Ultrafine powder additive capable of inducing negative air ions and preparation process thereof
By using raw materials and nanomaterials such as complexes of platinum and palladium in ultrafine powder additives, combined with specific grinding processes, the problem of existing ultrafine powder additives' insufficient ability to induce negative ions in the air has been solved, and a more efficient Negative ion generation and improved stability.
Patent Information
- Application Number
- CN202410716293.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-18
AI Technical Summary
Existing ultrafine powder additives have a weak ability to induce negative ions in the air, and in order to enhance this ability, their stability is easily reduced.
Using an ultra-fine powder additive including platinum and palladium complexes, hexacyclic stone, nano tourmaline, germanium stone, meteorite, wheat rare earth, diatomite, tremolite, silver ions, thiosulfate and other raw materials, Through a specific mixing and grinding process, nano nickel powder is added, Wheat hulls, dispersants, stabilizers, grinding aids, binders, microcrystalline glass fibers and nano-silica and other auxiliary materials enhance the discharge and photoelectric effect with air molecules, thereby improving the generation capacity of negative ions. And its properties are stabilized by titanium dioxide.
It significantly improves the negative ion inducing effect of ultra-fine powder additives, while ensuring its stability and enhancing the negative ion generation capacity and stability during use.
Smart Images

Figure BDA0004875677550000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ultrafine powder additives, and in particular to an ultrafine powder additive capable of inducing negative air ions and a preparation process thereof. Background Art
[0002] Ultrafine powder additives are micro powders with a particle size of less than a few microns. Ultrafine powder additives have broad application prospects in many fields due to their unique physical and chemical properties.
[0003] The existing ultrafine powder additives have a weak ability to induce negative ions in the air, and some ultrafine powder additives tend to reduce the stability of their ultrafine powder additives in order to enhance their ability to induce negative ions in the air.
[0004] Therefore, we proposed an ultrafine powder additive capable of inducing negative air ions and its preparation process to solve the above problems. Summary of the invention
[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose an ultrafine powder additive capable of inducing negative air ions and a preparation process thereof.
[0006] An ultrafine powder additive capable of inducing negative air ions, comprising an ultrafine powder additive body, wherein the ultrafine powder additive body comprises a base material, an additive material and an auxiliary material, and the weight ratio of the base material, an additive material and an auxiliary material when used is (60±2.5-30±2.5): (15±1.5-85±1.5): (25±0.5-75±0.5);
[0007] The base material includes the following raw materials in parts by weight: a complex of platinum and palladium, hexacyclic stone, nano-tourmaline, germanium stone, Bian stone, wheat rare earth, diatomite, tremolite, silver ions, and thiosulfate;
[0008] The additives include the following raw materials in parts by weight: titanium dioxide, nano nickel powder, and wheat husk;
[0009] The auxiliary materials include the following raw materials in parts by weight: dispersant, stabilizer, grinding aid, binder, microcrystalline glass fiber, and nano silicon dioxide.
[0010] Preferably, the base material comprises the following raw materials in parts by weight: 15-80 parts of platinum and palladium complexes, 50-80 parts of hexacyclic stone, 10-15 parts of nano-tourmaline, 5-10 parts of germanium stone, 100-210 parts of Bian stone, 20-100 parts of wheat rare earth, 5-8 parts of diatomite, 1-8 parts of tremolite, 20-50 parts of silver ions, and 5-10 parts of thiosulfate;
[0011] The additive comprises the following raw materials in parts by weight: 4-8 parts of titanium dioxide, 1-8 parts of nano nickel powder, and 0.2-0.8 parts of wheat husk;
[0012] The auxiliary materials include the following raw materials in parts by weight: 0.5-1 part of dispersant, 0.1-0.8 part of stabilizer, 0.1-0.5 part of grinding aid, 0.1-0.4 part of binder, 0.8-1.5 part of microcrystalline glass fiber, and 0.2-1.4 part of nano silicon dioxide.
