration, the product was washed with deionized water 3 times, washed with anhydrous ethanol 2 times, and dried at 60°C for 12 hours to obtain a porous BN fiber-loaded PEG@SiO2 microencapsulated phase change material.

[0043] The porous BN fiber loaded with PEG@SiO2 microencapsulated phase change material was added with deionized water, then placed in a mold and frozen at -15°C for 2 hours, and dried at 1Pa for 40 hours to obtain a porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material, which was then placed in a 3.5 mol / L NaOH solution for vacuum impregnation for 3 hours, and dried at 60°C for 12 hours to obtain a hydroxylated-modified porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material;

[0044] Put polyethylene glycol into a beaker, add surfactant hexadecyltrimethylammonium bromide, stir at 70°C for 2 hours, then put the hydroxylated modified porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material obtained in step 3 into polyethylene glycol, perform vacuum-assisted melt infiltration at 75°C, take out after 65 minutes, and obtain a thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material.

[0045] Example 2

[0046] The preparation method of the thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material of the present invention is specifically as follows:

[0047] Firstly, pure SiO2 microspheres with a diameter of 30 μm were used as templates in an amount of 6 wt.%, and mixed with a mixture of H3BO3 and C3H6N6 with a molar ratio of 3:1, and deionized water was added. The mixture was stirred at 90 ° C for 4 h, and then cooled and filtered, and then dried at 60 ° C for 12 h, and then calcined in a nitrogen atmosphere at a calcination temperature of 1100 ° C for 2 h. Finally, HF was used to remove SiO2, and porous BN fibers were obtained after washing and drying.

[0048] A 50wt.% PEG6000 solution and a 30wt.% tetraethyl silicate ethanol solution were prepared, and then the two were mixed at 50°C for 30 minutes, and then porous BN fibers were added and ammonia water was added dropwise at a rate of 0.4mol / min. During the addition of ammonia water, the mixture was mixed at 50°C for 20 hours. After filtration, the product was washed with deionized water 3 times, washed with anhydrous ethanol 2 times, and dried at 60°C for 12 hours to obtain a porous BN fiber-loaded PEG@SiO2 microencapsulated phase change material.

[0049] The porous BN fiber loaded with PEG@SiO2 microencapsulated phase change material was added with deionized water, then placed in a mold and frozen at -25°C for 2.5 hours, and dried at 1Pa for 40 hours to obtain a porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material, which was then placed in a 3.5 mol / L NaOH solution for vacuum impregnation for 3 hours, and dried at 60°C for 12 hours to obtain a hydroxylated-modified porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material;

[0050] Put polyethylene glycol into a beaker, add surfactant hexadecyltrimethylammonium bromide, stir at 70°C for 2 hours, then put the hydroxylated modified porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material obtained in step 3 into polyethylene glycol, perform vacuum-assisted melt infiltration at 80°C, take out after 70 minutes, and obtain a thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material.

[0051] Example 3

[0052] The preparation method of the thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material of the present invention is specifically as follows:

[0053] Firstly, pure SiO2 microspheres with a diameter of 40 μm were used as templates in an amount of 8 wt.%, and mixed with a mixture of H3BO3 and C3H6N6 with a molar ratio of 3:1, and deionized water was added. The mixture was stirred at 90 ° C for 4 h, and then cooled and filtered, and then dried at 60 ° C for 12 h, and then calcined in a nitrogen atmosphere at a calcination temperature of 1100 ° C for 2 h. Finally, HF was used to remove SiO2, and porous BN fibers were obtained after washing and drying.

[0054] A 50wt.% PEG6000 solution and a 35wt.% tetraethyl silicate ethanol solution were prepared, and then the two were mixed at 50°C for 30 minutes, and then porous BN fibers were added and ammonia water was added dropwise at a rate of 0.6mol / min. During the addition of ammonia water, the mixture was mixed at 50°C for 20 hours. After filtration, the product was washed with deionized water 3 times, washed with anhydrous ethanol 2 times, and dried at 60°C for 12 hours to obtain a porous BN fiber-loaded PEG@SiO2 microencapsulated phase change material.

