Dry water supported hydrotalcite powder explosion suppressant

Through the preparation of dry water-loaded hydrotalcite powder explosion suppressant, intercalation modifiers are used to improve the dispersion and adsorption properties of hydrotalcite to form a core-shell structure, which solves the problem of poor performance of traditional powder explosion suppressants. Efficient methane explosion suppression effect is achieved.

CN118774928APending Publication Date: 2024-10-15CHANGZHOU UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411127399.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Traditional powder explosion suppressors have poor explosion suppression performance and have problems such as high cost, poor dispersibility, easy deliquescence and agglomeration, and large consumption. There are also few studies on the collaborative explosion suppression of composite explosion suppressants.

Method used

Dry water-loaded hydrotalcite powder explosion suppressant is used, by crushing and grinding the massive hydrotalcite, adding N,N-dimethylformamide for intercalation modification, and combining it with nano-silica and silicone oil. Dry water-loaded powder forming a core-shell structure improves its explosion suppression effect in methane explosions.

Benefits of technology

The explosion suppression effect is achieved with low material cost, high performance and good stability. The intercalation modifier significantly improves the dispersion and adsorption performance of hydrotalcite, blocks heat and captures free radicals, delays the explosion reaction, and improves the explosion suppression effect. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118774928A_ABST
    Figure CN118774928A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of powder explosion suppressants, in particular to a dry water supported hydrotalcite powder explosion suppressant and a preparation method thereof. A traditional powder explosion suppressant is poor in explosion suppression performance. In order to solve the problems, the invention provides the dry-water-loaded hydrotalcite powder explosion suppressant, the obtained dry-water-loaded hydrotalcite powder explosion suppressant is formed by performing intercalation modification on hydrotalcite by adopting N, N-dimethylformamide and then loading the hydrotalcite on the surface of a dry-water carrier, and when the dry-water-loaded hydrotalcite powder explosion suppressant is impacted by high temperature and high pressure, the dry-water-loaded hydrotalcite powder explosion suppressant can be used for preparing the dry-water-loaded hydrotalcite powder explosion suppressant. The obtained dry-water supported hydrotalcite powder explosion suppressant can be involved in flames and decomposed into fine multi-component particles, intercalation modified hydrotalcite particles can be separated from the surface of a dry-water carrier and put into an explosion reaction, and when the intercalation modified hydrotalcite particles and the dry-water carrier explode, the intercalation modified hydrotalcite particles and the dry-water carrier can cooperatively absorb heat and continuously cool, so that the explosion suppressant is formed. The temperature in the reaction area is reduced, a large amount of water vapor and inert gas can be released, and the substances can dilute the content of the reaction gas, prevent the free radical chain reaction from continuing, dilute or remove toxic and harmful or greenhouse gas generated in the explosion process, prevent poisoning and pollution and improve the safety of the reaction. And the explosion suppression effect is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder explosion suppressants, and in particular to a dry water-loaded hydrotalcite powder explosion suppressant and a preparation method thereof. Background Art

[0002] Methane is a common gaseous fuel and an important component of natural gas. Due to the greenhouse effect and excessive consumption of mineral resources, methane is a gas that does not have much impact on the environment. However, there are major safety hazards in gas mining, transportation, and use. Once gas is mixed with air, it can easily cause an explosion, leading to major accidents in the fields of coal mine gas and civil natural gas, posing a great threat to people's lives and property. Therefore, it is of great research significance to develop an efficient explosion suppressant that can suppress methane-air explosions.

[0003] In recent years, people have conducted in-depth research on different types of explosion suppressants. Explosion suppressants for suppressing methane explosions are divided into inert gas explosion suppressants, water mist explosion suppressants, porous material explosion suppressants and powder explosion suppressants. Among the various explosion suppressants, powder explosion suppressants have become a popular explosion suppressant due to their low price, convenient transportation, easy storage and ability to adapt to complex environments. The explosion suppressant powder materials that have been studied more in the past mainly include CaCO3, NaHCO3, Mg(OH)2, Al(OH)3, NaCl, KCl, KH2PO4 and SiO2. However, these traditional powder explosion suppressants have technical problems such as low explosion suppression performance, difficulty in obtaining materials, poor dispersibility and suspension, easy deliquesce and agglomeration, and high consumption. In recent years, the research on composite powders with synergistic explosion suppression effects in methane explosions has attracted much attention from scholars.

