Method for reinforcing loess through combination of rubber particles and EICP

By using rubber particles and enzyme-induced calcium carbonate precipitation technology in loess, the problem of loess being susceptible to shear damage is solved, the shear strength and reinforcement effect are improved, and a cost-effective soil improvement and environmentally friendly solution is achieved.

CN118745728APending Publication Date: 2024-10-08THE SEVENTH ENGINEERING CO LTD OF CCCC FIRST HIGHWAY ENGINEERING CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410730514.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Untreated loess is susceptible to shear damage, leading to frequent geological disasters. Existing improvement methods are costly and have a large impact on the environment, making it difficult to be widely used in terms of economic benefits.

Method used

Rubber particles combined with enzyme-induced calcium carbonate precipitation (EICP) technology is used to add rubber particles, urease solution and cementing fluid to the loess to promote calcium carbonate precipitation and improve the shear strength and reinforcement effect of the loess.

Benefits of technology

It improves the overall reinforcement effect of loess, enhances shear strength, reduces the environmental impact of waste tires, and improves soil stability and environmental friendliness through uniformly distributed calcium carbonate precipitation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745728A_ABST
    Figure CN118745728A_ABST
Patent Text Reader

Abstract

The invention discloses a method for reinforcing loess through combination of rubber particles and EICP, and relates to the technical field of building materials.The method for reinforcing loess through combination of rubber particles and EICP comprises the following steps that S1, the address of yellow soil is selected, and the selected yellow soil is dried and smashed; s2, adding rubber particles into the crushed yellow soil, uniformly mixing, then adding a urease solution and a cementing liquid, and uniformly mixing to obtain pre-improved loess; and S3, the pre-improved loess is backfilled in a layered mode, tamped and covered with a thin film, and maintenance is conducted for 1-3 days. The urease solution comprises urease and water, and the urease is selected from one of beans; the cementing liquid comprises urea, calcium chloride and water. According to the method for reinforcing the loess through the combination of the rubber particles and the EICP, more adsorption sites are provided for calcium carbonate precipitation, the calcium carbonate precipitation generated in the loess is more uniform, and therefore the overall reinforcing effect of the loess is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of building material technology, and in particular to a method for reinforcing loess with rubber particles and EICP. Background Art

[0002] China's loess is widely distributed and thick, accounting for 6.6% of China's land area. Loess has a loose structure and is easily damaged by shear under the action of water and external loads. Therefore, untreated loess is very prone to geological disasters such as subsidence, landslides and collapses. It cannot be directly used in engineering practice and needs to improve the mechanical properties of loess. At present, the main improvement method is to add high-strength materials to the soil to improve the mechanical properties of loess, but high-strength materials are often expensive. In actual engineering practice, it is generally necessary to improve loess on a large scale, which is not conducive to economic benefits. Therefore, it is necessary to study a green and environmentally friendly improvement method with excellent economic benefits.

[0003] The Chinese invention patent with publication number CN111749227A discloses a method for inducing carbonate precipitation by combining microorganisms with rubber materials, comprising the following steps: (1) uniformly dispersing rubber particles and adding them to sand to obtain sand with rubber particles added; wherein the volume of the rubber particles accounts for 1-30% of the volume of the sand with rubber particles added; (2) alternately injecting bacterial solution and bacterial nutrient solution into the sand with rubber particles added.

[0004] Enzyme-induced calcium carbonate precipitation (EICP) is a green and environmentally friendly soil reinforcement technology that can directly use highly active urease extracted from plants as a stable urease source and induce calcium carbonate precipitation, eliminating the cumbersome microbial cultivation process in MICP (microbial induced calcium carbonate deposition) technology and avoiding the problem of secondary pollution by by-products. Compared with urease secreted by microorganisms, plant urease is nano-sized, has good water solubility, is free, and is degradable. Therefore, EICP technology is more suitable for reinforcing fine-grained soil and can further reduce the impact on the environment.

[0005] In addition, when bacterial solution and bacterial nutrient solution are alternately injected into sandy soil added with rubber particles, the bacterial nutrient solution has been decomposed and utilized by urease secreted by bacteria before completing its migration, so the soil skeleton is filled unevenly, resulting in a deviation in the overall effect of strengthening the soil. Summary of the invention

[0006] In order to improve the overall effect of loess reinforcement, the present application provides a method for reinforcing loess using rubber particles combined with EICP.

[0007] The present application provides a method for strengthening loess with rubber particles and EICP, which adopts the following technical solution: A method for reinforcing loess by combining rubber particles with EICP comprises the following steps: S1: Selecting the loess site, drying and crushing the selected loess; S2: adding rubber particles to the crushed loess, mixing evenly, and then adding urease solution and cementing liquid, mixing evenly to obtain pre-modified loess; S3: Backfill and compact the pre-improved loess in layers, cover with film, and cure for 1 to 3 days; The rubber particles account for 5-15% of the total volume of the rubber particles and loess; the total amount of urease solution and cementing liquid is 150-300L / m 3 ; The urease solution comprises urease and water, wherein the urease is derived from a kind of beans; The binder solution includes urea, calcium chloride and water.

[0008] By using EICP technology to further reinforce loess, on the one hand, it makes up for the weakening of the original soil sample skeleton bearing capacity when rubber particles replace soil particles; on the other hand, the use of legume urease, which is smaller in size, has a better effect in fine-grained soil, and the distribution of calcium carbonate precipitation is more uniform. This technology uses urease to decompose urea to generate ammonium ions and carbonate ions. The carbonate ions combine with calcium ions in the solution to generate calcium carbonate crystals. Calcium carbonate can fill the internal pores of loess, increase the strength of the loess skeleton, and thus improve the shear strength of loess. By evenly doping rubber particles, binder and urease solution in loess, the distribution of calcium carbonate precipitation is more uniform, thereby improving the overall effect of loess reinforcement.

[0009] Preferably, the particle size of the rubber particles does not exceed 3 mm.

[0010] Preferably, the method for preparing the urease solution comprises the following steps: Mix water and phosphate, adjust the pH value to 7.4-7.8, and then mix with urease to obtain a urease solution; The phosphate is a mixture of disodium hydrogen phosphate and sodium dihydrogen phosphate.

[0011] Preferably, the mass concentration of urease in the urease solution is 100-400 g / L.

[0012] Preferably, in step S2, the rubber particles are soaked in alkaline solution for 24 to 26 hours before use, and then solid-liquid separation, washed, dried, and then mixed into the pulverized yellow soil.

[0013] Preferably, in step S2, the rubber particles are modified rubber particles, and the preparation method of the modified rubber particles comprises the following steps, measured by weight: Ⅰ) taking 40 to 60 parts by weight of γ-glycidyloxypropyltrimethoxysilane solution and adjusting the pH value to 7.6 to 8.0 with aqueous ammonia to obtain a mixed solution A; II) 1 to 3 parts by weight of urea, 1 to 3 parts by weight of calcium chloride, 0.5 to 1.5 parts by weight of bentonite, 1 to 2 parts by weight of magnesium silicate and 30 to 50 parts by weight of water are mixed uniformly to obtain a mixed solution B; III) Mix the mixed solution A and the mixed solution B evenly, then add rubber particles accounting for 0.25 to 0.35 of the total volume of the mixed solution A and B, mix for 20 to 40 minutes, separate the solid and liquid, and dry the precipitate to obtain modified rubber particles.

[0014] Preferably, in step III), the precipitate is dried by natural air drying.

[0015] Preferably, the rubber particles are rinsed with clean water until the aqueous solution is neutral after rinsing.

[0016] Preferably, the alkali solution is a sodium hydroxide solution with a mass fraction of 1%.

