A fire-resistant water-based coating containing modified maleimide and preparation method thereof

By blending modified maleimide flame retardant with waterborne polyurethane, the problems of poor fire resistance and flame retardancy and compatibility of polyurethane coatings were solved, achieving high hardness, strong tensile strength and excellent fire resistance and flame retardancy.

CN118755367BActive Publication Date: 2024-11-29JUNXIU NEW MATERIAL TECH (SUZHOU) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410854237.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-29
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Existing polyurethane coatings have poor fire resistance and flame retardancy, and additive flame retardants have poor compatibility with the material matrix, affecting mechanical properties.

Method used

A modified maleimide flame retardant was prepared by addition polymerization of bismaleimide and dibenzyl thiol phosphate intermediates into N,N-dimethylacetamide solvent in nitrogen. The modified maleimide flame retardant was then blended with waterborne polyurethane to form a modified maleimide whose molecular backbone contains urethane groups and spirocyclic phosphate phosphorus flame retardant groups.

Benefits of technology

The compatibility between the flame retardant and polyurethane was improved, the hardness and tensile strength of the coating were increased, and the limiting oxygen index was improved through the intumescent flame retardant system, achieving the UL94 V0 level of fire resistance and flame retardant performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755367B_ABST
    Figure CN118755367B_ABST
Patent Text Reader

Abstract

The invention discloses a fire-resistant water-based coating containing modified maleimide and a preparation method thereof, including 100 parts by weight of waterborne polyurethane, 3-15 parts by weight of modified maleimide flame retardant; 0.4-1 parts by weight of defoamer, 0.5-0.8 parts by weight of leveling agent, 10-30 parts by weight of pigments and fillers, 0.5-1.5 parts by weight of dispersant; The present invention uses modified maleimide flame retardant to add blending modification to waterborne polyurethane coating, and the flame retardant has good compatibility with polyurethane, and the flame retardant molecular chain contains phenylmaleimide structure, has large rigidity, and has strong structural stability, and can improve the hardness and tensile strength of polyurethane coating film. The flame retardant contains spirocyclic phosphate phosphorus-containing flame retardant groups and maleimide nitrogen-containing heterocycles, and can form an expansion flame retardant system, which plays a role in heat insulation, oxygen isolation, smoke suppression and other fire-resistant flame retardant effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, in particular to a fire-resistant water-based coating containing modified maleimide and a preparation method thereof. Background Art

[0002] Waterborne polyurethane coatings are green and environmentally friendly, have good film-forming properties, and high toughness. They are widely used in wooden furniture, electronic appliances, machinery manufacturing, and other fields. Adding flame retardants to polyurethane coatings can improve their fire resistance and flame retardancy, making polyurethane have better practical applications in fireproof materials. Common flame retardants for polyurethane include brominated flame retardants, phosphorus-containing flame retardants, and intumescent flame retardants.

[0003] Maleimide and its resin materials have high strength and excellent high temperature resistance, and are widely used in coatings such as polyurethane and acrylic resin. Patent CN108440735B contains Diels-Alder bond self-healing flame-retardant polyurethane elastomer and its preparation method, using maleimide-modified hexachlorocyclotriphosphazene as a reactive flame retardant, and reacting with a polyurethane containing a furan functional group in the side chain, and the obtained polyurethane elastomer has good flame retardancy and mechanical properties. However, the reaction system of the maleimide-modified hexachlorocyclotriphosphazene and furan-based polyurethane is relatively complicated. The additive flame retardant is added to the material matrix in an additive blending manner, which is very simple to operate and does not undergo complex chemical reactions with the material matrix. However, if the additive flame retardant is not compatible with the material matrix, it will affect the mechanics and performance of the material. Summary of the invention

[0004] 1. Technical problems solved:

[0005] In view of the deficiencies in the prior art, the present invention provides a fire-resistant water-based coating containing modified maleimide, which solves the problem of poor fire-resistant and flame-retardant properties of polyurethane coatings.

