Composite hot melt adhesive material and preparation method thereof

By using composite materials with components such as SEPS and SEBS in hot melt adhesives, the problem of insufficient bonding strength of hot melt adhesives in high and low temperature environments has been solved, and its high and low temperature resistance and bonding strength have been improved, making it suitable for large-scale applications. Large-scale application and improved environmental performance.

CN118755409APending Publication Date: 2024-10-11SICHUAN UNISAI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202410992100.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing hot melt adhesives have poor bonding strength in high and low temperature environments, which affects their anti-aging ability and service life, and their reduced polarity results in poor bonding performance, limiting their large-scale application.

Method used

Composite hot melt adhesive material is used, which is composed of SEPS, SEBS, silane-modified amorphous α-olefin copolymer, hydrogenated C5 petroleum resin, pure monomer resin, Fischer-Tropsch wax and polar wax. Through synergistic effect, Improve the high and low temperature resistance and bonding strength of hot melt adhesive to avoid reduction in bonding strength.

Benefits of technology

It significantly improves the high and low temperature resistance and bonding strength of hot melt adhesive, enhances its adhesion and fluidity to the substrate, is suitable for large-scale applications, reduces the release of volatile oil, and improves environmental performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004959153470000061
    Figure BDA0004959153470000061
  • Figure BDA0004959153470000071
    Figure BDA0004959153470000071
  • Figure BDA0004959153470000072
    Figure BDA0004959153470000072
Patent Text Reader

Abstract

The invention discloses a composite hot melt adhesive material and a preparation method thereof, and belongs to the field of high polymer materials. The composite hot melt adhesive material is prepared from the following raw materials in parts by weight: 5 to 10 parts of SEPS, 15 to 20 parts of SEBS, 20 to 25 parts of polyolefin elastomer, 5 to 10 parts of silane modified amorphous alpha-olefin copolymer, 20 to 30 parts of hydrogenated C5 petroleum resin, 10 to 20 parts of pure monomer resin, 10 to 20 parts of Fischer-Tropsch wax, 1 to 5 parts of polar wax and 0.3 to 1 part of antioxidant. According to the composite hot melt adhesive material, the high and low temperature resistance of the hot melt adhesive is remarkably improved and the reduction of the bonding strength is avoided through the synergistic and matching effects of various components, so that the composite hot melt adhesive has excellent high and low temperature resistance and bonding strength, and the large-scale application of the hot melt adhesive is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polymer materials, in particular to the field of hot melt adhesive materials, and in particular to a composite hot melt adhesive material and a preparation method thereof. Background Art

[0002] Hot melt adhesive is a plastic adhesive. Within a certain temperature range, its physical state changes with temperature, while its chemical properties remain unchanged. It has the advantages of being non-toxic and odorless, fast bonding speed, simple production process, and easy to use. Therefore, it is widely used in food packaging, fast assembly line packaging and sealing, home appliance sealing, book binding and other industries.

[0003] The surface materials of mattresses are mainly cloth, sponge, natural latex, etc. Therefore, in the production process of mattresses, adhesives need to be used to fix the surface materials. In the early days, the adhesives used in mattress production were mostly water-based adhesives and solvent adhesives. However, with the improvement of people's environmental awareness, water-based adhesives and solvent adhesives have been gradually replaced by hot melt adhesives due to their strong odor, harm to the human body, and long bonding time.

[0004] At present, hot melt adhesives for mattresses are mostly made of polyolefin APAO, ethylene-vinyl acetate, polyester, polyamide and hot-melt resin, and have the advantages of good adhesion, controllable fluidity and fast curing speed. However, since the bonding process of hot melt adhesive is physical curing and reversible, it has poor anti-aging ability (easy to change color), and the bonding parts will be displaced and deformed at high temperatures after the glue is cured. In addition, there will be problems such as abnormal noise during the use of the mattress due to the easy stickiness of the glue at high temperatures, which seriously affects the quality of the mattress products. In order to improve the above-mentioned defects of hot melt adhesive, researchers have modified and optimized the hot melt adhesive.

[0005] Patent CN116694263A discloses a hot melt adhesive for mattress springs and a preparation method thereof. The hot melt adhesive is made of the following raw materials in parts by weight: 33 to 36 parts of tackifying resin, 12 to 18 parts of PB resin, 34 to 38 parts of polyolefin elastomer POE, and 14 to 16 parts of lubricating wax. Although the hot melt adhesive has good anti-aging and cold resistance, its high temperature resistance is still poor.