[0017] Since the bonding force between rubber particles and loess particles is poor, the roughness of the rubber particle surface can be enhanced by soaking in alkaline solution, which not only enhances the bonding force between rubber particles and loess particles, but also improves the unconfined compressive strength of the loess particles stabilized by rubber particles. And by introducing a certain amount of urea, calcium chloride, bentonite, and magnesium silicate into rubber particles, the generated calcium carbonate precipitation can further connect the rubber particles with the sand, and can enhance the wear resistance of the rubber particles, further improving the soil reinforcement effect.

[0018] Preferably, the total molar concentration of calcium chloride and urea in the binder is 0.5 to 2 mol / L.

[0019] Preferably, the method for preparing the cementing liquid comprises the following steps: Calcium chloride and urea are added to water in sequence and mixed evenly, and then mixed evenly with a certain amount of polyacrylamide to obtain a binder; the mass concentration of the polyacrylamide in the binder is 0.2-0.5 g / L.

[0020] Preferably, calcium chloride and urea are added to water and mixed evenly, an auxiliary agent is added and mixed evenly, and then mixed evenly with polyacrylamide to obtain a binder; the mass concentration of the auxiliary agent in the binder is 0.1-0.3 g / L, and the auxiliary agent is at least one of humic acid and thiourea.

[0021] Adding polyacrylamide to the binder increases the cohesive force between sand particles, allowing the sand particles to aggregate into clusters, making it easier to capture calcium carbonate crystals, increasing the yield of calcium carbonate precipitation, and improving the curing effect. The auxiliary agent can inhibit the activity of urease in the initial stage of addition, reduce the hydrolysis rate of urea, so that the urea and calcium chloride in the binder can be evenly distributed and migrated in the loess, making the distribution of calcium carbonate precipitation more uniform, thereby improving the overall effect of loess reinforcement.

[0022] Preferably, the urea is modified urea, and the preparation method of the modified urea comprises the following steps, measured by weight: 1800-2000 parts by weight of urea are placed in a coating machine and heated to 75-85°C. Then, 10-12 parts by weight of 2,6-xylyl isocyanate, 2-3 parts by weight of paraffin, 4-5 parts by weight of modified attapulgite and 4-5 parts by weight of calcium oxide are added and rotated for 3-5 minutes. Then, 10-12 parts by weight of polycaprolactone diol are added and mixed evenly. After reacting at 60-70°C for 2-4 hours, the mixture is dried to obtain modified urea.

[0023] Using a single layer of polyurethane to coat urea can slow down the release rate of urea in a short period of time, thereby reducing the decomposition rate of urease, so that the urea in the binder has enough time to be evenly distributed and migrated in the loess, thereby making the calcium carbonate precipitation more evenly distributed and improving the overall effect of loess reinforcement.

[0024] Preferably, the preparation method of the modified attapulgite comprises the following steps: 1. Calcine the attapulgite at 200-500°C for 1.5-2.5h, cool it down, take it out, and crush it to obtain powdered attapulgite; 2. Place the powdered attapulgite in a sodium hydroxide solution, soak for 10 to 12 minutes, separate the solid and liquid, and wash to obtain pre-modified attapulgite; 3) uniformly mixing the pre-modified attapulgite with the 3-aminopropyltrimethoxysilane solution, and then uniformly mixing with the modifier, soaking, solid-liquid separation, and drying to obtain modified attapulgite; The modifier is at least one of polyvinyl alcohol and polymethyl acrylate.

[0025] By modifying the attapulgite, the viscosity of the attapulgite is enhanced, and the strength of the polyurethane coated urea is improved, solving the problem of the fragility and disintegration of the modified urea. In addition, the modified attapulgite has a significantly increased specific surface area and average pore volume, which enhances the slow-release performance of urea.

[0026] Preferably, the urea is gelatinized starch urea.

[0027] In summary, the present application includes at least one of the following beneficial technical effects: 1. The method of reinforcing loess by using rubber particles in combination with EICP of the present application adopts legume urease and uniformly mixes rubber particles, urease solution, binder and loess, which not only provides adsorption sites for calcium carbonate precipitation, but also makes the calcium carbonate precipitation generated in the loess more uniform, thereby improving the overall reinforcement effect of the loess.

[0028] 2. This application adds polyacrylamide and auxiliary agents to the binder. On the one hand, the cohesion between sand particles is increased, so that the sand particles aggregate into agglomerates, thereby making it easier to capture calcium carbonate crystals, increase the yield of calcium carbonate precipitation, and improve the curing effect. On the other hand, the activity of urease is inhibited, and the hydrolysis and release rate of urea in the early stage is reduced, so that the urea and calcium chloride in the binder can be evenly distributed and migrated in the loess, making the distribution of calcium carbonate precipitation more uniform, thereby improving the overall effect of loess reinforcement.

[0029] 3. The present application adopts rubber particles and plant urease, wherein the rubber particles are light, high-strength, good in deformability and low in cost, which can not only improve the shear strength of solidified loess, but also reduce the pressure on the environment caused by the surge in waste tires; plant urease is small in size, has good water solubility, is in a free state, and is degradable, which can further reduce the impact on the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is the particle gradation curve of loess used in the embodiment; Figure 2 This is a schematic diagram of a sample of loess reinforced with rubber particles and EICP in Example 1; Figure 3 The shear strength relationship curves of the samples of comparative examples 1 to 25 when the vertical pressure is 100 kPa; Figure 4 The relationship curves of urease concentration and sample shear strength of samples of comparative examples 26 to 41 at different cementing solution concentrations; Figure 5 It is a shear stress-shear displacement relationship curve diagram of the samples of comparative example 1 and comparative examples 10 to 14 at a vertical pressure of 50 kPa; Figure 6 It is a shear stress-shear displacement relationship curve diagram of the samples of comparative example 1 and comparative examples 10 to 14 at a vertical pressure of 100 kPa; Figure 7 The cohesion curves of the samples of comparative examples 1 to 6, 10 to 14, and 18 to 22 at different rubber dosages and different rubber particle sizes; Figure 8 It is a curve diagram of the internal friction angle under different rubber content and different rubber particle size of the samples of comparative examples 1 to 6, 10 to 14, and 18 to 22; Fig. 9 The curves of shear strength growth rate versus rubber content of the samples of Examples 1 to 15 at a vertical pressure of 50 kPa; Fig.10 The graphs are the variation curves of the shear strength growth rate of the samples of Examples 1 to 15 with the rubber content at a vertical pressure of 100 kPa; Fig.11 The graphs are the variation curves of the shear strength growth rate of the samples of Examples 1 to 15 with the rubber content at a vertical pressure of 200 kPa; Fig.12 The graphs are the variation curves of the shear strength growth rate of the samples of Examples 1 to 15 with the rubber content at a vertical pressure of 300 kPa; Fig.13 It is a cohesion curve diagram of the samples of comparative example 1 and examples 1 to 15 at different rubber content and different rubber particle sizes; Fig.14 It is a curve diagram of the internal friction angle at different rubber content and different rubber particle sizes of the samples of Comparative Example 1 and Examples 1 to 15; Figure symbols: 1, loess particles; 2, calcium carbonate precipitation. DETAILED DESCRIPTION

[0031] The present application is further described in detail below in conjunction with embodiments and drawings.

[0032] In the following embodiments: Rubber particles are obtained by crushing and screening waste tires. The density of rubber particles is about 1.03g / cm 3 .

[0033] Urease comes from sword beans, has an activity of 1U / mg, and can be stored at a temperature of 2-8°C.

[0034] Preferably, in the embodiment, the adhesive liquid is prepared and used immediately.

[0035] The loess is from the excavation site 10 meters below the foundation pit of a project in Chang'an District, Xi'an City. The soil sample is yellow-brown in color. Its basic physical properties were measured and the results are shown in Table 1.