[0004] As an alkali metal aluminosilicate mineral, hydrotalcite is mainly composed of magnesium silicate and silicon dioxide. It can be seen that hydrotalcite contains a large amount of explosion-suppressing ingredients. In addition, the internal structure of hydrotalcite is similar to that of kaolinite, mainly an irregular layered structure. These layered structures have good barrier and adsorption properties, and can effectively block heat and adsorb free radicals in the gas phase. At present, hydrotalcite is widely used in flame retardant, fire extinguishing, petroleum processing and other fields due to its low price, convenient material acquisition, and green environmental protection. However, there are few studies on using hydrotalcite as an explosion suppressant for methane explosions.

[0005] Dry water is a new type of drying technology. It uses a special adsorbent to adsorb water molecules on the surface, so that the water molecules form a crystal state and lose fluidity, thereby achieving the drying of water. Dry water is mainly prepared by a micro-droplet particle encapsulated by a nano-scale silica particle coating layer. It is similar in shape to conventional explosion suppression powders, fire extinguishing powders and other powder materials. The overall dry powder material has a water content of up to 98% in the particles. In addition, dry water has a large specific surface area and excellent adsorption properties. It can be used as a carrier to load some inorganic substances, organic substances and mixtures of the two substances inside it to form a stable core-shell dry water loaded powder. Dry water material is a shell-like structure formed by silica powder encapsulating liquid. As a new type of fire extinguishing material, it has a powdery appearance and good fluidity. Dry water material not only has a special structure and composition, but also has good adsorption properties and heat absorption characteristics, making it a potential explosion suppressant. The heat absorption of dry water is mainly due to its special physical and chemical structure. This property and structure enables dry water to effectively absorb heat during combustion and explosion, especially during the evaporation process, it can take away a large amount of heat, thus achieving a good cooling effect. In addition, the main component of dry water is silicon dioxide, which as an inert substance can effectively absorb heat by physical means. The existing explosion suppressants only stay at the single modification level, and there are few studies on the synergistic explosion suppression of composite explosion suppressants. Therefore, it is of great research value to use dry water with a core-shell structure as a carrier to prepare a composite explosion suppressant. Summary of the invention

[0006] The problem in the prior art is that the traditional powder explosion suppressant has poor explosion suppression performance. In view of the above problem, the present invention provides a dry water-loaded hydrotalcite powder explosion suppressant, and the preparation method thereof comprises the following steps:

[0007] (1) crushing the blocky hydrotalcite, grinding it, and sieving it to obtain ultrafine hydrotalcite powder, wherein the sieved particle size is not less than 800 mesh;

[0008] (2) uniformly dispersing the ultrafine hydrotalcite powder obtained in step (1) into deionized water to obtain a hydrotalcite suspension having a mass concentration of 50%;

[0009] (3) adding N,N-dimethylformamide to the hydrotalcite suspension obtained in step (2), and stirring at a constant temperature of 45-50° C. for 3-4 hours to obtain an LN solution, wherein the volume ratio of N,N-dimethylformamide to the hydrotalcite suspension is 1:2;

[0010] (4) uniformly dispersing nano-silicon dioxide in a dimethyl sulfoxide solution to obtain a silicon dioxide suspension having a mass concentration of 50%;

[0011] (5) adding silicone oil to the silica suspension obtained in step (4), stirring at high speed for 5 minutes at room temperature to obtain a dry aqueous solution, wherein the mass percentage of the silicone oil in the silica suspension is 2%;

[0012] (6) adding the LN solution obtained in step (3) to the dry water solution obtained in step (5), adjusting the pH to 7-8, and mixing at high speed for 10-15 minutes to obtain a LND mixed solution, wherein the volume ratio of the LN solution to the dry water solution is 1:2;

[0013] (7) centrifuging the LND mixed solution obtained in step (6) to obtain a bulk precipitate;

[0014] (8) The block precipitate obtained in step (8) was repeatedly washed with distilled water for 3-5 times, immersed in liquid nitrogen for 10 hours, and then vacuum dried at 50-60° C. for 24-48 hours to obtain a pure block solid;

[0015] (9) Grinding the pure block solid obtained in step (9), adding a small amount of muscovite and talc during the grinding process, and the sieved particle size is 10 μm to obtain a dry water-loaded hydrotalcite powder explosion suppressant, wherein the ratio of the pure block solid to muscovite and talc is 1:0.8.

[0016] Preferably, the nano-silica is hydrophilic nano-silica.