[0006] Patent CN106536662A discloses a hot melt adhesive composition, which is made of polypropylene copolymer or polypropylene impact copolymer, polyolefin elastomer, low-density polyethylene, tackifying resin, plasticizer, and nucleating agent; the viscosity and viscoelasticity of the hot melt adhesive composition are controllable, and the high and low temperature resistance is also improved, but the polarity of the entire system is very low, and the bonding strength (especially to polar surfaces and fabric surfaces) is poor.

[0007] Patent CN107459954A discloses a hot melt adhesive rich in thermoplastic elastomers, which is used to bond two or more styrene-based or polyolefin-based thermoplastic elastomer products; the adhesive is a mixture comprising styrene block copolymers, polyolefin block copolymers, mineral oil, tackifying resins, reinforcing resins and additives. Although the adhesive has the advantages of good high and low temperature resistance and fast curing speed due to the addition of a large amount of block copolymers, it also leads to poor fluidity and bonding strength of the adhesive, which is not conducive to rapid and continuous production and processing.

[0008] It can be seen that although the high and low temperature resistance of hot melt adhesives have been modified and optimized by adding block copolymers or elastomers in the prior art, so that the hot melt adhesive has better high and low temperature resistance, it also leads to a decrease in the polarity of the hot melt adhesive and a decrease in the bonding strength, which is not conducive to the large-scale application of hot melt adhesives. Summary of the invention

[0009] The purpose of the present invention is to overcome the problem of poor bonding strength of existing high and low temperature resistant hot melt adhesives, and propose a composite hot melt adhesive material and a preparation method thereof.

[0010] In order to achieve the above-mentioned purpose of the invention, the present invention provides a composite hot melt adhesive material, which is prepared by the following raw materials in parts by weight: 5 to 10 parts of SEPS, 15 to 20 parts of SEBS, 20 to 25 parts of polyolefin elastomer (POE), 5 to 10 parts of silane-modified amorphous α-olefin copolymer (APAO), 20 to 30 parts of hydrogenated C5 petroleum resin, 10 to 20 parts of pure monomer resin, 10-20 parts of Fischer-Tropsch wax, 1-5 parts of polar wax, and 0.3 to 1 part of antioxidant.

[0011] The composite hot melt adhesive material of the present invention not only significantly improves the high and low temperature resistance of the hot melt adhesive by adding SEPS and SEBS; but also significantly improves the influence of the hot melt adhesive fluidity and bonding strength being greatly reduced due to the introduction of the rubber segment and the styrene segment by adding silane-modified APAO, hydrogenated C5 petroleum resin and polyolefin elastomer POE which have excellent solubility in the rubber segment in SEPS and SEBS, and pure monomer resin which has good solubility in the styrene segment in SEPS and SEBS; at the same time, polar wax is added to the system to improve the thermal conductivity of the hot melt adhesive. The non-polar segments and polar segments are solubilized, thereby promoting the synergistic effect of SEPS and SEBS under melting conditions, so that the two can further improve their adverse effects on the bonding strength of the hot melt adhesive without affecting their improvement of the high and low temperature resistance of the hot melt adhesive; the composite hot melt adhesive material, through the synergistic and coordinated effect between multiple components, significantly improves the high and low temperature resistance of the hot melt adhesive while avoiding the reduction of bonding strength, so that the composite hot melt adhesive has excellent high and low temperature resistance and bonding strength at the same time, which is more conducive to the large-scale application of hot melt adhesive.

[0012] Among them, SEPS is a special linear SIS that is hydrogenated to convert the polyisoprene in the molecular chain into a thermoplastic elastomer of polyethylene and polypropylene segments. SEPS has excellent low temperature resistance. Therefore, the addition of SEPS can significantly improve the low temperature resistance of the hot melt adhesive, but the introduction of the rubber segment will also lead to a decrease in the fluidity of the hot melt adhesive and a decrease in the bonding strength; preferably, in the molecular chain of the SEPS, the molar percentage ratio of the styrene segment (S) to the rubber segment (EP) is 20-40:80-60, and the molar percentage of the diblock (rubber segment) is 85-100%; the preferred SEPS block parameters, SEPS has better flexibility, while ensuring that the hot melt adhesive has excellent low temperature resistance, the bonding strength of the hot melt adhesive is also significantly improved, and more preferably, at 25°C, the viscosity of the toluene solution of SEPS with a mass fraction of 15% is <300mpa.s; the preferred SEPS viscosity, the hot melt adhesive has better fluidity and is easy to use.