[0036] Table 1 Physical parameters of loess Example 1 This embodiment provides a method for reinforcing loess by combining rubber particles with EICP, comprising the following steps: S1: The selected loess is excavated to a depth of about 1 m, and then the excavated loess is dried in the sun. After drying, the loess is crushed by a crusher until it completely passes through a 2 mm sieve to obtain crushed loess; S2: adding rubber particles to the crushed loess, mixing evenly, then adding urease solution and cementing liquid, mixing evenly, to obtain pre-modified loess; S3: Backfill the pre-improved loess in layers, compact it in layers, and finally cover it with plastic film and cure it for 2 days; The rubber particles are mixed evenly with the loess by adding them for many times, and the urease solution and the binder are sprayed for many times in sequence with the mixture of the loess and the rubber particles to mix evenly.

[0037] In step S3, the layered compaction coefficient is about 94-96%.

[0038] The particle size of rubber particles is 0-1 mm, and the rubber particles account for 5% of the total volume of rubber particles and loess; the dosage of urease solution is 100 L / m 3 The dosage of cementing liquid is 100L / m 3 .

[0039] The preparation method of the urease solution of this embodiment comprises the following steps: Disodium hydrogen phosphate and sodium dihydrogen phosphate are added to water at a molar concentration of 0.2 mol / L (phosphate concentration), the pH value is adjusted to 7.4 with 10% ammonia water, and then mixed with urease to obtain a urease solution; The mass concentration of urease in the urease solution is 200 g / L.

[0040] The preparation method of the cementing liquid in this embodiment comprises the following steps: Calcium chloride and urea are added into water, stirred and mixed evenly, and the pH value is adjusted to 7.4 with citric acid having a mass concentration of 20%, to obtain a cementing liquid; Among them, the molar concentration of calcium chloride in the binder is 0.5 mol / L, and the molar concentration of urea is 0.5 mol / L.

[0041] Example 2 The difference between this embodiment and embodiment 1 is that the rubber particles account for 7% of the total volume of the rubber particles and the loess.

[0042] The rest is the same as in Example 1.

[0043] Example 3 The difference between this embodiment and embodiment 2 is that the rubber particles account for 10% of the total volume of the rubber particles and the loess.

[0044] The rest is the same as in Example 2.

[0045] Example 4 The difference between this embodiment and embodiment 1 is that the rubber particles account for 13% of the total volume of the rubber particles and the loess.

[0046] The rest is the same as in Example 1.

[0047] Example 5 The difference between this embodiment and embodiment 4 is that the rubber particles account for 15% of the total volume of the rubber particles and the loess.

[0048] The rest is the same as Example 4.

[0049] Example 6 The difference between this embodiment and embodiment 1 is that the particle size of the rubber particles is 1 to 2 mm.

[0050] The rest is the same as in Example 1.

[0051] Example 7 The difference between this embodiment and embodiment 6 is that the rubber particles account for 7% of the total volume of the rubber particles and the loess.

[0052] The rest is the same as Example 6.

[0053] Example 8 The difference between this embodiment and embodiment 7 is that the rubber particles account for 10% of the total volume of the rubber particles and the loess.

[0054] The rest is the same as Example 7.

[0055] Example 9 The difference between this embodiment and embodiment 8 is that the rubber particles account for 13% of the total volume of the rubber particles and loess.

[0056] The rest is the same as Example 8.

[0057] Example 10 The difference between this embodiment and embodiment 9 is that the rubber particles account for 15% of the total volume of the rubber particles and the loess.

[0058] The rest is the same as Example 9.

[0059] Embodiment 11 The difference between this embodiment and embodiment 1 is that the particle size of the rubber particles is 2 to 3 mm.

[0060] The rest is the same as in Example 1.

[0061] Example 12 The difference between this embodiment and embodiment 11 is that the rubber particles account for 7% of the total volume of the rubber particles and loess.

[0062] The rest is the same as Example 11.

[0063] Example 13 The difference between this embodiment and embodiment 1 is that the rubber particles account for 10% of the total volume of the rubber particles and the loess.

[0064] The rest is the same as in Example 1.

[0065] Embodiment 14 The difference between this embodiment and embodiment 13 is that the rubber particles account for 13% of the total volume of the rubber particles and loess.

[0066] The rest is the same as Example 13.

[0067] Embodiment 15 The difference between this embodiment and embodiment 14 is that the rubber particles account for 15% of the total volume of the rubber particles and loess.

[0068] The rest is the same as Example 14.

[0069] Example 16 The difference between this embodiment and embodiment 8 is that the dosage of urease solution is 75 L / m 3 The dosage of cementing fluid is 75L / m 3 .

[0070] The rest is the same as Example 8.

[0071] Embodiment 17 The difference between this embodiment and embodiment 16 is that the dosage of urease solution is 150 L / m 3 The amount of cementing liquid is 150L / m 3 .

[0072] The rest is the same as Example 16.

[0073] Embodiment 18 The difference between this embodiment and embodiment 16 is that in step S2, before use, the rubber particles are immersed in a sodium hydroxide solution with a mass fraction of 1%, stirred for 5 minutes, soaked for 24 hours, filtered, and then rinsed with clean water until the aqueous solution is neutral after rinsing, dried in a drying oven at 70°C for 6 hours, and then mixed into the crushed loess.

[0074] The rest is the same as Example 16.

[0075] Embodiment 19 The difference between this embodiment and embodiment 18 is that: in step S2, before use, the rubber particles are immersed in a sodium hydroxide solution with a mass fraction of 1%, stirred for 5 minutes, soaked for 26 hours, filtered, and then rinsed with clean water until the aqueous solution is neutral after rinsing, dried in a drying oven at 80°C for 4 hours, and then mixed into the crushed loess.

[0076] The mass ratio of the sodium hydroxide solution to the rubber particles is 4:1.

[0077] The rest is the same as Example 18.

[0078] Embodiment 20 The difference between this embodiment and embodiment 19 is that: The preparation method of the cementing liquid in this embodiment comprises the following steps: Calcium chloride and urea are added into water, stirred and mixed evenly, polyacrylamide is added, stirred and mixed evenly, and the pH value is adjusted to 7.4 with citric acid having a mass concentration of 20%, to obtain a cementing liquid; Among them, the molar concentration of calcium chloride in the cementing liquid is 0.5 mol / L, the molar concentration of urea is 0.5 mol / L, and the mass concentration of polyacrylamide in the cementing liquid is 0.2 g / L.

[0079] In step S2, the rubber particles are modified rubber particles, and the preparation method of the modified rubber particles comprises the following steps: Ⅰ) taking 40 kg of 1% by mass γ-glycidyloxypropyltrimethoxysilane solution, adjusting the pH value to 7.6 with 10% by mass ammonia water, and obtaining a mixed solution A; II) 1 kg of urea, 1 kg of calcium chloride, 0.5 kg of bentonite, 1 kg of magnesium silicate and 30 kg of water were mixed to obtain a mixed solution B; III) Mix the mixed solution A and the mixed solution B evenly, then add rubber particles accounting for 0.25 of the total volume of the mixed solution, stir and mix for 20 minutes, filter, and naturally dry the precipitate to obtain modified rubber particles.

[0080] The rest is the same as Example 19.

[0081] Embodiment 21 The difference between this embodiment and Embodiment 20 is that the mass concentration of polyacrylamide in the binder is 0.5 g / L.

[0082] In step S2, the rubber particles are modified rubber particles, and the preparation method of the modified rubber particles comprises the following steps: Ⅰ) taking 60 kg of 1% by mass γ-glycidyloxypropyltrimethoxysilane solution, adjusting the pH value to 8.0 with 10% by mass ammonia water, and obtaining a mixed solution A; II) 3 kg of urea, 3 kg of calcium chloride, 1.5 kg of bentonite, 2 kg of magnesium silicate and 50 kg of water were mixed to obtain a mixed solution B; III) Mix the mixed solution A and the mixed solution B evenly, then add rubber particles accounting for 0.35 of the total mixed solution volume, stir and mix for 40 minutes, filter, and naturally dry the precipitate to obtain modified rubber particles.