[0006] (II) Technical solution: A fire-resistant water-based coating containing modified maleimide, comprising 100 parts by weight of water-based polyurethane, 3-15 parts by weight of modified maleimide flame retardant; 0.4-1 parts by weight of defoamer, 0.5-0.8 parts by weight of leveling agent, 10-30 parts by weight of pigment and filler, and 0.5-1.5 parts by weight of dispersant.

[0007] The preparation method of the modified maleimide flame retardant is as follows: in nitrogen, a bismaleimide intermediate, a bisbenzyl mercaptan phosphate intermediate and triethylamine are added to an N,N-dimethylacetamide solvent, the reaction is followed by filtering, a precipitate is washed with dichloromethane and dried to obtain the modified maleimide flame retardant.

[0008] The bismaleimide intermediate has the following structural formula (I):

[0009]

[0010] The bisbenzyl mercaptan phosphate intermediate has the following structural formula (II):

[0011]

[0012] Furthermore, the amount of the bismaleimide intermediate is 100 parts by weight, the bisbenzyl mercaptan phosphate intermediate is 82-87 parts by weight, and the triethylamine is 12-18 parts by weight.

[0013] Further, the reaction is carried out at 15-30°C for 1-2h.

[0014] Furthermore, the preparation method of the bismaleimide intermediate is as follows: diphenylmethane-4,4'-diisocyanate and N-(4-hydroxyphenyl)maleimide are added to a toluene solvent, the solution is concentrated after the reaction, the precipitate is washed with acetone, and recrystallized with ethanol to obtain the bismaleimide intermediate.

[0015] Furthermore, the amount of diphenylmethane-4,4'-diisocyanate is 100 parts by weight, and the amount of N-(4-hydroxyphenyl)maleimide is 152-165 parts by weight.

[0016] Furthermore, in the preparation method of the bismaleimide intermediate, the reaction is carried out at 60-80° C. for 2-4 h.

[0017] Further, the preparation method of the bis-benzyl mercaptan phosphate intermediate is:

[0018] (1) Add 100 parts by weight of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, 155-170 parts by weight of 4-bromomethylbenzyl alcohol, and 70-78 parts by weight of triethylamine to an acetonitrile solvent, react at 10-15° C. for 30-60 minutes, then at 65-75° C. for 4-6 hours, concentrate the solution, wash the precipitate with acetone, and dry to obtain an intermediate A.

[0019] (2) Add 100 parts by weight of intermediate A, 62-72 parts by weight of thioacetic acid, and 84-92 parts by weight of potassium carbonate to a methanol solvent, react at 20-30° C. for 30-60 minutes, then add 84-92 parts by weight of potassium carbonate, continue to react for 1-2 hours, add hydrochloric acid solution to neutralize the pH of the reaction solution to 6, concentrate the solution, precipitate a large amount of precipitate, wash with water and acetone in turn, and dry to obtain a bisbenzyl mercaptan phosphate intermediate.

[0020] Furthermore, the preparation method of the fire-resistant water-based coating containing modified maleimide is: stirring and dispersing water-based polyurethane, modified maleimide flame retardant, defoamer, leveling agent, pigment filler, dispersant and water in a high-speed disperser to obtain the fire-resistant water-based coating containing modified maleimide.

[0021] (III) Technical effect: The present invention uses triethylamine as a catalyst to carry out addition polymerization reaction on a novel bismaleimide intermediate and a bisbenzyl mercaptan phosphate intermediate to obtain a modified maleimide flame retardant containing a carbamate group on the molecular main chain, a spirocyclic phosphate phosphorus-containing flame retardant group, and a maleimide nitrogen-containing heterocycle.

[0022] The present invention utilizes a modified maleimide flame retardant to perform adding and blending modification on a waterborne polyurethane coating, wherein the main molecular chain of the modified flame retardant contains the same carbamate structural unit as that of the polyurethane, thereby making the flame retardant and the polyurethane have good compatibility, and adding the flame retardant will not affect the mechanical properties of the polyurethane, and the flame retardant molecular chain contains a phenylmaleimide structure, which has high rigidity and strong structural stability, and can improve the hardness and tensile strength of the polyurethane coating film.