[0055] The porous BN fiber loaded with PEG@SiO2 microencapsulated phase change material was added with deionized water, then placed in a mold and frozen at -35°C for 3 hours, and dried at 2Pa ​​for 50 hours to obtain a porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material, which was then placed in a 3.5 mol / L NaOH solution for vacuum impregnation for 3 hours, and dried at 60°C for 12 hours to obtain a hydroxylated-modified porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material;

[0056] Put polyethylene glycol into a beaker, add surfactant hexadecyltrimethylammonium bromide, stir at 70°C for 2 hours, then put the hydroxylated modified porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material obtained in step 3 into polyethylene glycol, perform vacuum-assisted melt infiltration at 85°C, take out after 75 minutes, and obtain a thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material.

[0057] Example 4

[0058] The preparation method of the thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material of the present invention is specifically as follows:

[0059] Firstly, pure SiO2 microspheres with a diameter of 50 μm were used as templates in an amount of 10 wt.%, and mixed with a mixture of H3BO3 and C3H6N6 with a molar ratio of 3:1, and deionized water was added. The mixture was stirred at 90 ° C for 4 h, and then cooled and filtered, and then dried at 60 ° C for 12 h, and then calcined in a nitrogen atmosphere at a calcination temperature of 1100 ° C for 2 h. Finally, HF was used to remove SiO2, and porous BN fibers were obtained after washing and drying.

[0060] A 50wt.% PEG6000 solution and a 40wt.% tetraethyl silicate ethanol solution were prepared, and then the two were mixed at 50°C for 30 minutes, and then porous BN fibers were added and ammonia water was added dropwise at a rate of 0.8mol / min. During the addition of ammonia water, the mixture was mixed at 50°C for 20 hours. After filtration, the product was washed with deionized water 3 times, washed with anhydrous ethanol 2 times, and dried at 60°C for 12 hours to obtain a porous BN fiber-loaded PEG@SiO2 microencapsulated phase change material.

[0061] The porous BN fiber loaded with PEG@SiO2 microencapsulated phase change material was added with deionized water, then placed in a mold and frozen at -45°C for 3.5 hours, and dried at 1.5Pa for 45 hours to obtain a porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material, which was then placed in a 3.5 mol / L NaOH solution for vacuum impregnation for 3 hours, and dried at 60°C for 12 hours to obtain a hydroxylated-modified porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material;

[0062] Put polyethylene glycol into a beaker, add surfactant hexadecyltrimethylammonium bromide, stir at 70°C for 2 hours, then put the hydroxylated modified porous BN fiber aerogel loaded with PEG@SiO2 microencapsulated phase change material obtained in step 3 into polyethylene glycol, perform vacuum-assisted melt infiltration at 90°C, take out after 80 minutes, and obtain a thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material.

[0063] Table 1 is a comparison of the phase change performance, thermal conductivity and leakage rate of the thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material and the cellulose aerogel composite phase change thermal insulation material and the sealing gasket filled with the phase change material in Examples 1-4.

[0064] Table 1

[0065]

[0066] As can be seen from Table 1, the crystallization enthalpy and melting enthalpy of the thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material in Example 1 are not significantly decreased compared with pure polyethylene glycol. This is not only because the aerogel skeleton adsorbs polyethylene glycol, but also the inner core of the microcapsule is polyethylene glycol, so the polyethylene glycol content is relatively high. Therefore, its phase change performance is better than that of the "cellulose aerogel composite phase change insulation material" and the "sealing pad filled with phase change material". Its leakage rate and thermal conductivity also reach 0.02 mL / min and 40.8 W / K•m, respectively. This is because the aerogel skeleton and the PEG@SiO2 microencapsulated phase change material loaded thereon are blocked when the polyethylene glycol melts, thereby improving its leakage resistance. Moreover, the aerogel not only acts as a skeleton, but also contains BN and SiO2 shells with high thermal conductivity. The two synergistically form an efficient heat conduction path, so its thermal conductivity is also good.

