A control method for circuit board ICD
Through the three-stage gas treatment and temperature control of the plasma degumming machine, the problem of removing residual glue from via holes in high Tg material sheets is solved, an efficient and uniform glue removal effect is achieved, the problem of inner layer interconnection defects is solved, and The stability and safety of the processing process are guaranteed.
Patent Information
- Application Number
- CN202411106025.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The traditional glue removal process cannot effectively clean the via hole glue residue in high Tg material sheets, resulting in inner interconnection defects. Especially on high-precision circuit boards, it is difficult to completely remove inert components and fiber residues, resulting in connection and separation defects. .
Using a plasma degumming machine, mixed gases of different proportions are introduced through three stages: in the first stage, O2 and N2 perform oxidation reactions, in the second stage, CF4 is introduced to generate fluorine radicals to remove pollutants that are difficult to oxidize, and in the third stage, pure oxygen is used Remove carbonization by-products, combined with temperature control and plasma generator power adjustment, to ensure glue removal efficiency and stability.
It achieves efficient removal of residual glue on the inner layer of the circuit board, improves the glue removal rate and uniformity, effectively solves the problem of inner interconnection defects, and does not damage the hole wall, ensuring the stability and safety of the equipment.
Smart Images

Figure CN118632442B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a circuit board inner layer interconnection defect improvement technology, belongs to the field of printed circuit manufacturing, and particularly relates to a circuit board ICD control method. Background Art
[0002] In recent years, the demand for circuit boards has continued to grow, driving the rapid development of related technologies. For multi-layer circuit boards, the traditional multi-layer board lamination and via hole (through hole) degumming process is no longer effective. In addition, with the reform of PCB (printed circuit board) material technology and the refinement of appearance, as well as the use of new material boards with high Tg (glass transition temperature ≥ 170℃) and low signal loss, these boards have solved the problem of thermal expansion coefficient and have been widely used.
[0003] However, the sheet materials currently used have a high Tg resin system. These resins may contain more cross-linking points or rigid groups in the molecular structure, making the material more stable when heated, but at the same time increasing the content of inert components. Some sheet materials also use carbon fiber or silicon fiber as reinforcement materials. These fibers may break during the drilling process and remain in the hole wall. In addition, the via holes are smaller in size on more delicate circuit boards. The above factors make the original chemical degumming process less effective. The traditional (potassium permanganate, sodium hydroxide) degumming process solution cannot completely penetrate into the small via holes, nor can it effectively clean the residual glue formed by drilling in the current sheet materials. In particular, the inert materials cannot be cleaned. The occurrence of this problem is very likely to cause ICD problems (Inner Connection Defects), that is, connection separation defects caused by residual glue in the inner layer. Such as Figure 2 , Figure 3 As shown in the figure, it can be seen that after being processed by the existing processing method, there is a clear separation between the metal material of the via hole and a layer of connecting wires in the circuit board. Figure 4 It shows that there is 2.67μm of residual glue at the separation point, which is a relatively serious connection separation defect. Summary of the invention
[0004] In view of the above problems, the present invention provides a control method for ICD of a circuit board, which can effectively solve the problem of inner layer interconnection defects of the circuit board and has a high glue removal efficiency.
[0005] In order to achieve the purpose of the present invention, the following scheme is adopted:
[0006] A control method for a circuit board ICD comprises the following steps:
[0007] S100: placing the circuit board into a processing chamber of a plasma debonding machine, and exhausting the air in the processing chamber;
[0008] S200: Start the plasma degumming machine and increase the temperature of the processing chamber to 80℃~100℃;
[0009] S300: introducing a first mixed gas into the processing chamber at a flow rate of 2SLM to 3.25SLM, wherein the first mixed gas includes O2 and N2, and the mixing ratio of O2 to N2 is 3:1 to 5:1, and the time for introducing the first mixed gas lasts for 30 minutes to 70 minutes;
[0010] S400: introducing a second mixed gas into the processing chamber at a flow rate of 2SLM~3.25SLM, the second mixed gas comprising O2, CF4, and N2, wherein O2 accounts for 60%~90%, CF4 accounts for 5%~20%, and N2 accounts for 5%~20%, and the time for introducing the second mixed gas lasts for 45 minutes~90 minutes;
[0011] S500: O2 is introduced into the processing chamber at a flow rate of 2SLM~3.25SLM, and the time for introducing O2 is 10 minutes~15 minutes.