[0083] The rest is the same as Example 20.

[0084] Embodiment 22 The difference between this embodiment and embodiment 21 is that: The preparation method of the cementing liquid in this embodiment comprises the following steps: Calcium chloride and urea are added into water, stirred and mixed evenly, humic acid is added first, stirred and mixed evenly, polyacrylamide is added, stirred and mixed evenly, and citric acid with a mass concentration of 20% is used to adjust the pH value to 7.4 to obtain a cementing liquid; Among them, the molar concentration of calcium chloride in the cementing fluid is 0.5 mol / L, the molar concentration of urea is 0.5 mol / L, the mass concentration of humic acid in the cementing fluid is 0.1 g / L, and the mass concentration of polyacrylamide in the cementing fluid is 0.3 g / L.

[0085] The rest is the same as Example 21.

[0086] Embodiment 23 The difference between this embodiment and embodiment 22 is that: The preparation method of the urease solution of this embodiment comprises the following steps: Disodium hydrogen phosphate and sodium dihydrogen phosphate are added to water at a molar concentration of 0.2 mol / L (phosphate concentration), the pH value is adjusted to 7.8 with 10% ammonia water, and then mixed with urease to obtain a urease solution; The mass concentration of urease in the urease solution is 200 g / L.

[0087] The preparation method of the cementing liquid in this embodiment comprises the following steps: Calcium chloride and urea are added into water, stirred and mixed evenly, humic acid and thiourea are added first, stirred and mixed evenly, polyacrylamide is added, stirred and mixed evenly, and pH value is adjusted to 7.4 with citric acid having a mass concentration of 20%, to obtain a cementing liquid; Among them, the molar concentration of calcium chloride in the cementing fluid is 0.5 mol / L, the molar concentration of urea is 0.5 mol / L, the mass concentration of humic acid in the cementing fluid is 0.1 g / L, the mass concentration of thiourea in the cementing fluid is 0.2 g / L, and the mass concentration of polyacrylamide in the cementing fluid is 0.4 g / L.

[0088] Urea is gelatinized starch urea.

[0089] The rest is the same as Example 22.

[0090] Embodiment 24 The difference between this embodiment and Embodiment 23 is that the urea in the binder fluid of this embodiment is modified urea.

[0091] The preparation method of modified urea in this embodiment comprises the following steps: 1800g of urea was placed in a coating machine and heated to 75°C. Then, 10g of 2,6-xylyl isocyanate, 2g of paraffin, 4g of modified attapulgite and 4g of calcium oxide were added and rotated for 3min. Then, 10g of polycaprolactone diol was added and mixed evenly. After reacting at 60°C for 4h, the mixture was dried at 60°C to obtain modified urea.

[0092] The preparation method of modified attapulgite in this embodiment comprises the following steps: 1. Put 12g of attapulgite into a calcining furnace, calcine at 200℃ for 2.5h, cool to room temperature, take out and grind to obtain powdered attapulgite; 2. Place the powdered attapulgite in 500 mL of a 0.5 mol / L sodium hydroxide solution, stir for 3 min, soak for 10 min, filter, and wash the precipitate with water until it is neutral to obtain pre-modified attapulgite; 3. Mix the pre-modified attapulgite with 500 mL of 2% 3-aminopropyltrimethoxysilane solution, then add it into 200 mL of 10% polyvinyl alcohol aqueous solution, stir and mix evenly, soak for 40 minutes, filter, place the precipitate in a drying oven, and dry it at 40°C for 4 hours to obtain modified attapulgite.

[0093] The rest is the same as Example 23.

[0094] Embodiment 25 The difference between this embodiment and Embodiment 24 is that the urea in the binder fluid of this embodiment is modified urea.

[0095] The preparation method of modified urea in this embodiment comprises the following steps: 2000g of urea was placed in a coating machine and heated to 85°C. Then, 12g of 2,6-xylyl isocyanate, 3g of paraffin, 5g of modified attapulgite and 5g of calcium oxide were added and rotated for 5min. Then, 12g of polycaprolactone diol was added and mixed evenly. After reacting at 70°C for 2h, the mixture was dried at 70°C to obtain modified urea.

[0096] The preparation method of modified attapulgite in this embodiment comprises the following steps: 1. Put 14g of attapulgite into a calcining furnace, calcine at 500℃ for 1.5h, cool to room temperature, take out and grind to obtain powdered attapulgite; 2. Place the powdered attapulgite in 600 mL of a 0.5 mol / L sodium hydroxide solution, stir for 3 min, soak for 12 min, filter, and wash the precipitate with water until it is neutral to obtain pre-modified attapulgite; 3. Immerse the pre-modified attapulgite in 600 mL of 2% 3-aminopropyltrimethoxysilane solution and mix evenly, then add 200 mL of 10% polyvinyl alcohol aqueous solution and 5 g of polymethyl acrylate, stir and mix evenly, soak for 50 minutes, filter, place the precipitate in a drying oven, and dry it at 50°C for 3 hours to obtain modified attapulgite.

[0097] The rest is the same as Example 24.

[0098] Embodiment 26 The difference between this embodiment and embodiment 8 is that in step S3, the curing time is 3 days.

[0099] The mass concentration of urease in the urease solution is 100 g / L, the molar concentration of calcium chloride in the cementing solution is 0.25 mol / L, and the molar concentration of urea is 0.25 mol / L.

[0100] Embodiment 27 The difference between this embodiment and embodiment 8 is that in step S3, the curing time is 1 day.

[0101] The mass concentration of urease in the urease solution is 400 g / L, the molar concentration of calcium chloride in the cementing solution is 1 mol / L, and the molar concentration of urea is 1 mol / L.

[0102] Comparative Example 1 This comparative example provides a method for consolidating loess, comprising the following steps: S1: The selected loess is excavated to a depth of about 1 m, and then the excavated loess is dried in the sun. After drying, the loess is crushed by a crusher until it completely passes through a 2 mm sieve to obtain crushed loess; S2: adding purified water to the crushed loess and mixing them evenly to obtain pre-modified loess; S3: Backfill the pre-improved loess in layers, compact it in layers, and finally cover it with plastic film and cure it for 2 days; The pure water is evenly mixed with the crushed loess by spraying multiple times.

[0103] In step S3, the layered compaction coefficient is about 94-96%.

[0104] The amount of pure water is 200L / m 3 .

[0105] Comparative Example 2 This comparative example provides a method for reinforcing loess with rubber particles, comprising the following steps: S1: The selected loess is excavated to a depth of about 1 m, and then the excavated loess is dried in the sun. After drying, the loess is crushed by a crusher until it completely passes through a 2 mm sieve to obtain crushed loess; S2: adding rubber particles to the crushed loess, mixing evenly, and then adding purified water, mixing evenly, to obtain pre-modified loess; S3: Backfill the pre-improved loess in layers, compact it in layers, and finally cover it with plastic film and cure it for 2 days; The rubber particles are mixed evenly with the loess by adding them multiple times, and the pure water is mixed evenly with the mixture of loess and rubber particles by spraying them multiple times.

[0106] In step S3, the layered compaction coefficient is about 94-96%.

[0107] The particle size of rubber particles is 0-1 mm, and the rubber particles account for 5% of the total volume of rubber particles and loess. The amount of pure water used is 200L / m 3 .

[0108] Comparative Example 3 The difference between this comparative example and comparative example 2 is that the rubber particles account for 7% of the total volume of the rubber particles and the loess.

[0109] The rest is the same as Comparative Example 2.

[0110] Comparative Example 4 The difference between this comparative example and comparative example 3 is that the rubber particles account for 10% of the total volume of the rubber particles and the loess.

[0111] Other details are the same as those in Comparative Example 3.

[0112] Comparative Example 5 The difference between this comparative example and comparative example 4 is that the rubber particles account for 13% of the total volume of the rubber particles and the loess.