[0013] Among them, SEBS is a special linear SBS that is hydrogenated to convert the polybutadiene segments in the molecular chain into a thermoplastic elastomer of polyethylene and polybutylene segments. SEBS has excellent oil absorption and cohesive strength. Therefore, the addition of SEBS can significantly improve the high temperature resistance of the hot melt adhesive, but similarly, the introduction of the rubber segment will also lead to a decrease in the fluidity of the hot melt adhesive and a decrease in the bonding strength; preferably, in the molecular chain of the SEBS, the molar percentage ratio of the styrene segment (S) to the rubber segment (EB) is 20-30:80-70; the preferred SEBS has better oil absorption and cohesive strength, ensuring that the hot melt adhesive has better high temperature resistance, while significantly reducing the influence of SEBS on the bonding strength of the hot melt adhesive; more preferably, the melt index of the SEBS at 190°C and 2.16kg is 50-200g / 10min; the preferred SEBS melt index, the hot melt adhesive has better fluidity and high temperature resistance.

[0014] Among them, the polyolefin elastomer can be miscible with the rubber segments in SEPS and SEBS at high temperature to form a homogeneous transparent solution, thereby significantly improving the wettability of the hot melt adhesive, which is beneficial to improving the initial viscosity of the hot melt adhesive; preferably, the polyolefin elastomer is an ethylene and octene copolymer, and the melt index under 190°C and 2.16kg conditions is 500-1200g / 10min; the preferred polyolefin elastomer can better dissolve with the SEPS and SEBS rubber segments, thereby improving the wettability of the hot melt adhesive, and the bonding strength of the hot melt adhesive is significantly improved.

[0015] Among them, silane-modified APAO is formed by grafting active silane groups on the molecular chain of APAO; the silane groups in silane-modified APAO can form chemical bonds with higher bond energy with the surface of the substrate, thereby improving the adhesion of the hot melt adhesive and significantly improving the bonding strength of the hot melt adhesive; but the greater the amount of silane grafting, the higher the degree of cross-linking of the hot melt adhesive system, the greater the cold brittleness, which seriously affects the low-temperature resistance of the hot melt adhesive; preferably, in the silane-modified APAO, the mass percentage of silane is 1.0-2.5%; more preferably, the mass percentage of silane is 1.5-2.5%. The preferred silane content ensures that the hot melt adhesive has excellent adhesion while also having a lower softening point and better fluidity, which is easy to use.

[0016] Preferably, the softening point of the silane-modified APAO is 95-105° C., and the viscosity at 180° C. is 5000-15000 mPa.s. The preferred silane-modified APAO has better fluidity of the hot melt adhesive and is more conducive to the use of the hot melt adhesive.

[0017] Among them, hydrogenated C5 petroleum resin has a thickening effect, which can improve the fluidity and wettability of the rubber segment, polyolefin elastomer (POE) and silane-modified APAO in the molten SEBS and SEPS, thereby helping to improve the bonding strength of the hot melt adhesive; preferably, the softening point of the hydrogenated C5 petroleum resin is 90-110°C; the preferred hydrogenated C5 petroleum resin has a better thickening effect on the non-polar segments in the hot melt adhesive system, making the system have better fluidity and wettability.

[0018] Preferably, the hydrogenated C5 petroleum resin is fully hydrogenated C5 petroleum resin; fully hydrogenated C5 petroleum resin has lower polarity and better high temperature aging resistance.

[0019] Among them, the pure monomer resin can dissolve the styrene block in the system, thereby effectively reducing the viscosity of the system and improving the high temperature resistance of the system; the pure monomer resin is a hydrogenated poly-α-methylstyrene resin with a softening point of 90-110°C; preferably, the softening point of the hydrogenated poly-α-methylstyrene resin is 95-105°C, and the viscosity at 160°C is 1000-2000mPa.s; the preferred monomer resin has better solubility for styrene in the rubber segment in the system, better fluidity of the hot melt adhesive, and better high temperature resistance.