[0012] Further, after S500 is completed, S600 is executed: taking out the circuit board and cooling it.
[0013] Furthermore, in S200, the temperature of the processing chamber is increased to 90°C.
[0014] Further, in S300, the flow rate of the first mixed gas into the processing chamber is 3.25 SLM; in S400, the flow rate of the second mixed gas into the processing chamber is 3.25 SLM; in S500, the flow rate of O2 into the processing chamber is 3.25 SLM.
[0015] Furthermore, the mixing ratio of O2 to N2 in the first mixed gas is 4:1.
[0016] Furthermore, in the second mixed gas, O2 accounts for 80%, CF4 accounts for 10%, and N2 accounts for 10%.
[0017] Furthermore, the first mixed gas is introduced for 50 minutes, and the second mixed gas is introduced for 75 minutes; in S500, O2 is introduced for 10 minutes.
[0018] Furthermore, a plasma degumming machine with a plasma generator rated power ≥ 10000W is used for processing. In S300, the plasma generator power is set to 7000W~8500W; in S400, the plasma generator power is set to 4500W~6000W; in S500, the plasma generator power is set to 3000W~4500W.
[0019] Further, in S300, the power of the plasma generator is set to 8500W; in S400, the power of the plasma generator is set to 6000W; in S500, the power of the plasma generator is set to 4500W.
[0020] The beneficial effects of this technical solution are:
[0021] 1. In the control method of ICD of the circuit board, firstly, through the plasma degumming method, comprehensive degumming can be achieved inside the tiny holes. Secondly, on this basis, the method has three stages of introducing gas for plasma degumming. The types and proportions of gases used in these three stages have the following effects and principles for solving the ICD problem: (1) In the first stage: O2, as a strong oxidant, can react with the residual glue in the inner layer of the via hole during the plasma degumming process to accelerate its decomposition and removal. N2 does not directly participate in the chemical reaction, but can dilute oxygen. and other active components in the plasma, which helps to control the reaction rate and maintain the stability of the plasma, protect the processing chamber and equipment from direct erosion by high temperature and active gases, and extend the service life of the equipment. Controlling the mixing ratio of O2 and N2 can maintain the smooth progress of the reaction while increasing the degumming rate. When O2 and N2 are mixed in a ratio of 3:1~5:1, it is sufficient to achieve a higher degumming rate; (2) In the second stage: O2 and N2 continue to play a role, introducing a small amount of CF4, which decomposes in the plasma to produce fluorine free radicals. Fluorine free radicals have extremely strong reactivity and can remove pollutants that are difficult to be removed by oxygen alone in the first stage, such as certain compounds containing silicon or carbon, and inert additives or fillers. These substances are not sensitive to oxidation reactions and are therefore difficult to be completely removed by O2. In addition, CF4 is introduced in the second stage to avoid the premature introduction of CF4, which causes strong fluorination and oxidation to occur simultaneously, and the fluorine free radicals react with organic matter that has not been completely oxidized, resulting in the inability to remove residual glue well. In addition, although the current circuit board materials increase the inert components in the via holes, some boards also use carbon fiber. Or silicon fiber as reinforcing material, but the proportion of these materials is not large, and excessive use of CF4 will produce some toxic and harmful fluorides, and will also produce corrosive substances, which will damage the processing chamber and equipment. Therefore, when the gas ratio is carried out in the second stage, O2 is still the main gas. Taking these factors into consideration, O2 accounts for 60%~90%, CF4 accounts for 5%~20%, and N2 accounts for 5%~20%, which can ensure a good degumming effect and improve stability; (3) In the third stage: pure oxygen can be used to remove the carbonization byproducts of the plasma reaction to the resin in the previous stage.
[0022] 2. After the temperature of the processing chamber is raised to 80℃~100℃, the gas is plasmatized by a plasma generator to maintain the temperature. A longer processing time is adopted in the first stage to make the surface temperature of the sheet material evenly distributed, avoid local overheating or insufficient temperature, and facilitate oxidation reaction. CF4 is introduced in the second stage. It takes a certain amount of time for the gas mixture of different components and proportions to reach a stable state in the reaction chamber. Therefore, the reaction time required is longer, which is convenient for deep degumming. The third stage is the finishing stage, and the by-products are removed in a shorter time.