[0023] The modified maleimide flame retardant of the present invention contains a spirocyclic phosphate phosphorus-containing flame retardant group and a maleimide nitrogen-containing heterocycle, and can form an expansion flame retardant system. During combustion, the flame retardant spirocyclic phosphate serves as an acid source and a carbon source, and nitrogen atoms such as nitrogen-containing heterocycles serve as a gas source, forming a foam expansion carbon layer on the surface of the polyurethane, which has fire-resistant and flame-retardant effects such as heat insulation, oxygen isolation, and smoke suppression. Now the limiting oxygen index of the polyurethane is improved, and the UL94 reaches the V0 level. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the reaction formula for preparing bismaleimide intermediate.

[0025] Figure 2 This is the reaction formula for preparing the intermediate of bisbenzyl mercaptan phosphate.

[0026] Figure 3 It is the reaction formula for preparing modified maleimide flame retardant. DETAILED DESCRIPTION

[0027] The technical solution of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the purpose of the embodiments is to further illustrate the content of the present invention and cannot be interpreted as limiting the protection scope of the present invention in any sense.

[0028] The CAS registration number of diphenylmethane-4,4'-diisocyanate of the present invention is 101-68-8. The CAS registration number of N-(4-hydroxyphenyl)maleimide is 7300-91-6. The registration number of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide is 714-87-4. The CAS registration number of 4-bromomethylbenzyl alcohol is 71831-21-5.

[0029] Waterborne polyurethane brand F0401. Defoamer brand AFN-20, leveling agent brand BYK381, dispersant TEGO-Dispers655.

[0030] The preparation method of the bismaleimide intermediate is as follows: 100 parts by weight of diphenylmethane-4,4'-diisocyanate and 152-165 parts by weight of N-(4-hydroxyphenyl)maleimide are added to a toluene solvent, reacted at 60-80° C. for 2-4 hours, the solution is concentrated, the precipitate is washed with acetone, and recrystallized with ethanol to obtain a bismaleimide intermediate.

[0031] Preparation method of bis-benzyl mercaptan phosphate intermediate:

[0032] (1) Add 100 parts by weight of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, 155-170 parts by weight of 4-bromomethylbenzyl alcohol, and 70-78 parts by weight of triethylamine to an acetonitrile solvent, react at 10-15° C. for 30-60 minutes, then at 65-75° C. for 4-6 hours, concentrate the solution, wash the precipitate with acetone, and dry to obtain an intermediate A.

[0033] (2) Add 100 parts by weight of intermediate A, 62-72 parts by weight of thioacetic acid, and 84-92 parts by weight of potassium carbonate to a methanol solvent, react at 20-30° C. for 30-60 minutes, then add 84-92 parts by weight of potassium carbonate, continue to react for 1-2 hours, add hydrochloric acid solution to neutralize the pH of the reaction solution to 6, concentrate the solution, precipitate a large amount of precipitate, wash with water and acetone in turn, and dry to obtain a bisbenzyl mercaptan phosphate intermediate.

[0034] The preparation method of the modified maleimide flame retardant is as follows: 100 parts by weight of a bismaleimide intermediate, 82-87 parts by weight of a bisbenzyl mercaptan phosphate intermediate, and 12-18 parts by weight of triethylamine are added to an N,N-dimethylacetamide solvent in nitrogen, and the mixture is reacted at 15-30° C. for 1-2 hours, filtered, and the precipitate is washed with dichloromethane and dried to obtain the modified maleimide flame retardant.

[0035] The preparation method of a fire-resistant water-based coating containing modified maleimide is as follows: 100 parts by weight of water-based polyurethane, 3-15 parts by weight of a modified maleimide flame retardant, 0.4-1 parts by weight of a defoamer, 0.5-0.8 parts by weight of a leveling agent, 10-30 parts by weight of a pigment filler, 0.5-1.5 parts by weight of a dispersant, and 120 parts by weight of water are stirred and dispersed in a high-speed disperser to obtain a fire-resistant water-based coating containing modified maleimide.