[0113] The rest is the same as Comparative Example 4.

[0114] Comparative Example 6 The difference between this comparative example and comparative example 5 is that the rubber particles account for 15% of the total volume of the rubber particles and the loess.

[0115] Other details are the same as those in Comparative Example 5.

[0116] Comparative Example 7 The difference between this comparative example and comparative example 6 is that the rubber particles account for 20% of the total volume of the rubber particles and the loess.

[0117] Other details are the same as those in Comparative Example 6.

[0118] Comparative Example 8 The difference between this comparative example and comparative example 7 is that the rubber particles account for 25% of the total volume of the rubber particles and the loess.

[0119] Other details are the same as those in Comparative Example 7.

[0120] Comparative Example 9 The difference between this comparative example and comparative example 8 is that the rubber particles account for 30% of the total volume of the rubber particles and the loess.

[0121] Other details are the same as those in Comparative Example 8.

[0122] Comparative Example 10 The difference between this comparative example and comparative example 2 is that the particle size of the rubber particles is 1 to 2 mm.

[0123] The rest is the same as Comparative Example 2.

[0124] Comparative Example 11 The difference between this comparative example and comparative example 10 is that the rubber particles account for 7% of the total volume of the rubber particles and the loess.

[0125] Other details are the same as those in Comparative Example 10.

[0126] Comparative Example 12 The difference between this comparative example and comparative example 11 is that the rubber particles account for 10% of the total volume of the rubber particles and the loess.

[0127] Other details are the same as those in Comparative Example 11.

[0128] Comparative Example 13 The difference between this comparative example and comparative example 12 is that the rubber particles account for 13% of the total volume of the rubber particles and the loess.

[0129] Other details are the same as those in Comparative Example 12.

[0130] Comparative Example 14 The difference between this comparative example and comparative example 13 is that the rubber particles account for 15% of the total volume of the rubber particles and the loess.

[0131] Other details are the same as those in Comparative Example 13.

[0132] Comparative Example 15 The difference between this comparative example and comparative example 14 is that the rubber particles account for 20% of the total volume of the rubber particles and the loess.

[0133] Other details are the same as those in Comparative Example 14.

[0134] Comparative Example 16 The difference between this comparative example and comparative example 15 is that the rubber particles account for 25% of the total volume of the rubber particles and the loess.

[0135] Other details are the same as those in Comparative Example 15.

[0136] Comparative Example 17 The difference between this comparative example and comparative example 16 is that the rubber particles account for 30% of the total volume of the rubber particles and the loess.

[0137] Other details are the same as those in Comparative Example 16.

[0138] Comparative Example 18 The difference between this comparative example and comparative example 2 is that the particle size of the rubber particles is 2 to 3 mm.

[0139] The rest is the same as Comparative Example 2.

[0140] Comparative Example 19 The difference between this comparative example and comparative example 18 is that the rubber particles account for 7% of the total volume of the rubber particles and the loess.

[0141] Other details are the same as those in Comparative Example 18.

[0142] Comparative Example 20 The difference between this comparative example and comparative example 19 is that the rubber particles account for 10% of the total volume of the rubber particles and the loess.

[0143] Other details are the same as those in Comparative Example 19.

[0144] Comparative Example 21 The difference between this comparative example and comparative example 20 is that the rubber particles account for 13% of the total volume of the rubber particles and the loess.

[0145] Other details are the same as those in Comparative Example 20.

[0146] Comparative Example 22 The difference between this comparative example and comparative example 21 is that the rubber particles account for 15% of the total volume of the rubber particles and the loess.

[0147] Other details are the same as those in Comparative Example 21.

[0148] Comparative Example 23 The difference between this comparative example and comparative example 22 is that the rubber particles account for 20% of the total volume of the rubber particles and the loess.

[0149] Other details are the same as those in Comparative Example 22.

[0150] Comparative Example 24 The difference between this comparative example and comparative example 23 is that the rubber particles account for 25% of the total volume of the rubber particles and the loess.

[0151] Other details are the same as those in Comparative Example 23.

[0152] Comparative Example 25 The difference between this comparative example and comparative example 24 is that the rubber particles account for 30% of the total volume of the rubber particles and the loess.

[0153] Other details are the same as those in Comparative Example 24.

[0154] Comparative Example 26 This comparative example provides a method for EICP reinforcement of loess, comprising the following steps: S1: The selected loess is excavated to a depth of about 1 m, and then the excavated loess is dried in the sun. After drying, the loess is crushed by a crusher until it completely passes through a 2 mm sieve to obtain crushed loess; S2: adding urease solution and cementing liquid to the crushed loess, mixing them evenly, and obtaining pre-modified loess; S3: Backfill the pre-improved loess in layers, compact it in layers, and finally cover it with plastic film and cure it for 2 days; The urease solution and the binder solution are sprayed multiple times in sequence with the mixture of loess and rubber particles to be evenly mixed.

[0155] In step S3, the layered compaction coefficient is about 94-96%.

[0156] The dosage of urease solution is 100L / m 3 The dosage of cementing liquid is 100L / m 3 .

[0157] The preparation method of the urease solution of this comparative example comprises the following steps: Disodium hydrogen phosphate and sodium dihydrogen phosphate are added to water at a molar concentration of 0.2 mol / L (phosphate concentration), the pH value is adjusted to 7.4 with 10% ammonia water, and then mixed with urease to obtain a urease solution; The mass concentration of urease in the urease solution is 100 g / L.

[0158] The preparation method of the cementing fluid of this comparative example comprises the following steps: Calcium chloride and urea are added into water, stirred and mixed evenly, and the pH value is adjusted to 7.4 with citric acid having a mass concentration of 20%, to obtain a cementing liquid; Among them, the molar concentration of calcium chloride in the binder is 0.25 mol / L, and the molar concentration of urea is 0.25 mol / L.

[0159] Comparative Example 27 The difference between this comparative example and comparative example 26 is that the mass concentration of urease in the urease solution is 200 g / L.

[0160] Other details are the same as those in Comparative Example 26.

[0161] Comparative Example 28 The difference between this comparative example and comparative example 27 is that the mass concentration of urease in the urease solution is 300 g / L.

[0162] Other details are the same as those in Comparative Example 27.

[0163] Comparative Example 29 The difference between this comparative example and comparative example 28 is that the mass concentration of urease in the urease solution is 400 g / L.

[0164] Other details are the same as those in Comparative Example 28.

[0165] Comparative Example 30 The difference between this comparative example and comparative example 26 is that the molar concentration of calcium chloride in the binder is 0.5 mol / L, and the molar concentration of urea is 0.5 mol / L.

[0166] Other details are the same as those in Comparative Example 26.

[0167] Comparative Example 31 The difference between this comparative example and comparative example 30 is that the mass concentration of urease in the urease solution is 200 g / L.

[0168] Other details are the same as those in Comparative Example 30.

[0169] Comparative Example 32 The difference between this comparative example and comparative example 31 is that the mass concentration of urease in the urease solution is 300 g / L.

[0170] Other details are the same as those in Comparative Example 31.

[0171] Comparative Example 33 The difference between this comparative example and comparative example 32 is that the mass concentration of urease in the urease solution is 400 g / L.

[0172] Other details are the same as those in Comparative Example 32.

[0173] Comparative Example 34 The difference between this comparative example and comparative example 26 is that the molar concentration of calcium chloride in the binder is 0.75 mol / L, and the molar concentration of urea is 0.75 mol / L.

[0174] Other details are the same as those in Comparative Example 26.

[0175] Comparative Example 35 The difference between this comparative example and comparative example 34 is that the mass concentration of urease in the urease solution is 200 g / L.

[0176] Other details are the same as those in Comparative Example 34.

[0177] Comparative Example 36 The difference between this comparative example and comparative example 35 is that the mass concentration of urease in the urease solution is 300 g / L.