[0023] 3. The control method of the circuit board ICD is used to treat the residual glue in the via holes of the multi-layer board. The degumming rate is high, and the glue residue and drilling contamination in the hole can be effectively removed. When degumming multiple circuit boards at the same time, the uniformity of the degumming rate is good, which can solve the problem of inner layer interconnection defects of the circuit board, and will not cause unnecessary damage to the hole wall after treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The brief steps of the circuit board ICD control method are shown.
[0025] Figure 2 Background technology schematic diagram Figure 1 .
[0026] Figure 3 Background technology schematic diagram Figure 2 .
[0027] Figure 4 Background technology schematic diagram Figure 3 .
[0028] Figure 5 A circuit board degumming rate test result table is shown.
[0029] Figure 6 The table shows the test results of negative etching of residual glue in the hole by plasma gas. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solutions and advantages of the present application clearer, the implementation methods of the present application are described in detail below, but the embodiments described in this application are only part of the embodiments of the present application, rather than all the embodiments.
[0031] In such Figure 1 Based on the brief steps of the circuit board ICD control method shown, it is implemented in detail according to the following steps:
[0032] S100: placing the circuit board into a processing chamber of a plasma debonding machine, and exhausting the air in the processing chamber;
[0033] S200: starting the plasma degumming machine, raising the temperature of the processing chamber to 80° C. to 100° C., preferably 90° C. Specifically, this step realizes heating through an electric heating plate inside the plasma degumming machine;
[0034] S300: introducing a first mixed gas into the processing chamber at a flow rate of 2SLM to 3.25SLM, preferably 3.25SLM, wherein the first mixed gas includes O2 and N2, and the mixing ratio of O2 to N2 is 3:1 to 5:1, preferably 4:1, and the time for introducing the first mixed gas lasts for 30 minutes to 70 minutes, preferably 50 minutes;
[0035] S400: introducing a second mixed gas into the processing chamber at a flow rate of 2SLM~3.25SLM, preferably 3.25SLM, the second mixed gas comprising O2, CF4, and N2, wherein O2 accounts for 60%~90%, CF4 accounts for 5%~20%, and N2 accounts for 5%~20%, preferably O2 accounts for 80%, CF4 accounts for 10%, and N2 accounts for 10%, and the time for introducing the second mixed gas lasts for 45 minutes to 90 minutes, preferably 75 minutes;
[0036] S500: introducing O2 into the processing chamber at a flow rate of 2SLM to 3.25SLM, preferably 3.25SLM, and the time for introducing O2 lasts for 10 minutes to 15 minutes, preferably 10 minutes;
[0037] S600: Take out the circuit board and cool it to room temperature, specifically, it needs to be cooled to below 30° C. at least.
[0038] The SLM mentioned above is the abbreviation of Standard Liter per Minute, which is used to indicate the volume of fluid flowing through a certain place per unit time under standard conditions (0°C, 1 standard atmospheric pressure).
[0039] Preferably, a plasma degumming machine with a plasma generator rated power ≥ 10000W is used for processing, and: in S300, the plasma generator power is set to 7000W~8500W, preferably 8500W. High power can produce high-density plasma and strong physical bombardment effect, which can more effectively bombard the residual glue in the hole wall, causing it to begin to decompose and loosen; in S400, the plasma generator power is set to 4500W~6000W, preferably 6000W. Medium power can maintain a certain plasma density and active particle energy, and avoid unnecessary damage to the circuit board caused by excessive energy; in S500, the plasma generator power is set to 3000W~4500W, preferably 4500W. This stage is mainly to remove carbonization by-products, so low power is maintained to make the plasma density and active particle energy moderate.
[0040] In order to illustrate the ICD control effect that can be achieved by the above method, the following tests were performed:
[0041] 1. Glue removal rate test: Figure 5 In the figure, "circuit board number on carrier" indicates a specified circuit board on a circuit board carrier in the processing chamber. There are 9 circuit boards placed on each circuit board carrier. "Circuit board carrier position in the processing chamber" indicates the circuit board carriers at the left, middle and right positions in the processing chamber respectively. Since plasma is more likely to bombard the circuit board that is perpendicular to the airflow direction in the processing chamber, the degumming process is sometimes not uniform. Therefore, it is necessary to test the degumming rate of the circuit boards at various positions.