[0020] Among them, Fischer-Tropsch wax can increase the fluidity and curing speed of the hot melt adhesive, which is conducive to rapid and continuous production and processing; preferably, the softening point of the Fischer-Tropsch wax is 60-100°C; more preferably, the softening point of the Fischer-Tropsch wax is 65-85°C; the preferred Fischer-Tropsch wax can better soften SEBS and SEPS, so that the SEPS and SEBS molecular chains dissolve more evenly under the stirring action of external force, and the fluidity and wettability of the hot melt adhesive are better.

[0021] Among them, the polar wax is a wax with a strong polar group grafted next to a straight-chain alkane, and the polar group contained in it can form hydrogen bonds with the surface of the substrate, thereby significantly improving the initial adhesion and lasting adhesion of the hot melt adhesive; preferably, the polar wax includes at least one of oxidized polyethylene wax, ethylene-acrylic acid copolymer wax, and ethylene-vinyl acetate copolymer wax; more preferably, the softening point of the polar wax is 95-105°C; most preferably, the viscosity of the polar wax at 160°C is 500-2000mPa.s; the preferred polar wax can more effectively solubilize the styrene segment and non-polar molecular chain in the system, can better form hydrogen bonds with the surface of the substrate, and the bonding strength of the hot melt adhesive is better.

[0022] Among them, the antioxidant can improve the antioxidant performance of the hot melt adhesive; preferably, the antioxidant is antioxidant 1010 and antioxidant 168; the preferred antioxidant has good antioxidant performance and is pollution-free.

[0023] In order to achieve the above-mentioned object of the invention, the present invention further provides a method for preparing a composite hot melt adhesive material, comprising the following steps:

[0024] S1. Under nitrogen protection, Fischer-Tropsch wax, pure monomer resin, SEBS, SEPS, antioxidant, silane-modified APAO, and hydrogenated C5 resin are mixed, stirred, and melted to obtain a mixed melt A;

[0025] S2, subjecting the mixed melt A to vacuum treatment to obtain a mixed melt B;

[0026] S3, sieving the mixed melt B to obtain a composite hot melt adhesive material.

[0027] Among them, in step S2, the vacuum treatment is to place the mixed melt A in a negative pressure environment so that the low-boiling point impurities in the melt can be volatilized, thereby avoiding the hot melt adhesive from generating harmful gases during use and improving the environmental friendliness of the hot melt adhesive; preferably, the vacuum treatment temperature is 100 to 120°C, the vacuum pressure is -0.05 to -0.08Mpa, and the time is 30 to 40 minutes.

[0028] Among them, in step S3, the mixed melt B is sieved to remove infusible substances in the melt and increase the fluidity and adhesion of the hot melt adhesive; preferably, the aperture of the sieve is 200-400 mesh.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The composite hot melt adhesive material of the present invention significantly improves the high and low temperature resistance of the hot melt adhesive by adding SEPS and SEBS.

[0031] 2. The composite hot melt adhesive material of the present invention significantly improves the effect of greatly reduced hot melt adhesive fluidity and bonding strength caused by the introduction of rubber segments and styrene segments by adding silane-modified APAO, hydrogenated C5 petroleum resin and polyolefin elastomer POE that have excellent solubility in the rubber segments in SEPS and SEBS, as well as pure monomer resin that has good solubility in the styrene segments in SEPS and SEBS. The composite hot melt adhesive material can quickly penetrate into the pores on the surface of the substrate to form good physical bonding, thereby significantly improving the bonding strength of the hot melt adhesive.

[0032] 3. The composite hot melt adhesive material of the present invention solubilizes the non-polar segments and polar segments in the system by adding polar wax, thereby promoting the synergistic effect of SEPS and SEBS under melting conditions, so that the two can further improve their adverse effects on the bonding strength of the hot melt adhesive without affecting their improvement of the high and low temperature resistance of the hot melt adhesive.

[0033] 4. The composite hot melt adhesive material of the present invention adds Fischer-Tropsch wax and utilizes the high oil absorption of SEBS to enable the Fischer-Tropsch wax to be better compounded with SEBS. Not only can the low molecular weight compounds in the Fischer-Tropsch wax be better utilized to soften the molten SEBS, but the low penetration and high crystallinity of the Fischer-Tropsch wax can also be better utilized to enhance the strength of the rubber, thereby significantly improving the high temperature resistance and curing speed of the hot melt adhesive.