Claims

1. Preparation method of thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material, It is characterized in that Follow the steps below to implement it: Step 1, preparing porous BN fibers; Step 2: Preparation of porous BN fibers loaded with PEG@SiO 2 Microencapsulated phase change materials; Step 3, constructing aerogel and modifying it by hydroxylation; Step 4, vacuum-assisted melt infiltration; In step 1, specifically: using pure SiO 2 The microspheres were used as templates and mixed with H 3 BO 3 and C 3 H 6 N 6 Melamine was mixed, deionized water was added and stirred, then it was naturally cooled and filtered, dried and calcined in a nitrogen atmosphere, and finally HF was used to remove SiO 2 , after washing and drying, porous BN fibers were obtained; In step 2, specifically, a polyethylene glycol solution and a tetraethyl silicate ethanol solution are prepared, and then the two are mixed, the mixed solution is added to the porous BN fiber obtained in step 1, and ammonia water is added dropwise, and after filtration, it is washed with deionized water and anhydrous ethanol respectively and dried to obtain a porous BN fiber loaded with PEG@SiO 2 Microencapsulated phase change materials; In step 3, specifically, the porous BN fiber obtained in step 2 is loaded with PEG@SiO 2 The microencapsulated phase change material was added with deionized water and then placed in a mold for directional freeze drying to obtain a microencapsulated phase change material loaded with PEG@SiO 2 The porous BN fiber aerogel of microencapsulated phase change material was then placed in a NaOH solution for vacuum impregnation and dried to obtain hydroxylated modified loaded PEG@SiO 2 Porous BN fiber aerogels for microencapsulated phase change materials; In step 4, specifically, polyethylene glycol is placed in a beaker, a surfactant is added and stirred, and then the hydroxylated modified loaded PEG@SiO obtained in step 3 is added. 2 The porous BN fiber aerogel of the microencapsulated phase change material is placed in polyethylene glycol, vacuum-assisted melt infiltration is performed, and the thermally conductive enhanced and leak-proof polyethylene glycol composite phase change material is obtained.

2. The method for preparing the thermally conductive and leak-proof polyethylene glycol composite phase change material according to claim 1, It is characterized in that In step 1, pure SiO 2 The diameter of the microspheres is 20 μm to 50 μm, and the dosage is 4 wt.% to 10 wt.%, H 3 BO 3 and C 3 H 6 N 6 The molar ratio is 3:1, the stirring temperature and time are 90℃ and 4h respectively, the drying temperature and time are 60℃ and 12h respectively, the calcination temperature is 1100℃, and the insulation is 2h.

3. The method for preparing the thermally conductive and leak-proof polyethylene glycol composite phase change material according to claim 1, It is characterized in that In the step 2, the polyethylene glycol solution is PEG6000, which is a polyethylene glycol aqueous solution with a mass fraction of 50wt.%, the tetraethyl silicate ethanol solution is a tetraethyl silicate ethanol solution with a mass fraction of 25wt.% to 40wt.%, the mixing temperature is 50°C, the time is 30min, the dropping rate of ammonia water is 0.2mol / min to 0.8mol / min, and the mixing is carried out at 50°C for 20h during the dropping of ammonia water. The product after suction filtration is washed 3 times with deionized water and 2 times with anhydrous ethanol. The drying time and temperature are 12h and 60°C, respectively.

4. The method for preparing the thermally conductive and leak-proof polyethylene glycol composite phase change material according to claim 1, It is characterized in that In step 3, the directional freeze-drying parameters are: freezing at -45°C to -15°C for 2h to 3.5h, drying at 1Pa to 2Pa for 40h to 50h, NaOH solution concentration of 3.5mol / L, immersion for 3h, and drying time and temperature of 12h and 60°C respectively.

5. The method for preparing the thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material according to claim 1, It is characterized in that In step 4, the surfactant is hexadecyltrimethylammonium bromide, the stirring temperature is 70° C., the time is 2 hours, the vacuum oven temperature is 75° C. to 90° C., and the penetration time is 65 min to 80 min.

6. A thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material prepared according to the method for preparing the thermally conductive enhanced leakage-proof polyethylene glycol composite phase change material according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Graphene elastic polymer phase-change composite material and preparation method thereof

    CN109385254A

  • Preparation method of porous boron nitride fibers with high specific surface area

    CN112877810A

  • Heat-conducting composite PEG phase-change material based on aerogel porous skeleton and preparation method and application of heat-conducting composite PEG phase-change material

    CN115785911A

  • Boron nitride-based aerogel reinforced phase change energy storage composite material and preparation method thereof

    CN116731680A

  • Composite phase-change material for phase-change temperature-adjusting fiber and preparation method of composite phase-change material

    CN116751566A

Cited By

  • Anti-leakage high-thermal-conductivity composite phase change material and preparation method thereof

    CN120248837A