[0178] Other details are the same as those in Comparative Example 35.

[0179] Comparative Example 37 The difference between this comparative example and comparative example 36 is that the mass concentration of urease in the urease solution is 400 g / L.

[0180] Other details are the same as those in Comparative Example 36.

[0181] Comparative Example 38 The difference between this comparative example and comparative example 26 is that the molar concentration of calcium chloride in the binder is 1 mol / L, and the molar concentration of urea is 1 mol / L.

[0182] Other details are the same as those in Comparative Example 26.

[0183] Comparative Example 39 The difference between this comparative example and comparative example 38 is that the mass concentration of urease in the urease solution is 200 g / L.

[0184] Other details are the same as those in Comparative Example 38.

[0185] Comparative Example 40 The difference between this comparative example and comparative example 39 is that the mass concentration of urease in the urease solution is 300 g / L.

[0186] Other details are the same as those in Comparative Example 39.

[0187] Comparative Example 41 The difference between this comparative example and comparative example 40 is that the mass concentration of urease in the urease solution is 400 g / L.

[0188] Other details are the same as those in Comparative Example 40.

[0189] Experimental testing This test adopts a quick shear test, using a ZJ strain-controlled direct shear apparatus, with a direct shear rate of 0.8mm / min to 1.2mm / min, and the test data is automatically recorded by a computer. The test is divided into two parts: a preliminary test and a shear characteristic test.

[0190] The proportion range of rubber particles and the optimal concentrations of urease and binder were determined by preliminary experiments, and then the shear properties test was carried out on the loess improved by only rubber particles and the loess improved by rubber particles combined with EICP to test the data.

[0191] (1) Preliminary experiment First, a quick shear test was conducted on the improved loess mixed with only rubber particles. After the curing of the improved loess in comparative examples 1 to 25 was completed, a ring knife with a diameter of 61.80 mm and a height of 20 mm was used to cut multiple undisturbed soil samples from different parts of the undisturbed soil samples of comparative examples 1 to 25, and the two ends were leveled. Multiple undisturbed soil samples from different parts of each comparative example were placed on the shear box, with an impermeable stone placed on the top and bottom, and the sample was pressed into the shear box with a top cap. The equipment was started after applying a vertical pressure of 100 kPa, and the test was started after adjusting the shear rate to 0.8 mm / min. When the dial indicator reading no longer moved forward but retreated, the shearing continued until the shear displacement was 4 mm, and the shear strength corresponding to the peak value was read. When the dial indicator reading had no peak value, the test was stopped when the shear displacement was 6 mm, and the shear strength corresponding to the shear displacement of 4 mm was read, and the average value of multiple undisturbed soil samples at different parts of the same comparative example was obtained. The experimental results are as follows: Figure 3 As shown, the optimal dosage range of rubber particles is screened according to the shear strength of the samples in Comparative Examples 1 to 25.

[0192] in: In Comparative Example 1, the amount of rubber added is 0%; In comparative examples 2 to 9, the rubber content is 5 to 30% and the rubber particles are 0 to 1 mm; In comparative examples 10 to 17, the rubber content is 5 to 30% and the rubber particles are 1 to 2 mm; In Comparative Examples 18 to 25, the rubber content is 5 to 30% and the rubber particles are 2 to 3 mm.

[0193] Depend on Figure 3 It can be seen that under different rubber particle sizes, as the rubber content increases, the change trend of the shear strength of the samples has certain similarities, all showing a law of first increasing and then decreasing. Compared with the 0% rubber particle content in Comparative Example 1, the rubber content ranges in which the shear strength of the samples increases are different, but the shear strength peaks appear between 7% and 13% rubber content. Although the shear strength of the samples is lower than that of 0% when the rubber content is 7% to 13% under some particle sizes, considering that the EICP technology will continue to improve the shear strength of the samples, the rubber content range is selected to be 5% to 15% for subsequent shear property tests.

[0194] Loess itself is a loose material, while rubber particles are a material with a rough surface and a dense interior. Adding a small amount of rubber particles to loess reduces the internal pore defects of the sample and inhibits the development of sample cracks during shear failure, so the shear strength of the sample is improved. However, the strength of rubber particles is lower than that of soil particles. When rubber particles replace soil particles in equal volume, the overall strength of the soil is reduced. Moreover, when the rubber content increases, rubber particles are prone to aggregation and floating during the mixing process with loess. The aggregation of rubber particles will increase the pores of the sample and produce a weak interface. The sample is more likely to be damaged when sheared, resulting in a decrease in shear strength. Therefore, when the rubber content exceeds the critical value, the shear strength tends to decrease.

[0195] Secondly, a quick shear test was carried out on the improved loess mixed with only urease solution and binder. After the curing of the improved loess in Comparative Examples 26 to 41 was completed, a plurality of original soil samples from different parts of the original soil samples of Comparative Examples 26 to 41 were cut using a ring cutter with a diameter of 61.80 mm and a height of 20 mm, and the two ends were leveled. The multiple original soil samples from different parts of each comparative example were placed on the shear box, with an impermeable stone placed on the top and bottom, and the sample was pressed into the shear box with a top cap. The equipment was started after applying a vertical pressure of 100 kPa, and the test was started after adjusting the shear rate to 0.8 mm / min. When the dial indicator reading no longer moved forward but retreated, the shearing was continued until the shear displacement was 4 mm, and the shear strength corresponding to the peak value was read. When there was no peak in the dial indicator reading, the test was stopped when the shear displacement was 6 mm, and the shear strength corresponding to the shear displacement of 4 mm was read, and the average value of multiple original soil samples from different parts of the same comparative example was obtained. The experimental results are as follows Figure 4 As shown, the optimal concentrations of urease and binder are determined based on the shear strength of the samples in Comparative Examples 26 to 41.

[0196] Among them, the urease concentration in Comparative Examples 1 to 5 is 100-400 g / L, and the total molar concentration of the cementing solution is 0.5 mol / L, the urease concentration in Example 2 is 100-400 g / L, and the total molar concentration of the cementing solution is 1 mol / L, the urease concentration in Example 3 is 100-400 g / L, and the total molar concentration of the cementing solution is 1.5 mol / L, and the urease concentration in Example 4 is 100-400 g / L, and the total molar concentration of the cementing solution is 2 mol / L.

[0197] Depend on Figure 4It can be seen that under different cementing fluid concentrations, the shear strength of the samples changes with the urease concentration in a uniform trend. As the urease concentration increases, the shear strength of the samples increases first and then decreases, and the urease concentration corresponding to the peak shear strength is 200g / L. Under different urease concentrations, the shear strength of the samples changes with the cementing fluid concentration in a similar manner, and they all approximately show a law of first increasing and then decreasing. The cementing fluid concentration corresponding to the peak shear strength is 1mol / L (that is, the molar concentration of calcium chloride in the cementing fluid is 0.5mol / L, and the molar concentration of urea is 0.5mol / L). Therefore, through this orthogonal test, the urease concentration for the subsequent shear property test is determined to be 200g / L, and the cementing fluid concentration is 1mol / L.

[0198] Based on the working principle of EICP, when the concentration of the cementing fluid is fixed, the shear strength of the sample is enhanced to varying degrees by adding urease solutions of different concentrations, and the urease concentration corresponding to the peak shear strength is 200g / L. The reason for this phenomenon is that when the urease concentration is low, the ability of urease to decompose urea is limited, so the amount of calcium carbonate generated is small, and the shear strength improvement rate of the sample is low; when the urease concentration is high, the amount of cementing fluid is fixed, urease completely decomposes urea, and the output of calcium carbonate is fixed, but considering that the distribution of the cementing fluid is not completely uniform during the sample preparation process, during the sample curing process, the cementing fluid has been decomposed and utilized by urease before the migration is completed, so the filling of the sample skeleton is uneven, resulting in a low shear strength growth rate, so there is a critical value for the urease concentration. When the urease concentration is fixed, as the cementing fluid concentration increases, the calcium ion concentration also increases. When the cementing fluid concentration is less than the critical value, the calcium carbonate produced by the decomposition of urea by urease combines with calcium ions, and the calcium carbonate production increases. However, excessively high concentrations of calcium ions will inhibit urease activity and reduce urea decomposition, thereby reducing carbonate concentration and reducing calcium carbonate production. Therefore, there is a critical value for the cementing fluid concentration.