[0036] Example 1

[0037] (1) Add 2 g of diphenylmethane-4,4'-diisocyanate and 3.3 g of N-(4-hydroxyphenyl)maleimide to 30 mL of toluene solvent, react at 60° C. for 3 h, concentrate the solution, wash the precipitate with acetone, and recrystallize with ethanol to obtain a bismaleimide intermediate.

[0038] (2) 4 g of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, 6.2 g of 4-bromomethylbenzyl alcohol, and 2.8 g of triethylamine were added to 60 mL of acetonitrile solvent, and the mixture was reacted at 10° C. for 60 min and then at 70° C. for 6 h. After the reaction, the solution was concentrated, the precipitate was washed with acetone, and dried to obtain intermediate A.

[0039] (3) Add 5 g of intermediate A, 3.3 g of thioacetic acid and 4.6 g of potassium carbonate to 80 mL of methanol solvent, react at 25° C. for 30 min, then add 4.6 g of potassium carbonate and continue to react for 2 h. Add hydrochloric acid solution to neutralize the pH of the reaction solution to 6, concentrate the solution, precipitate a large amount of precipitate, wash with water and acetone in turn, and dry to obtain a bis-benzyl mercaptan phosphate intermediate.

[0040] (4) In nitrogen, 20 g (31.84 mmol) of bismaleimide intermediate, 17.4 g (32.70 mmol) of bisbenzyl mercaptan phosphate intermediate, and 3.6 g of triethylamine were added to 300 mL of N,N-dimethylacetamide solvent, and the mixture was reacted at 30° C. for 1 h. The mixture was filtered, and the precipitate was washed with dichloromethane and dried to obtain a modified maleimide flame retardant.

[0041] (5) 1000 g of waterborne polyurethane, 30 g of modified maleimide flame retardant, 4 g of defoamer, 8 g of leveling agent, 100 g of pigment titanium dioxide, 15 g of dispersant, and 1200 g of water are stirred and dispersed in a high-speed disperser to obtain a fire-resistant waterborne coating containing modified maleimide.

[0042] Example 2

[0043] (1) Prepare the bismaleimide intermediate according to the method of Example 1.

[0044] (2) Prepare the dibenzyl mercaptan phosphate intermediate according to the method of Example 1.

[0045] (3) In nitrogen, 20 g of bismaleimide intermediate, 16.4 g of bisbenzyl mercaptan phosphate intermediate, and 3.6 g of triethylamine were added to 300 mL of N,N-dimethylacetamide solvent, and the mixture was reacted at 20° C. for 1 h. The mixture was filtered, and the precipitate was washed with dichloromethane and dried to obtain a modified maleimide flame retardant.

[0046] (4) 1000 g of waterborne polyurethane, 30 g of modified maleimide flame retardant, 10 g of defoamer, 5 g of leveling agent, 100 g of titanium dioxide pigment, 5 g of dispersant, and 1200 g of water were stirred and dispersed in a high-speed disperser to obtain a fire-resistant waterborne coating containing modified maleimide.

[0047] Example 3

[0048] (1) Prepare the bismaleimide intermediate according to the method of Example 1.

[0049] (2) Prepare the dibenzyl mercaptan phosphate intermediate according to the method of Example 1.

[0050] (3) In nitrogen, 20 g of bismaleimide intermediate, 17.4 g of bisbenzyl mercaptan phosphate intermediate, and 3.2 g of triethylamine were added to 400 mL of N,N-dimethylacetamide solvent, and the mixture was reacted at 15° C. for 2 h. The mixture was filtered, and the precipitate was washed with dichloromethane and dried to obtain a modified maleimide flame retardant.

[0051] (4) 1000 g of waterborne polyurethane, 30 g of modified maleimide flame retardant, 6 g of defoamer, 8 g of leveling agent, 100 g of pigment titanium dioxide, 5 g of dispersant, and 1200 g of water are stirred and dispersed in a high-speed disperser to obtain a fire-resistant waterborne coating containing modified maleimide.