[0017] Preferably, the average particle size of the hydrophilic nano-silica is 50 nm.

[0018] Preferably, the stirring speed in step (5) is 10000-12000 r / min.

[0019] Preferably, the stirring speed in step (6) is 10000-12000 r / min.

[0020] Preferably, the centrifugal speed in step (7) is 8000-1000 r / min.

[0021] The present invention has the following beneficial effects:

[0022] (1) The dry water-loaded hydrotalcite powder explosion suppressant obtained by the present invention has a reasonable structural design, low material cost, economy and environmental protection, stable properties, high performance, simple preparation method, strong operability and practicability;

[0023] (2) The dry water-loaded hydrotalcite powder explosion suppressant obtained by the present invention is formed by first using N,N-dimethylformamide to perform intercalation modification on the hydrotalcite and then loading it on the surface of the dry water carrier. The N,N-dimethylformamide intercalation modifier can not only significantly improve the dispersibility of hydrotalcite powder in water and organic solvents and reduce its agglomeration phenomenon, but the N element in the molecular structure of N,N-dimethylformamide can adsorb free radicals in the methane explosion reaction and terminate the chain reaction between the free radicals, thereby achieving a certain explosion suppression effect, which has a better effect than other intercalation modifiers;

[0024] (3) Strongly polar N,N-dimethylformamide is intercalated into the interlayers of hydrotalcite as intercalated particles, which can destroy the interlayer hydrogen bonds, improve the charge transfer performance, interface compatibility and overall stability of the molecule in the solution, make it easier to react with dry water, and thus easier to adsorb on the dry water surface;

[0025] (4) The dry water-loaded hydrotalcite powder explosion suppressant obtained by the present invention has a core-shell structure. The dry water carrier has a large specific surface area and excellent adsorption performance. The intercalated modified hydrotalcite particles are firmly adsorbed on the outer surface of the dry water carrier. A large number of intercalated modified hydrotalcite particles are attached to the surface of the dry water carrier, making the surface of the dry water-loaded hydrotalcite powder explosion suppressant very rough, making it easier to attach to explosive substances (mainly referring to the reactants methane and oxygen in the explosion, and various free radicals formed in the explosion reaction, such as H· and OH·, etc.), and undergo a series of reactions with the explosive substances. The core-shell structure of the dry water and the layered structure of the modified hydrotalcite can block and capture free radicals, reduce the free radicals in the explosion reaction, and thus terminate the explosion chain reaction. In addition, the above structure can effectively block heat, and the rough surface structure can form a certain friction force, which brings a certain resistance to the explosion reactants, free radicals and explosion energy, delays the reaction, and has a better explosion suppression effect;

[0026] (5) The dry water-loaded hydrotalcite powder explosion suppressant obtained by the present invention is subjected to the impact of high temperature and high pressure during the methane explosion process, and will be engulfed in the flame and decomposed into fine multi-component particles. The intercalated modified hydrotalcite particles will be separated from the surface of the dry water carrier and put into the explosion reaction. When the explosion occurs, the intercalated modified hydrotalcite particles and the dry water carrier can synergistically absorb heat and continuously cool down to reduce the temperature in the reaction area. Both will also release a large amount of water vapor and non-combustible gases (carbon dioxide, sulfur dioxide and nitrogen, etc.). These substances can not only dilute the content of the reaction gas, but also prevent the continued occurrence of free radical chain reactions. They can also dilute or remove toxic and harmful or greenhouse gases generated during the explosion to prevent poisoning and pollution.

[0027] (6) The dry water-loaded hydrotalcite powder explosion suppressant obtained by the present invention is a core-shell three-dimensional structure with a rough surface, a large specific surface area, and a high porosity. It has good adsorption performance and heat insulation properties, and can block and insulate the explosion flame shock wave at multiple levels, thereby increasing the contact and collision probability between the explosion flame shock wave and the free radicals in the explosion reaction, achieving random and efficient capture of the free radicals in the explosion reaction, effectively isolating the heat, cooling the reaction system, delaying the explosion process, and preventing the harm caused by the secondary explosion.

[0028] (7) The dry water-loaded hydrotalcite powder explosion suppressant obtained by the present invention contains a large amount of alkali metal ions and formyl groups in its structure. These active free radicals can participate in free radical reactions when methane undergoes an explosion reaction and affect the reaction process, especially reacting with the key free radicals OH· and H· in the explosion reaction, so that the number of free radicals required to maintain the explosion reaction is rapidly reduced, thereby blocking the reaction chain and preventing the explosion reaction from proceeding. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 : is a thermogravimetric analysis curve of the dry water-loaded hydrotalcite powder explosion suppressant obtained in Example 1.