[0013] Preferably, the carbon material is carbon nanotubes and graphene, and the weight ratio of carbon nanotubes to graphene is (40-60): (35-65).
[0014] Preferably, the complex of platinum and palladium is platinum and palladium, and the weight ratio of platinum to palladium is (40-60): (35-65).
[0015] A preparation process of an ultrafine powder additive capable of inducing negative air ions comprises the following steps:
[0016] S1. Place hexacyclic stone, nano tourmaline, germanium stone, Bian stone, rare earth, diatomite, tremolite, nano nickel powder, microcrystalline glass fiber, and nano silicon dioxide in a stirring cleaning machine and add 50-60 parts of a water-based cleaning agent for cleaning. After cleaning, place them in a dryer for drying. The drying time is 40-60 minutes. The working pressure of the dryer is 0.5-1MPa. After drying, place them in a jet mill for preliminary crushing.
[0017] S2, the crushed six ring stone, nano tourmaline, germanium stone, Bian stone, rare earth, diatomite, tremolite, nano nickel powder, microcrystalline glass fiber, nano silicon dioxide are placed in a blender, and titanium dioxide, silver ions, thiosulfate, silver ions, thiosulfate are added to the blender in sequence to mix to obtain a mixture, and the mixing time is 20-30min, the stirring speed is 600-700rpm, and the vacuum degree is 1800-2000Pa;
[0018] S3, placing the mixed material in S2 in a ball mill for preliminary grinding, and gradually adding wheat husks to continue grinding, wherein the grinding time is 15-20 minutes, and the grinding speed is 100-200 r / min;
[0019] S4, placing the preliminarily ground mixed material in S3 in a jet mill for ultrafine grinding, wherein the grinding disc speed of the jet mill is 700-800 rpm, the grinding pressure is 0.5-0.6 MPa, and the air flow speed in the jet mill is 800-1000 m / s;
[0020] S5, placing the ultrafinely crushed mixture in S4 in a blender and adding 50-60 parts of distilled water, and sequentially adding a dispersant, a stabilizer, a grinding aid, and a binder into the blender for dispersion and stirring to obtain a mixed solution, wherein the stirring time is 25-35 min, the stirring speed is 900-1000 rpm, and the vacuum degree is 1500-1900 Pa;
[0021] S6, placing the mixed solution obtained by the dispersion and stirring in S5 in a box-type dryer for drying to obtain preliminary dried particles, and placing the preliminary dried particles after drying in a multi-layer screening machine for screening, wherein the multi-layer screening machine has 5 layers of screens, and the mesh number of the screen is 400-500 meshes
[0022] S7. The preliminary dried particles after screening in S6 are placed in an air flow screen for impurity removal, wherein the screening particle size of the air flow screen is 1-5 microns, and the preliminary dried particles after impurity removal are placed in an air flow mill for ultrafine grinding. After ultrafine grinding, the particles are introduced into a packaging bag for sealed packaging to obtain an ultrafine powder additive, and the grinding disc speed of the air flow mill is 700-800rmp, the grinding pressure is 0.5-0.6MPa, and the air flow speed in the air flow mill is 800-1000m / s.
[0023] Preferably, in S5, the dispersant, stabilizer, grinding aid and binder are sieved through a sieve before being added into the mixer, and the mesh number of the sieve is 300-400 meshes.
[0024] Preferably, in S1, after cleaning, the hexacyclic stone, nano-tourmaline, germanium stone, Bian stone, rare earth and diatomaceous earth are rinsed with pure water for multiple times until the residual cleaning agent is removed.
[0025] Preferably, in S1, the grinding disc speed of the jet mill is 500-700 rpm, the grinding pressure is 0.4-0.5 MPa, and the speed of the airflow in the jet mill is 600-800 m / s.