[0052] Comparative Example 1

[0053] 1000 g of waterborne polyurethane, 30 g of modified maleimide flame retardant, 4 g of defoamer, 8 g of leveling agent, 100 g of pigment filler titanium dioxide, 15 g of dispersant, and 1200 g of water were stirred and dispersed in a high-speed disperser to obtain a waterborne coating.

[0054] Comparative Example 2

[0055] (1) Prepare the bismaleimide intermediate according to the method of Example 1.

[0056] (1) In nitrogen, 20 g (31.84 mmol) of bismaleimide intermediate and 5.56 g (32.70 mmol) of 1,4-benzenedimethanethiol (structural formula: ), 3.6 g of triethylamine, react at 30°C for 1 hour, filter, wash the precipitate with dichloromethane, and dry to obtain a modified maleimide flame retardant.

[0057] (2) 1000 g of waterborne polyurethane, 30 g of modified maleimide flame retardant, 4 g of defoamer, 8 g of leveling agent, 100 g of pigment titanium dioxide, 15 g of dispersant, and 1200 g of water are stirred and dispersed in a high-speed disperser to obtain a fire-resistant waterborne coating containing modified maleimide.

[0058] Comparative Example 3

[0059] (1) Prepare the bis-benzyl mercaptan phosphate intermediate according to the method of Example 1.

[0060] (2) In nitrogen, 8.53 g (31.84 mmol) of N,N'-(1,4-phenylene)bismaleimide (structural formula: ), 17.4 g (32.70 mmol) of bis-benzyl mercaptan phosphate intermediate, 3.6 g of triethylamine, react at 30° C. for 1 h, filter, wash the precipitate with dichloromethane, and dry to obtain a modified maleimide flame retardant.

[0061] (3) 1000 g of waterborne polyurethane, 30 g of modified maleimide flame retardant, 4 g of defoamer, 8 g of leveling agent, 100 g of pigment titanium dioxide, 15 g of dispersant, and 1200 g of water are stirred and dispersed in a high-speed disperser to obtain a fire-resistant waterborne coating containing modified maleimide.

[0062] The hardness and adhesion of water-based coatings were tested according to GB / T 6739-2022 and GB / T 9286-2021. The film curing temperature was 60°C and the curing time was 24 hours.

[0063] The water-based paint was poured into a glass mold and dried and cured at 70°C for 48 hours to form a film. The tensile properties of the film were tested according to GB / T1040.1-2018. The test results are as follows.

[0064]

[0065] As can be seen from the table above, the polyurethane water-based coating of Comparative Example 1 has a hardness of 2H, an adhesion of level 1, a tensile strength of 25.8 MPa, an elongation at break of 768.4%, a limiting oxygen index of 17.3%, no UL94 vertical combustion rating, and very poor fire resistance.

[0066] In Examples 1 to 3, a modified maleimide flame retardant is added, and its molecular backbone contains the same urethane structural unit as the polyurethane. Thus, the flame retardant and polyurethane have good compatibility, and the addition of the flame retardant will not affect the mechanical properties of the polyurethane. The flame retardant molecular chain contains a phenylmaleimide structure, which has high rigidity and strong structural stability. Compared with comparative example 1, the hardness and tensile strength of the polyurethanes in Examples 1 to 3 are significantly improved. And the modified maleimide flame retardant contains a spirocyclic phosphate phosphorus flame retardant group The nitrogen-containing heterocyclic ring of maleimide can form an expanding flame retardant system. When burning, the flame retardant spirocyclic phosphate acts as an acid source and a carbon source, and the nitrogen atoms such as the nitrogen-containing heterocyclic ring act as a gas source to form a foam expanding carbon layer on the surface of the polyurethane, which has the fire-resistant and flame-retardant effects of heat insulation, oxygen isolation, smoke suppression, etc., and improves the limiting oxygen index of the polyurethane, and the UL94 reaches V1 level.