[0030] Figure 2 : is the particle size distribution diagram of the dry water-loaded hydrotalcite powder explosion suppressant obtained in Example 1.

[0031] Figure 3 : This is a scanning electron microscope image of the dry water-loaded hydrotalcite powder explosion suppressant obtained in Example 1 at a magnification of 5000 times.

[0032] Figure 4 : This is a scanning electron microscope image of the dry water-loaded hydrotalcite powder explosion suppressant obtained in Example 1 at a magnification of 8000 times.

[0033] Figure 5 : It is a comparison chart of the maximum explosion pressure change curve of the dry water-loaded hydrotalcite powder explosion suppressant obtained in Example 1 under different powder spraying amounts (180-420 mg) in a methane explosion pipeline, and 9.5% methane-air. In the figure, 9.5% CH4 represents a mixed gas formed by methane and air with a volume concentration of 9.5%.

[0034] Figure 6 : This is a comparison of the maximum flame speed change curve of the dry water-loaded hydrotalcite powder explosion suppressant obtained in Example 1 under different powder spraying amounts (180-420 mg) in a methane explosion pipeline with that of 9.5% methane-air. In the figure, 9.5% CH4 represents a mixed gas formed by methane and air with a volume concentration of 9.5%. DETAILED DESCRIPTION

[0035] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.

[0036] The hydrophilic nano-silicon dioxide used in the following examples of the present invention was purchased from Hebei Zhuyan Alloy Material Co., Ltd. and the product number is HK-SiO2-1.

[0037] The silicone oil used in the following examples of the present invention has a CAS number of 63148-62-9.

[0038] Example 1

[0039] A dry water-loaded hydrotalcite powder explosion suppressant, the preparation method of which is as follows:

[0040] (1) crushing the blocky hydrotalcite, grinding it, and sieving it to obtain ultrafine hydrotalcite powder, the sieved particle size of which is 800 mesh;

[0041] (2) uniformly dispersing the ultrafine hydrotalcite powder obtained in step (1) into deionized water to obtain a hydrotalcite suspension having a mass concentration of 50%;

[0042] (3) adding N,N-dimethylformamide to the hydrotalcite suspension obtained in step (2), and stirring at a constant temperature of 45° C. for 3 h to obtain an LN solution, wherein the volume ratio of N,N-dimethylformamide to the hydrotalcite suspension is 1:2;

[0043] (4) uniformly dispersing nano-silicon dioxide in a dimethyl sulfoxide solution to obtain a silicon dioxide suspension having a mass concentration of 50%;

[0044] (5) adding silicone oil to the silica suspension obtained in step (4), stirring at high speed for 5 minutes at room temperature to obtain a dry aqueous solution, wherein the mass percentage of the silicone oil in the silica suspension is 2%;

[0045] (6) adding the LN solution obtained in step (3) to the dry water solution obtained in step (5), adjusting the pH to 7, and mixing at high speed for 10 minutes to obtain a LND mixed solution, wherein the volume ratio of the LN solution to the dry water solution is 1:2;

[0046] (7) centrifuging the LND mixed solution obtained in step (6) to obtain a bulk precipitate;

[0047] (8) The block precipitate obtained in step (8) was repeatedly washed with distilled water for 5 times, immersed in liquid nitrogen for 10 hours, and then vacuum dried at 50° C. for 24 hours to obtain a pure block solid;

[0048] (9) Grinding the pure block solid obtained in step (9), adding a small amount of muscovite and talc during the grinding process, and the sieved particle size is 10 μm to obtain a dry water-loaded hydrotalcite powder explosion suppressant, wherein the ratio of the pure block solid to muscovite and talc is 1:0.8.