[0199] (2) Shear property test (a) After the curing of the improved loess in Comparative Example 1 and Comparative Examples 10 to 14 is completed, a ring cutter with a diameter of 61.80 mm and a height of 20 mm is used to cut multiple original soil samples from different parts of the original soil samples of Comparative Examples 1 and Comparative Examples 10 to 14, and the two ends are leveled. Shear tests are carried out under two different vertical pressures, and the vertical pressures can be: 50 kPa and 100 kPa. Multiple original soil samples from different parts of each comparative example are placed on a shear box, with an impermeable stone placed on the top and bottom, and the samples are pressed into the shear box with a top cap. After applying vertical pressure, the equipment is started, and the shear rate is adjusted to 0.8 mm / min before the test is started. The shear strength corresponding to different shear displacements is measured, and the average value of multiple original soil samples at different parts of the same comparative example is calculated. Then, according to the Mohr-Coulomb shear strength criterion, a linear fit is performed on the shear strength of a single sample under different vertical pressures to obtain a shear stress-shear displacement relationship curve under different vertical pressures, as shown in FIG. Figure 5 and Figure 6 shown.

[0200] The rubber particle content in Comparative Example 1 and Comparative Examples 10 to 14 is 0 to 15%, and the rubber particle diameter is 1 to 2 mm.

[0201] Depend on Figure 5 and Figure 6 It can be seen that the variation law of the shear stress-shear displacement curve of the samples under different rubber content is similar. When the vertical pressure is 50kPa, the samples with different rubber content show strain softening characteristics, that is, after the shear stress reaches the maximum value, the shear stress gradually decreases with the increase of shear displacement; when the vertical pressure is 100kPa, the sample shows strain hardening characteristics, that is, after the shear stress reaches the maximum value, the shear stress remains unchanged or continues to increase with the increase of shear displacement. In view of this, the strain characteristics of the samples of comparative examples 2 to 6 and comparative examples 18 to 22 can be inferred, and the strain characteristics of comparative examples 1 to 6, 10 to 14, and 18 to 22 are statistically shown in Table 2.

[0202] Table 2 Statistical table of strain characteristics of samples of comparative examples 1-6, 10-14, 18-22 (rubber content 0-15%) From the results in Table 2, it can be seen that the strain characteristics of the samples with different rubber content and different rubber particle sizes are similar. Under low pressure, the strain characteristics of the samples show a softening law. When the vertical pressure increases, the strain characteristics change from softening to hardening. Under high pressure, they all show strain hardening characteristics.

[0203] (b) After the curing of the improved loess in Comparative Examples 1-6, 10-14, 18-22 is completed, a plurality of original soil samples from different parts of the original soil samples of Comparative Examples 1-6, 10-14, 18-22 are cut by a circular cutter with a diameter of 61.80 mm and a height of 20 mm, and the two ends are leveled. Shear tests are carried out under four different vertical pressures, and the vertical pressures can be: 50 kPa, 100 kPa, 200 kPa, and 300 kPa. Multiple undisturbed soil samples from different parts of each comparative example were placed on the shear box, with an impermeable stone placed on the top and bottom. The samples were pressed into the shear box with a top cap. The equipment was started after applying vertical pressure. The shear rate was adjusted to 0.8 mm / min and the test was started. When the dial indicator reading no longer moved forward but backward, shearing was continued until the shear displacement was 4 mm, and the shear strength corresponding to the peak value was read. When there was no peak in the dial indicator reading, the test was stopped when the shear displacement was 6 mm, and the shear strength corresponding to the shear displacement of 4 mm was read. The average values ​​of multiple undisturbed soil samples from different parts of the same comparative example were obtained, as shown in Table 3.

[0204] Table 3 Shear strength of samples of comparative examples 1-6, 10-14, 18-22 (rubber content 0-15%) under different vertical pressures Analysis of the shear strength results of the samples in Table 3 shows that under the same vertical pressure and different rubber particle sizes, with the increase of rubber content, the shear strength of the samples has a similar change pattern, showing a trend of first increasing and then decreasing, and the shear strength of the corresponding samples when the rubber particle size is 1-2mm is higher than the shear strength of the corresponding samples when the rubber particle size is 0-1mm and 2-3mm. Under different vertical pressures, compared with the 0% content control group, the rubber content range corresponding to the increase in the shear strength of the samples is roughly between 7% and 13%, and under different vertical pressures, the maximum increase in the shear strength of the samples is 19.49%, 30.41%, 24.92% and 28.74% respectively.

[0205] The shear strength results of the samples in Table 3 under different vertical pressures were linearly fitted to obtain the curves of cohesion and internal friction angle of the samples under different rubber content and different rubber particle sizes, as shown in Figure 2. Figure 7 and Figure 8 As shown. Under different rubber particle sizes, the cohesion and internal friction angle of the samples increase first and then decrease with the change of rubber content, and the cohesion and internal friction angle of the corresponding samples are the largest when the rubber particle size is 1-2mm. Compared with the 0% content control group, when the rubber particle size is 1-2mm and the rubber content is 10%-13%, the cohesion and internal friction angle of the samples increase, with the maximum increase in cohesion being 31.57% and the maximum increase in internal friction angle being 27.89%.

[0206] Comprehensive comparison table 3 and Figure 7-8 The results show that the shear strength index of the sample is composed of cohesion and internal friction angle. For the improved loess only mixed with rubber particles, although the maximum increase in cohesion is higher than the maximum increase in internal friction angle, the increase range of cohesion is only in the interval of rubber particle size of 1-2mm and the addition amount of 10%-13%, while the internal friction angle increases in the interval of rubber particle size of 0-1mm, the addition amount of 10%-13% and the rubber particle size of 1-2mm, the addition amount of 7%-15%. The increase range of the internal friction angle is wider. Therefore, for the improved loess only mixed with rubber particles with increased shear strength, the internal friction angle plays a major role in most of them.

[0207] (c) After the curing of the improved loess in Examples 1 to 25 is completed, a plurality of original soil samples at different positions are cut from the original soil samples of Examples 1 to 25 using a circular cutter with a diameter of 61.80 mm and a height of 20 mm, and the two ends are flattened. Shear tests are performed under four different vertical pressures, and the vertical pressures can be: 50 kPa, 100 kPa, 200 kPa, and 300 kPa. The multiple original soil samples at different positions in each embodiment are placed on a shear box, and a piece of impermeable stone is placed on the top and bottom. The sample is pressed into the shear box with a top cap. After applying vertical pressure, the equipment is started, and the shear rate is adjusted to 0.8 mm / min before the test is started. When the dial indicator reading no longer moves forward but moves backward, the shearing is continued until the shear displacement is 4 mm, and the corresponding shear strength at the peak is read. When the dial indicator reading has no peak, the test is stopped when the shear displacement is 6 mm, and the corresponding shear strength at the shear displacement of 4 mm is read, and the average value of the multiple original soil samples at different positions of the same embodiment is obtained, as shown in Table 4.

[0208] Table 4 Shear strength of samples of Examples 1 to 15 (rubber content 5 to 15%) under different vertical pressures The deformation development rules of the samples in Examples 1 to 15 during shear failure were compared and analyzed to obtain the strain characteristics of each sample, and the results were consistent with the results of the samples in Comparative Examples 10 to 14.