[0067] Comparative Example 2: 1,4-benzenedimethanethiol polymerization reaction is carried out with bismaleimide intermediate, and the obtained modified maleimide flame retardant molecular chain contains the same carbamate structural unit as polyurethane, which has good compatibility with polyurethane and will not affect the mechanical properties of polyurethane. In addition, the flame retardant molecular chain contains a phenylmaleimide structure with high rigidity and strong structural stability, which significantly improves the hardness and tensile strength of polyurethane. However, the modified maleimide flame retardant does not contain spirocyclic phosphate phosphorus flame retardant groups, and cannot form an expansion flame retardant system, and has poor fire retardant effect on polyurethane. The limiting oxygen index is 18.1%, and UL94 vertical combustion has no grade.

[0068] Comparative Example 3: Polymerization reaction is carried out with N,N'-(1,4-phenylene) bismaleimide and bisbenzyl mercaptan phosphate intermediates. The obtained maleimide flame retardant molecular chain contains spirocyclic phosphate phosphorus-containing flame retardant groups and maleimide nitrogen-containing heterocycles, which can form an expansion flame retardant system, improve the limiting oxygen index of polyurethane, and reach UL94 V1 level. The fire retardant performance is good. However, the maleimide flame retardant molecular chain does not contain carbamate structural units, and the compatibility with polyurethane is poor, which has a great influence on the mechanical properties of polyurethane, reducing the hardness, tensile strength and adhesion.

[0069] Example 4

[0070] (1) 1000 g of waterborne polyurethane, 70 g of modified maleimide flame retardant, 6 g of defoamer, 8 g of leveling agent, 100 g of pigment titanium dioxide, 5 g of dispersant, and 1200 g of water are stirred and dispersed in a high-speed disperser to obtain a fire-resistant waterborne coating containing modified maleimide.

[0071] Example 5

[0072] (1) 1000 g of waterborne polyurethane, 100 g of modified maleimide flame retardant, 6 g of defoamer, 8 g of leveling agent, 100 g of pigment titanium dioxide, 5 g of dispersant, and 1200 g of water are stirred and dispersed in a high-speed disperser to obtain a fire-resistant waterborne coating containing modified maleimide.

[0073] Example 6

[0074] (1) 1000 g of waterborne polyurethane, 150 g of modified maleimide flame retardant, 6 g of defoamer, 8 g of leveling agent, 100 g of pigment titanium dioxide, 5 g of dispersant, and 1200 g of water are stirred and dispersed in a high-speed disperser to obtain a fire-resistant waterborne coating containing modified maleimide.

[0075] The hardness and adhesion of water-based coatings are tested according to GB / T 6739-2022 and GB / T 9286-2021 standards. The paint film curing temperature is 60°C and the time is 24h.

[0076] The water-based paint was poured into a glass mold and dried and cured at 70°C for 48 hours to form a film. The tensile properties of the film were tested according to the standard GB / T1040.1-2018. The test results are as follows.

[0077]

[0078] As can be seen from the above table, in Examples 1, 4 to 6, the amount of the modified maleimide flame retardant gradually increases, the limiting oxygen index becomes larger and larger, and UL94 reaches V0 grade. The fire retardant performance is excellent.

[0079] It should be noted that the above-mentioned specific implementation methods can enable those skilled in the art to understand the present invention more comprehensively, but do not limit the present invention in any way. Therefore, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents; and all technical solutions and improvements that do not deviate from the spirit and technical essence of the present invention should be included in the protection scope of the patent of the present invention.