[0034] 5. The composite hot melt adhesive material of the present invention utilizes the synergistic effect between the active oxygen atoms in the polar wax and the active silicon atoms in the silane modification by introducing polar wax and silane-modified APAO, so that the hot melt adhesive can chemically react with the surface of the substrate to form a stronger chemical bond, with better initial adhesion and lasting adhesion, thereby significantly improving the bonding strength of the hot melt adhesive (chemical viscosity enhancement).

[0035] 6. The composite hot melt adhesive material of the present invention significantly improves the high and low temperature resistance of the hot melt adhesive through the synergistic and coordinated effects of various components, while avoiding the reduction of bonding strength. As a result, the composite hot melt adhesive has excellent high and low temperature resistance and bonding strength, which is more conducive to the large-scale application of hot melt adhesive.

[0036] 7. The composite hot melt adhesive material of the present invention contains no volatile oil and plasticizer, and compared with the existing rubber hot melt adhesive, the release of VOC is significantly reduced, and the environmental protection performance is excellent.

[0037] 8. The preparation method of the composite hot melt adhesive material of the present invention has simple process, controllable performance, good stability, and is suitable for large-scale production of composite hot melt adhesive materials. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with test examples and specific implementation methods. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following embodiments, and all technologies realized based on the content of the present invention belong to the scope of the present invention.

[0039] Example 1

[0040] The raw materials mentioned in this embodiment can be purchased from the market, and the specific product information is as follows:

[0041] SEPS: The molar percentage ratio of the styrene segment to the rubber segment is 30:70, and the molar percentage of the diblock segment is 100%;

[0042] SEBS: The molar percentage ratio of styrene segment to rubber segment is 25:75;

[0043] POE: ethylene-octene copolymer, with a melt index of 760 g / 10 min at 190°C and 2.16 kg;

[0044] Silane-modified APAO: the mass percentage of silane is 1.5%;

[0045] Hydrogenated C5 petroleum resin: fully hydrogenated C5 petroleum resin, softening point is 100℃;

[0046] Pure monomer resin: hydrogenated poly-α-methylstyrene resin, softening point is 100°C, viscosity at 160°C is 1350mpa.s;

[0047] Fischer-Tropsch wax: softening point is 85°C;

[0048] Polar wax: ethylene-acrylic acid copolymer wax, softening point is 100°C;

[0049] Antioxidant: Antioxidant 1010.

[0050] A method for preparing a composite hot melt adhesive material comprises the following steps:

[0051] S1, mixing and stirring Fischer-Tropsch wax, pure monomer resin, SEBS, SEPS, antioxidant, and hydrogenated C5 resin for melting treatment to obtain a mixed melt A;

[0052] S2, subjecting the mixed melt A to vacuum treatment (the vacuum treatment temperature is 110° C., the vacuum pressure is -0.07 MPa, and the time is 35 min) to obtain a mixed melt B;

[0053] S3, sieving the mixed melt B (300 meshes) to obtain a composite hot melt adhesive material.

[0054] In this embodiment, the raw material types of the composite hot melt adhesive material are controlled to remain unchanged, and only the weight ratio of the raw materials is adjusted, and the above-mentioned preparation method is used for preparation. The specific weight ratio of the raw materials is shown in Table 1:

[0055] Table 1 Weight distribution ratio of raw materials in each experimental group in Example 1

[0056]

[0057]

[0058] Performance testing:

[0059] The composite hot melt adhesive material prepared according to the weight proportion of the raw materials in Table 1 in the above Example 1 was sampled according to the requirements of the relevant test methods. After the sample preparation was completed, the sample was placed in a constant temperature and humidity chamber at a temperature of 25°C and a humidity of 85% for maintenance for 48 hours, and then the bonding strength (peel strength) (YBB00102003-2015, the bonding substrate is aluminum foil), high temperature resistance (testing method: 1. Prepare the hot melt adhesive into a standard sample strip according to the national standard GB / T 1701-2001; 2. Then hang a 1Kg weight on one end of the standard sample strip, put it in an 85°C adhesion test oven for baking, and test the time for the adhesive strip to break at 95°C, which is limited to 24 hours. If there is no breakage after 24 hours, it is recorded as no breakage), and low temperature resistance test.