[0042] From the degumming rates of 27 circuit boards, it can be seen that the minimum value is 169.70 mg / cm 2 , the maximum value is 279.40mg / cm 2 , the average value is 212.28 mg / cm 2 , the degumming rate is relatively high.
[0043] For the uniformity of the degumming rate, if the formula [1-(maximum value-minimum value) / (2*average value)]*100% is used for calculation, we can get [1-(279.40-169.70) / (2*212.28)]*100%=74.16%, which is a high uniformity.
[0044] 2. Negative etching test of residual glue in the hole by plasma gas: First of all, "negative etching" means that in the plasma treatment process, in addition to removing the residual glue in the hole, it may also cause unnecessary erosion or damage to the hole wall or substrate material to a certain extent.
[0045] In this test, the metal connection positions and negative etch distances of the 27 circuit boards in the previous debonding rate test were observed. First, there was no disconnection at the metal connection positions of all the circuit boards, and the negative etch distances were: (1) The negative etch distances of the first to ninth circuit boards on the left circuit board carrier were: 0.36mil, 0.33mil, 0.36mil, 0.33mil, 0.36mil, 0.40mil, 0.36mil, 0.43mil, 0.36mil; (2) The negative etch distances of the first to ninth circuit boards on the middle circuit board carrier were: 0.36mil, 0.33mil, 0.36mil, 0.33mil, 0.36mil, 0.40 ... The negative etching distances of the first to ninth circuit boards are: 0.40mil, 0.33mil, 0.36mil, 0.33mil, 0.47mil, 0.36mil, 0.36mil, 0.43mil, 0.36mil; (3) The negative etching distances of the first to ninth circuit boards on the right circuit board carrier are: 0.40mil, 0.40mil, 0.33mil, 0.43mil, 0.36mil, 0.40mil, 0.36mil, 0.40mil, 0.33mil. Figure 6 This is a negative etching test summary table. The first row and columns in the table represent the circuit board carrier position, actual negative etching distance, required negative etching distance, and test results. The distance unit is mil, which is commonly used in the circuit board field and represents one thousandth of an inch. 1mil=0.0254 mm.
[0046] It can be seen from the negative etching test results that all the test circuit boards have solved the ICD problem and achieved normal internal connection. The negative etching distance range of the circuit boards on the left and right is controlled at 0.33mil~0.43mil, and the negative etching distance of the circuit board in the middle can reach 0.47mil. However, all negative etching distances are between 0.1mil~0.6mil required by the process. Therefore, it can be seen from the last column that all meet the process requirements.
[0047] The above are only some of the embodiments listed in this application and are not intended to limit this application.
Claims
1. A control method for a circuit board ICD, characterized in that: The following steps are involved: S100: placing the circuit board into a processing chamber of a plasma debonding machine with a plasma generator rated power ≥ 10000W, and exhausting the air in the processing chamber; S200: Start the plasma degumming machine and increase the temperature of the processing chamber to 90°C; S300: introducing a first mixed gas into the processing chamber at a flow rate of 3.25 SLM, the first mixed gas including O2 and N2, the mixing ratio of O2 to N2 being 4:1, the time for introducing the first mixed gas lasts for 50 minutes, and the power of the plasma generator is set to 8500 W; S400: introducing a second mixed gas into the processing chamber at a flow rate of 3.25 SLM, the second mixed gas comprising O2, CF4, and N2, wherein O2 accounts for 80%, CF4 accounts for 10%, and N2 accounts for 10%. The second mixed gas is introduced for 75 minutes, and the power of the plasma generator is set to 6000 W; S500: O2 is introduced into the processing chamber at a flow rate of 3.25 SLM for 10 minutes, and the power of the plasma generator is set to 4500 W; S600: Remove the circuit board and allow it to cool.
Citation Information
Patent Citations
Method for improving copper breaking in hole of PTFER-material-made PCB board
CN107072075A
Manufacturing method of circuit board structure
CN113473708A
PCB glue removing device and method
CN113518510A
Method for manufacturing PCB (Printed Circuit Board) via hole with high thickness-diameter ratio
CN117042300A
Circuit board hole metallization method and circuit board
CN117545194A