Claims

1. A fire-resistant water-based coating containing modified maleimide, characterized in that: The fire-resistant water-based coating containing modified maleimide comprises 100 parts by weight of water-based polyurethane and 3-15 parts by weight of modified maleimide flame retardant; 0.4-1 parts by weight of defoamer, 0.5-0.8 parts by weight of leveling agent, 10-30 parts by weight of pigment and filler, 0.5-1.5 parts by weight of dispersant; The preparation method of the modified maleimide flame retardant comprises: adding a bismaleimide intermediate, a bisbenzyl mercaptan phosphate intermediate and triethylamine to an N,N-dimethylacetamide solvent in nitrogen, filtering after the reaction, washing the precipitate and drying to obtain the modified maleimide flame retardant; The bismaleimide intermediate has the following structural formula (I): The bisbenzyl mercaptan phosphate intermediate has the following structural formula (II):

2. The fire-resistant water-based coating containing modified maleimide according to claim 1, characterized in that: The usage of the bismaleimide intermediate is 100 parts by weight, the usage of the bisbenzyl mercaptan phosphate intermediate is 82-87 parts by weight, and the usage of triethylamine is 12-18 parts by weight.

3. The fire-resistant water-based coating containing modified maleimide according to claim 1, characterized in that: The reaction is carried out at 15-30°C for 1-2 h.

4. The fire-resistant water-based coating containing modified maleimide according to claim 2, characterized in that: The preparation method of the bismaleimide intermediate comprises the following steps: adding diphenylmethane-4,4'-diisocyanate and N-(4-hydroxyphenyl)maleimide to a toluene solvent, concentrating the solution after the reaction, washing the precipitate, and recrystallizing to obtain the bismaleimide intermediate.

5. The fire-resistant water-based coating containing modified maleimide according to claim 4, characterized in that: The amount of diphenylmethane-4,4'-diisocyanate used is 100 parts by weight, and the amount of N-(4-hydroxyphenyl)maleimide is 152-165 parts by weight.

6. The fire-resistant water-based coating containing modified maleimide according to claim 4, characterized in that: In the method for preparing the bismaleimide intermediate, the reaction is carried out at 60-80° C. for 2-4 hours.

7. The fire-resistant water-based coating containing modified maleimide according to claim 4, characterized in that: The preparation method of the bis-benzyl mercaptan phosphate intermediate is: (1) adding 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, 4-bromomethylbenzyl alcohol and triethylamine to an acetonitrile solvent, concentrating the solution after the reaction, washing the precipitate and drying it to obtain an intermediate A; (2) Add 100 parts by weight of intermediate A, 62-72 parts by weight of thioacetic acid, and 84-92 parts by weight of potassium carbonate to a methanol solvent, react at 20-30° C. for 30-60 minutes, then add 84-92 parts by weight of potassium carbonate, continue the reaction for 1-2 hours, add hydrochloric acid solution to neutralize the reaction solution, concentrate the solution, wash the precipitate, and dry it to obtain a bisbenzyl mercaptan phosphate intermediate.

8. The fire-resistant water-based coating containing modified maleimide according to claim 7, characterized in that: In the above (1), the amount of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide is 100 parts by weight, the amount of 4-bromomethylbenzyl alcohol is 155-170 parts by weight, and the amount of triethylamine is 70-78 parts by weight.

9. The fire-resistant water-based coating containing modified maleimide according to claim 7, characterized in that: In the step (1), the reaction is first carried out at 10-15°C for 30-60 min, and then at 65-75°C for 4-6 h.

10. A method for preparing a fire-resistant water-based coating containing modified maleimide according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: stirring and dispersing waterborne polyurethane, modified maleimide flame retardant, defoamer, leveling agent, pigment, filler, dispersant and water in a high-speed disperser to obtain fire-resistant waterborne coating containing modified maleimide.

Citation Information

Patent Citations

  • Self-healing flame-retardant polyurethane elastomer containing Diels-Alder bonds and its preparation method

    CN108440735B

  • Flame retardant containing silicon and spiro pentaerythritol amyl phosphonate and preparation method thereof

    CN102344583A

  • Swelling flame retardant and preparation method thereof

    CN103073725A

  • Nitrogen-phosphorus flame retardant containing carbamate structure and preparation method of flame retardant

    CN103641971A

  • High-temperature-resistant flame-retardant polyester fiber and preparation process thereof

    CN116770453A