[0060] (GB / T1682—2014), the test results are shown in Table 2:

[0061] Table 2 Performance test results of each experimental group in Example 1

[0062]

[0063]

[0064] Analysis of the test results shows that:

[0065] From the experimental groups 1-1 to 1-5, it can be seen that the amount of SEPS added has a significant effect on the low-temperature brittle temperature and bonding strength of the hot melt adhesive system. As the content of SEPS increases, the low-temperature resistance of the hot melt adhesive increases rapidly, which is mainly due to the use of the second The rubber segment of the SEPS can move freely, which can effectively increase the free volume of the polymer chain segment, thereby improving the low temperature resistance of the adhesive. At the same time, with the excessive addition of SEPS, the bonding strength of the hot melt adhesive system becomes significantly lower. When the dosage exceeds 10 parts, the high temperature resistance of the hot melt adhesive is significantly reduced.

[0066] Comparing the experimental groups 1-6 to 1-9 and 1-3, it can be seen that the amount of SEBS has a significant effect on the high temperature resistance and bonding strength of the hot melt adhesive. When the amount reaches 15 parts, its high temperature resistance increases rapidly. When the SEBS content is small, increasing SEBS can also increase the low temperature resistance of the system. This is mainly because the rubber segment contained in SEBS can effectively lock the small and medium molecules in the system, thereby preventing the small molecules from being arranged and crystallized in an orderly manner, and improving the toughness of the system. When the amount of SEBS reaches 25 parts or more, the high hardness and brittleness of the plastic segment (S segment) in SEBS reduces the low temperature resistance of the system.

[0067] Comparing 1-10 to 1-13 and 1-3, it can be seen that within a certain range, the amount of POE has a significant effect on the high and low temperature resistance of the hot melt adhesive system. This is mainly due to the increase in the POE content. The small molecular weight POE in the system is completely miscible with the rubber segments in SEBS and SEPS, allowing the rubber segments in the system to stretch freely in the system, thereby increasing the high and low temperature resistance of the system. At the same time, with the increase in the POE content, the wettability of the adhesive has been greatly improved, and the adhesive bonding strength has been slightly improved, but the proportion of POE in the hot melt adhesive system is too large, which will significantly reduce the high and low temperature resistance and bonding of the hot melt adhesive.

[0068] Comparing the experimental groups 1-14 to 1-18 and 1-3, it can be seen that the content of silane-grafted APAO has a crucial influence on the bonding strength of the system. Without the addition of modified APAO, the bonding strength is only 3.86N / mm 2 . This is mainly because the hot melt adhesive of the present invention is a reactive hot melt adhesive. During the curing and bonding process, as water molecules enter the environment, they can undergo a cross-linking reaction with the active silane in the hot melt adhesive and form a chemical bond with the surface of the adhesive, thereby greatly improving the bonding performance of the hot melt adhesive. At the same time, as the content increases, the grafting points gradually increase, the strength and high temperature resistance of the adhesive increase rapidly, but the cold brittleness of the hot melt adhesive increases sharply. This is mainly because the cross-linking points in the system lock the rubber segments of SEPS and SEBS, the activity of the molecular chain segments becomes weak, and the low temperature resistance decreases rapidly.

[0069] By comparing experimental groups 1-19 to 1-22 and 1-3, it can be seen that polar wax can significantly improve the bonding strength of hot melt adhesive. This is mainly because the introduction of polar wax can enhance the melting of various components in the system, thereby making it difficult for polymer segments to precipitate at low temperatures. At the same time, the polar groups of the polar wax and the active silane groups synergistically increase the adhesion between the system and the bonded surface. However, the addition of excessive polar wax causes it to account for too large a proportion in the hot melt adhesive system, which will significantly reduce the high and low temperature resistance of the hot melt adhesive.

[0070] Example 2

[0071] In this embodiment, the weight proportions of the raw materials of the composite hot melt adhesive material are controlled to remain unchanged (according to the weight proportions of groups 1-3 in Example 1), only the performance parameters of a single raw material are adjusted, and the preparation is carried out by the same preparation method as in Example 1. The specific raw material performance data are shown in Table 3: The product ratio is based on the ratios in Examples 1-3.