[0049] Example 2

[0050] A dry water-loaded hydrotalcite powder explosion suppressant, the preparation method of which is as follows:

[0051] (1) crushing the blocky hydrotalcite, grinding it, and sieving it to obtain ultrafine hydrotalcite powder, the sieved particle size of which is 800 mesh;

[0052] (2) uniformly dispersing the ultrafine hydrotalcite powder obtained in step (1) into deionized water to prepare a hydrotalcite suspension with a mass concentration of 50%;

[0053] (3) adding N,N-dimethylformamide to the hydrotalcite suspension obtained in step (2), and stirring at a constant temperature of 50° C. for 4 hours to obtain an LN solution, wherein the volume ratio of N,N-dimethylformamide to the hydrotalcite suspension is 1:2;

[0054] (4) uniformly dispersing nano-silicon dioxide in a dimethyl sulfoxide solution to obtain a silicon dioxide suspension having a mass concentration of 50%;

[0055] (5) adding silicone oil to the silica suspension obtained in step (4), stirring at high speed for 5 minutes at room temperature to obtain a dry aqueous solution, wherein the mass percentage of the silicone oil in the silica suspension is 2%;

[0056] (6) adding the LN solution obtained in step (3) to the dry water solution obtained in step (5), adjusting the pH to 8, and mixing at high speed for 15 minutes to obtain a LND mixed solution, wherein the volume ratio of the LN solution to the dry water solution is 1:3;

[0057] (7) centrifuging the LND mixed solution obtained in step (6) to obtain a bulk precipitate;

[0058] (8) The block precipitate obtained in step (8) was repeatedly washed with distilled water for 3 times, immersed in liquid nitrogen for 10 h, and then vacuum dried at 60 ° C for 48 h to obtain a pure block solid;

[0059] (9) Grinding the pure block solid obtained in step (9), adding a small amount of muscovite and talc during the grinding process, and the sieved particle size is 10 μm to obtain a dry water-loaded hydrotalcite powder explosion suppressant, wherein the ratio of the pure block solid to muscovite and talc is 1:0.8.

[0060] Comparative Example 1 is the same as Example 1, except that the pH in step (6) of Comparative Example 1 is 6.

[0061] Comparative Example 2 is the same as Example 1, except that the pH in step (6) of Comparative Example 2 is 9.

[0062] Comparative Example 3 is 800 mesh pure talcum powder.

[0063] Comparative Example 4 is intercalation-modified hydrotalcite, and the preparation method is as follows:

[0064] (1) crushing the blocky hydrotalcite, grinding it, and sieving it to obtain ultrafine hydrotalcite powder, the sieved particle size of which is 800 mesh;

[0065] (2) uniformly dispersing the ultrafine hydrotalcite powder obtained in step (1) into deionized water to obtain a hydrotalcite suspension having a mass concentration of 50%;

[0066] (3) adding N,N-dimethylformamide to the hydrotalcite suspension obtained in step (2), and stirring at a constant temperature of 45° C. for 3 h to obtain an LN solution, which was centrifuged, washed with water, dried, and ground to obtain 10 μm N,N-dimethylformamide intercalated modified talc powder, wherein the volume ratio of N,N-dimethylformamide to the hydrotalcite suspension was 1:2;

[0067] Comparative Example 5 is a dry water carrier, and the preparation method is as follows:

[0068] (1) uniformly dispersing nano-silicon dioxide in a dimethyl sulfoxide solution to obtain a silicon dioxide suspension having a mass concentration of 50%;

[0069] (2) adding silicone oil to the silica suspension obtained in step (4), stirring at high speed for 5 minutes at room temperature to obtain a dry water solution, and then centrifuging, washing, drying and grinding to obtain a dry water carrier powder, wherein the mass percentage of the silicone oil in the silica suspension is 2%.

[0070] Comparative Example 6 is a mixture of intercalated modified hydrotalcite and dry water carrier in a mass ratio of 1:1. The intercalated modified hydrotalcite is the same as the intercalated modified hydrotalcite prepared in Comparative Example 4, and the dry water carrier is the same as the dry water carrier prepared in Comparative Example 5.

[0071] Comparative Example 7 is the same as Example 1, except that the intercalation modifier N,N-dimethylformamide in Example 1 is replaced by an equal amount of sodium dodecylbenzenesulfonate in Comparative Example 7.