[0209] The shear strength growth rate of each sample of Examples 1 to 15 under different vertical pressures was calculated, and a curve of the shear strength growth rate of the sample versus the rubber content was plotted, as shown in FIG. Figures 9 to 12 The shear strength growth rate is a comparison of the shear strength of each sample of Examples 1 to 15 with the shear strength of each sample of Comparative Examples 2 to 6, 10 to 14, and 18 to 22 under the same conditions.

[0210] Comprehensive analysis of Table 4 and Figures 9 to 12The test results show that the shear strength variation law of each sample in Examples 1 to 15 is consistent with that of each sample in Comparative Examples 2 to 6, 10 to 14, and 18 to 22, and after being treated with EICP technology, the shear strength of the samples increases to varying degrees. Under the same vertical pressure and different rubber particle sizes, with the increase of rubber content, the shear strength of the samples increases first and then decreases, and the shear strength growth rate of the samples decreases gradually. When the rubber particle size is 1 to 2 mm, the shear strength and shear strength growth rate of the corresponding samples are higher than those of the corresponding samples at 0 to 1 mm and 2 to 3 mm. Under different vertical pressures, compared with the results of only adding rubber particles, the maximum increase ratio of the shear strength of the samples is 18.16%, 16.75%, 17.4% and 18.62% respectively; compared with the 0% content control group, the maximum increase ratio of the shear strength of the samples is 36.41%, 45.5%, 39.5% and 46.43% respectively.

[0211] The shear strength results of each sample of Examples 1 to 15 in Table 4 under different vertical pressures were linearly fitted to obtain a curve diagram of the cohesion and internal friction angle of the samples under different rubber content and different rubber particle sizes, as shown in FIG. Fig.13 and Fig.14 Comprehensive comparative analysis Figures 7-8 and Figures 13-14 The results show that the variation curves of the cohesion and internal friction angle of the samples with the rubber content under different reinforcement conditions show that the variation laws of the cohesion and internal friction angle of the samples under different reinforcement conditions are relatively consistent, and the results are increased to varying degrees after being treated with EICP technology. Compared with the results of comparative examples 2-6, 10-14, 18-22 (only rubber particles), the maximum increase ratios of sample cohesion and internal friction angle were 15.19% and 28.56%, respectively; compared with the control group of comparative example 1 (rubber 0% dosage), the maximum increase ratios of sample cohesion and internal friction angle were 47.87% and 64.42%, respectively, the increase range of cohesion was the interval of rubber particle size of 0-1mm and dosage of 7% and rubber particle size of 1-2mm and dosage of 7%-13%, the increase range of internal friction angle was the interval of rubber particle size of 0-1mm and 1-2mm and dosage of 5%-15% and rubber particle size of 2-3mm and dosage of 10-13%, therefore, under the reinforcement condition, when the shear strength of the sample increased, the internal friction angle still played a major role.

[0212] Comparative analysis of the data results of Example 8 and Examples 16 to 25 shows that the shear strength of the samples under different vertical pressures has decreased and increased. This is mainly due to: First, too high calcium ion content will inhibit urease activity, reduce urea decomposition, thereby reducing carbonate concentration, resulting in a decrease in calcium carbonate production; too low urea content will also reduce carbonate concentration, resulting in a decrease in calcium carbonate production; thus, the shear strength has decreased and increased. Second, by soaking in alkaline solution, the roughness of the rubber particle surface can be enhanced, which not only enhances the bonding force between the rubber particles and the loess particles, but also improves the unconfined compressive strength of the rubber particles stabilizing the loess particles; third, by introducing polyacrylamide, introducing auxiliary agents, and modifying urea in the binder, on the one hand, the cohesion between the sand particles is increased, so that the sand particles are aggregated, thereby making it easier to capture calcium carbonate crystals, increase the calcium carbonate precipitation yield, and improve the curing effect. On the other hand, it inhibits the activity of urease and reduces the hydrolysis and release rate of the initial urea, so that the urea and calcium chloride in the binder can be evenly distributed and migrated in the loess, making the calcium carbonate precipitation more evenly distributed, thereby improving the overall effect of loess reinforcement.

Claims

1. A method for reinforcing loess by using rubber particles and EICP, characterized in that: The following steps are involved: S1: Selecting the loess site, drying and crushing the selected loess; S2: adding rubber particles to the crushed loess, mixing evenly, and then adding urease solution and cementing liquid, mixing evenly to obtain pre-modified loess; S3: Backfill and compact the pre-improved loess in layers, cover with film, and cure for 1 to 3 days; The rubber particles account for 5-15% of the total volume of the rubber particles and loess; the total amount of urease solution and cementing fluid is 150-300 L / m 3 ; The urease solution comprises urease and water, wherein the urease is derived from a kind of beans; The binder solution includes urea, calcium chloride and water.

2. The method for reinforcing loess by using rubber particles and EICP according to claim 1, characterized in that: The particle size of the rubber particles does not exceed 3 mm.

3. The method for reinforcing loess by using rubber particles and EICP according to claim 1, characterized in that: The mass concentration of urease in the urease solution is 100-400 g / L.

4. The method for reinforcing loess by using rubber particles and EICP according to claim 1, characterized in that: In step S2, the rubber particles are soaked in an alkaline solution for 24 to 26 hours before use, and then solid-liquid separation, washed, dried, and then mixed into the pulverized yellow soil.

5. The method for reinforcing loess by using rubber particles and EICP according to claim 1, characterized in that: The total molar concentration of calcium chloride and urea in the binder is 0.5-2 mol / L.

6. The method for reinforcing loess by using rubber particles and EICP according to claim 5, characterized in that: The preparation method of the cementing liquid comprises the following steps: Add calcium chloride and urea into water and mix them evenly, then mix them evenly with polyacrylamide to obtain a cementing liquid; The mass concentration of polyacrylamide in the binder is 0.2-0.5 g / L.

7. The method for reinforcing loess by using rubber particles and EICP according to claim 6, characterized in that: Calcium chloride and urea are added into water and mixed evenly, an auxiliary agent is added and mixed evenly, and then mixed evenly with polyacrylamide to obtain a binder; the mass concentration of the auxiliary agent in the binder is 0.1-0.3 g / L, and the auxiliary agent is at least one of humic acid and thiourea.

8. The method for strengthening loess by using rubber particles and EICP according to claim 7, characterized in that: The urea is modified urea, and the preparation method of the modified urea comprises the following steps by weight: 1800-2000 parts by weight of urea are placed in a coating machine and heated to 75-85°C. Then, 10-12 parts by weight of 2,6-xylyl isocyanate, 2-3 parts by weight of paraffin, 4-5 parts by weight of modified attapulgite and 4-5 parts by weight of calcium oxide are added and rotated for 3-5 minutes. Then, 10-12 parts by weight of polycaprolactone diol are added and mixed evenly. After reacting at 60-70°C for 2-4 hours, the mixture is dried to obtain modified urea.

9. The method for reinforcing loess by using rubber particles and EICP according to claim 8, characterized in that: The preparation method of the modified attapulgite comprises the following steps: Calcine the attapulgite at 200-500°C for 1.5-2.5h, cool it down, take it out, and crush it to obtain powdered attapulgite; The powdered attapulgite is placed in a sodium hydroxide solution, soaked for 10 to 12 minutes, separated from the solid and the liquid, and washed to obtain pre-modified attapulgite; The pre-modified attapulgite is uniformly mixed with a 3-aminopropyltrimethoxysilane solution, and then uniformly mixed with a modifier, soaked, solid-liquid separated, and dried to obtain modified attapulgite; The modifier is at least one of polyvinyl alcohol and polymethyl acrylate.

Citation Information

Cited By

  • Underwater self-cementation reinforcing and filling unit and throwing and filling reinforcing method thereof

    CN119308260A

  • Coal mine filling material based on loess composite curing agent and preparation method thereof

    CN120058333A

  • Preparation method of cured loess suitable for high-grade highway base construction

    CN121107815A