[0072] Table 3 Performance parameters of raw materials in each experimental group in Example 2

[0073]

[0074]

[0075] Performance testing:

[0076] The composite hot melt adhesive material prepared according to the weight proportion of the raw materials in Table 3 in the above Example 2 was sampled according to the requirements of the relevant test method. After the sample preparation was completed, the sample was placed in a constant temperature and humidity chamber at a temperature of 25°C and a humidity of 85% for maintenance for 48 hours, and then the bonding strength (peel strength) (YBB00102003-2015, the bonding substrate is aluminum foil), high temperature resistance (see Example 1 for the detection method), low temperature resistance test (GB / T1682-2014), fluidity (GB / T 2794-2022), and adhesive transparency (detection method: weigh 40g of the hot melt adhesive and put it into a 50ml beaker, put it into an oven at 160°C for 4 hours to completely melt, and observe whether the adhesive is transparent). The test results are shown in Table 4:

[0077] Table 4 Performance test results of each experimental group in Example 2

[0078]

[0079]

[0080] Analysis of the test results shows that:

[0081] Comparative Examples 2-1 to 2-4 and 1-3 show that the content of the S segment in SEBS has a significant effect on the high and low temperature resistance, bonding strength and transparency of the hot melt adhesive. As the S segment increases, the viscosity of the hot melt adhesive gradually increases, the transparency of the adhesive solution deteriorates, and the high temperature resistance of the hot melt adhesive is significantly enhanced. This is because the S segment in SEBS has poor compatibility with POE and hydrogenated carbon five resin in the system. When the S segment is greater than 30%, despite the solubilization of hydrogenated monomer resin and polar wax, the system compatibility is still poor and becomes turbid, and the low temperature resistance of the hot melt adhesive deteriorates, and the cold brittleness becomes more obvious. When the S segment is less than 20%, there are too few rigid embedding points in the system, resulting in an enhanced ability of the molecular chain to move freely and poor high temperature resistance.

[0082] From the comparative examples 2-5 to 2-8 and 1-3, it can be seen that the diblock content in SEPS has a significant effect on the bonding strength, viscosity and high and low temperature resistance of the hot melt adhesive; with the increase of the diblock content in SEPS, the viscosity of the hot melt adhesive system decreases rapidly. This is mainly because both ends of the rubber in SEPS are restricted by the S segment, which makes it extremely difficult for its molecules to move, thereby increasing the viscosity of the system. At the same time, due to the difficulty in molecular movement, the free volume becomes smaller, and thus the compatibility of the system deteriorates rapidly. With the increase of the diblock, the uniformity of the system increases rapidly, the adhesive solution becomes clear and transparent from turbid, and the low temperature resistance is also rapidly improved. When the diblock reaches 85%, the viscosity and low temperature resistance of the hot melt adhesive meet the performance requirements. Although the subsequent increase in the diblock content reduces the high temperature resistance of the hot melt adhesive, the reduction is small, and the high temperature resistance of the hot melt adhesive is still good.

[0083] Comparative Examples 2-9 to 2-12 and 1-3 show that the content of the S segment in SEPS has a significant effect on the high and low temperature resistance, bonding strength and transparency of the hot melt adhesive. As the S segment increases, the viscosity of the hot melt adhesive gradually increases, the transparency of the adhesive liquid deteriorates, and the high temperature resistance of the hot melt adhesive is significantly enhanced. This is because the S segment in SEPS has poor compatibility with POE and hydrogenated carbon five resin in the system. When the S segment is greater than 40%, despite the solubilization of hydrogenated monomer fat and polar wax, the system compatibility is still poor and becomes turbid, and the low temperature resistance of the hot melt adhesive deteriorates, and the cold brittleness becomes more obvious. When the S segment is less than 20%, there are too few rigid embedding points in the system, resulting in an enhanced ability of the molecular chain to move freely and poor high temperature resistance.

[0084] Comparative Examples 2-13 to 2-17 and 1-3 show that the mass fraction of silane in silane-modified APAO significantly affects the bonding strength and high and low temperature resistance of the hot melt adhesive. When the mass fraction of modified silane is lower than 0.5%, the bonding strength of the hot melt adhesive is significantly reduced. This is mainly because the silane content is too low, the cross-linking points of moisture curing are reduced, resulting in lower strength of the colloid and less chemical bonding between the colloid and the surface of the object being tested, resulting in reduced bonding strength. When the mass fraction of silane is greater than 3.5%, its low temperature resistance decreases rapidly. This is mainly because there are too many cross-linking points in the system, which restricts the movement of the hot melt adhesive molecules at low temperatures, resulting in brittle fracture at low temperatures; at the same time, the excessive silane has poor compatibility with the non-polar segments in the system, resulting in poor transparency of the adhesive.