[0072] Performance Testing

[0073] The explosion test platform used in the experiment is mainly composed of a 2.5L closed methane explosion pipeline, a gas distribution system, a high-frequency pulse automatic ignition system, a powder spraying system, a data acquisition system, a synchronous controller and a high-speed camera. Before the explosion experiment, the methane explosion pipeline was dried. The specific experimental steps are to first pass the methane-air premixed gas with a methane volume concentration of 9.5% into the pipeline through a premixed gas bottle, use a powder storage tank and a powder spraying device to spray the required mass of explosion suppressant into the pipeline, and after the explosion suppressant is evenly dispersed in the pipeline and forms a dust cloud, turn on the high-speed camera and the pressure signal acquisition card, and then ignite the methane through the automatic ignition device to cause the methane to explode. After the experiment is over, the relevant pressure data and flame images are stored and processed. Under the condition of 9.5% methane gas, the explosion suppressant actively suppresses the explosion, and a PVC film is used at the end of the pipeline to achieve the purpose of explosion relief, which can not only obtain reliable pressure data, but also ensure the safety of the experiment. The explosion suppression performance test results of the explosion suppressants obtained in Examples 1-2 of the present invention and Comparative Examples 1-7 are shown in Table 1. The specific surface area data of the explosion suppressants obtained in Examples 1-2 of the present invention and Comparative Examples 1-7 are shown in Table 2.

[0074] Specific surface area test: The specific surface area of ​​the powder is measured by a specific surface area analyzer using the gas adsorption method (BET method).

[0075] Table 1

[0076]

[0077] In Table 1, 9.5% methane-air means that no explosion suppressant is sprayed into the methane explosion pipeline, and the methane explosion pipeline is only filled with a mixture of methane and air with a volume concentration of 9.5%.

[0078] Table 2

[0079] Test items <![CDATA[Specific surface area (m 2 / g)]]> Example 1 295 Example 2 290 Comparative Example 1 286 Comparative Example 2 285 Comparative Example 3 186 Comparative Example 4 232 Comparative Example 5 276 Comparative Example 6 293 Comparative Example 7 280

[0080] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A dry water-loaded hydrotalcite powder explosion suppressant, It is characterized in that The preparation method comprises the following steps: (1) crushing the blocky hydrotalcite, grinding it, and sieving it to obtain ultrafine hydrotalcite powder, wherein the sieved particle size is not less than 800 mesh; (2) uniformly dispersing the ultrafine hydrotalcite powder obtained in step (1) into deionized water to obtain a hydrotalcite suspension having a mass concentration of 50%; (3) adding N,N-dimethylformamide to the hydrotalcite suspension obtained in step (2), and stirring at a constant temperature of 45-50° C. for 3-4 hours to obtain an LN solution, wherein the volume ratio of N,N-dimethylformamide to the hydrotalcite suspension is 1:2; (4) uniformly dispersing nano-silicon dioxide in a dimethyl sulfoxide solution to obtain a silicon dioxide suspension having a mass concentration of 50%; (5) adding silicone oil to the silica suspension obtained in step (4), stirring at high speed for 5 minutes at room temperature to obtain a dry aqueous solution, wherein the mass percentage of the silicone oil in the silica suspension is 2%; (6) adding the LN solution obtained in step (3) to the dry water solution obtained in step (5), adjusting the pH to 7-8, and mixing at high speed for 10-15 minutes to obtain a LND mixed solution, wherein the volume ratio of the LN solution to the dry water solution is 1:2; (7) centrifuging the LND mixed solution obtained in step (6) to obtain a bulk precipitate; (8) The block precipitate obtained in step (8) was repeatedly washed with distilled water for 3-5 times, immersed in liquid nitrogen for 10 hours, and then vacuum dried at 50-60° C. for 24-48 hours to obtain a pure block solid; (9) Grinding the pure block solid obtained in step (9), adding a small amount of muscovite and talc during the grinding process, and the sieved particle size is 10 μm to obtain a dry water-loaded hydrotalcite powder explosion suppressant, wherein the ratio of the pure block solid to muscovite and talc is 1:0.

8.

2. A dry water-loaded hydrotalcite powder explosion suppressant according to claim 1, It is characterized in that Nano-silica is hydrophilic nano-silica.

3. A dry water-loaded hydrotalcite powder explosion suppressant according to claim 2, It is characterized in that The average particle size of the hydrophilic nano-silica is 50 nm.

4. The dry water-loaded hydrotalcite powder explosion suppressant according to claim 1, It is characterized in that The stirring speed in step (5) is 10000-12000r / min.

5. The dry water-loaded hydrotalcite powder explosion suppressant according to claim 1, It is characterized in that The stirring speed in step (6) is 10000-12000 r / min.

6. The dry water-loaded hydrotalcite powder explosion suppressant according to claim 1, It is characterized in that The centrifugal speed in step (7) is 8000-1000 r / min.

Citation Information

Cited By

  • Composite dry water explosion suppressant for suppressing explosion of organic dust and preparation method of composite dry water explosion suppressant

    CN119982039A