[0085] Comparative Examples 2-18 to 2-21 and 1-3 show that the softening point of the polar wax has a great influence on the bonding strength and high and low temperature resistance of the hot melt adhesive. As the softening point of the polar wax increases, the low temperature resistance of the hot melt adhesive deteriorates, and the high temperature resistance increases rapidly. As the softening point increases, the molecular weight of the wax increases, and the compatibility with SEBS and SEPS deteriorates, resulting in a certain degree of reduction in the overall performance of the hot melt adhesive system.

Claims

1. A composite hot melt adhesive material, characterized in that: The invention is prepared by the following raw materials in parts by weight: 5 to 10 parts of SEPS, 15 to 20 parts of SEBS, 20 to 25 parts of polyolefin elastomer, 5 to 10 parts of silane-modified amorphous α-olefin copolymer, 20 to 30 parts of hydrogenated C5 petroleum resin, 10 to 20 parts of pure monomer resin, 10 to 20 parts of Fischer-Tropsch wax, 1 to 5 parts of polar wax, and 0.3 to 1 part of antioxidant; In the molecular chain of the SEPS, the molar percentage ratio of the styrene segment to the rubber segment is 20-40:80-60, and the molar percentage of the diblock segment is 85-100%; In the molecular chain of the SEBS, the molar percentage ratio of the styrene segment to the rubber segment is 20-30:80-70; In the silane-modified APAO, the mass percentage content of silane is 1.0-2.5%.

2. The composite hot melt adhesive material according to claim 1, characterized in that: The viscosity of the toluene solution of the SEPS with a mass fraction of 15% at 25° C. is less than 300 mPa.s; and / or the melt index of the SEBS at 190° C. and 2.16 kg is 50-200 g / 10 min.

3. The composite hot melt adhesive material according to claim 1, characterized in that: The polyolefin elastomer is a copolymer of ethylene and octene, and has a melt index of 500-1200 g / 10 min at 190° C. and 2.16 kg.

4. The composite hot melt adhesive material according to claim 1, characterized in that: The softening point of the hydrogenated C5 petroleum resin is 90-110°C.

5. The composite hot melt adhesive material according to claim 1, characterized in that: The softening point of the silane-modified APAO is 95-105° C., and the viscosity at 180° C. is 5000-15000 mPa.s.

6. The composite hot melt adhesive material according to claim 1, characterized in that: The pure monomer resin is a hydrogenated poly-α-methylstyrene resin having a softening point of 90-110°C.

7. The composite hot melt adhesive material according to claim 1, characterized in that: The softening point of the Fischer-Tropsch wax is 60-100°C.

8. The composite hot melt adhesive material according to claim 1, characterized in that: The polar wax includes at least one of oxidized polyethylene wax, ethylene-acrylic acid copolymer wax, and ethylene-vinyl acetate copolymer wax.

9. The composite hot melt adhesive material according to claim 8, characterized in that: The softening point of the polar wax is 95-105°C.

10. A method for preparing the composite hot melt adhesive material according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Under nitrogen protection, Fischer-Tropsch wax, pure monomer resin, SEBS, SEPS, antioxidant, and hydrogenated C5 resin are mixed, stirred, and melted to obtain a mixed melt A; S2, subjecting the mixed melt A to vacuum treatment to obtain a mixed melt B; S3, sieving the mixed melt B to obtain a composite hot melt adhesive material.

Citation Information

Cited By

  • Preparation method and application of washing-resistant, temperature-change-resistant and fast-curing hot melt adhesive

    CN119161837A

  • Thermoplastic elastomer composite material as well as preparation method and application thereof

    CN120137340A

  • Thermoplastic elastomer composite material, method for preparing same, and use thereof

    CN120137340B

  • Adhesive resin for A2-grade aluminum-plastic panel fireproof core material, hot melt adhesive film and aluminum-plastic panel

    CN122146193A

  • A2 grade aluminum plastic plate fireproof core material with adhesive resin, hot melt adhesive film and aluminum plastic plate