[0026] The beneficial effects of the present invention are:
[0027] 1. In the present invention, the discharge effect between the ultrafine powder additive and the air molecules can be enhanced by adding nano-tourmaline, tremolite, nano-nickel powder and wheat husk in the process of preparing the ultrafine powder additive, thereby increasing the generation of negative ions, and the addition of microcrystalline glass fiber and nano-silicon dioxide can increase the photoelectric effect of the ultrafine powder additive, further increase the generation of negative ions, thereby enhancing the effect of inducing negative ions of the ultrafine powder additive.
[0028] 2. In the present invention, by adding the complex of platinum and palladium, the negative ions can be stabilized, the stability of the ultrafine powder additive is further enhanced, and the stability of the ultrafine powder additive during use is ensured. By adding titanium dioxide during the preparation process of the ultrafine powder additive, the ability of the ultrafine powder additive to induce negative ions in the air can be further improved. DETAILED DESCRIPTION
[0029] The present invention will be further explained below in conjunction with specific embodiments.
[0030] Example 1
[0031] An ultrafine powder additive capable of inducing negative air ions, comprising an ultrafine powder additive body, wherein the ultrafine powder additive body comprises a base material, an additive material and an auxiliary material in a weight ratio of 62.5:16.5:25.5 when in use;
[0032] The base material includes the following raw materials in parts by weight: complex of platinum and palladium, hexacyclic stone, nano tourmaline, germanium stone, Bian stone, wheat rare earth, diatomite, tremolite, silver ion, thiosulfate;
[0033] The additives include the following raw materials in parts by weight: titanium dioxide, nano nickel powder, and wheat husk;
[0034] The auxiliary materials include the following raw materials in parts by weight: dispersant, stabilizer, grinding aid, binder, microcrystalline glass fiber, and nano silicon dioxide.
[0035] The base material includes the following raw materials in parts by mass: 15 parts of platinum and palladium complex, 50 parts of hexacyclic stone, 10 parts of nano tourmaline, 5 parts of germanium stone, 100 parts of Bian stone, 20-100 parts of wheat rare earth, 5 parts of diatomite, 1 part of tremolite, 20 parts of silver ions, and 5 parts of thiosulfate;
[0036] The additives include the following raw materials in parts by weight: 4 parts of titanium dioxide, 1 part of nano nickel powder, and 0.2 parts of wheat husk;
[0037] The auxiliary materials include the following raw materials in parts by weight: 0.5 parts of dispersant, 0.1 parts of stabilizer, 0.1 parts of grinding aid, 0.1 parts of binder, 0.8 parts of microcrystalline glass fiber, and 0.2 parts of nano silicon dioxide.
[0038] The carbon materials are carbon nanotubes and graphene, and the weight ratio of the carbon nanotubes to the graphene is 60:40.
[0039] The complex of platinum and palladium is platinum and palladium, and the weight ratio of platinum to palladium is 60:40.
[0040] A preparation process of an ultrafine powder additive capable of inducing negative air ions comprises the following steps:
[0041] S1. Place hexacyclic stone, nano tourmaline, germanium stone, Bian stone, rare earth, diatomite, tremolite, nano nickel powder, microcrystalline glass fiber, and nano silicon dioxide in a stirring cleaning machine and add 50 parts of a water-based cleaning agent for cleaning. After cleaning, place them in a dryer for drying. The drying time is 40 minutes. The working pressure of the dryer is 0.5 MPa. After drying, place them in a jet mill for preliminary crushing.
[0042] S2, the crushed six ring stone, nano tourmaline, germanium stone, Bian stone, rare earth, diatomite, tremolite, nano nickel powder, microcrystalline glass fiber, nano silicon dioxide are placed in a blender, and titanium dioxide, silver ions, thiosulfate, silver ions, thiosulfate are added to the blender in sequence to mix to obtain a mixture, and the mixing time is 20min, the stirring speed is 600rpm, and the vacuum degree is 1800Pa;
[0043] S3, placing the mixed material in S2 in a ball mill for preliminary grinding, and gradually adding wheat husks to continue grinding, wherein the grinding time is 15 minutes and the grinding speed is 100 r / min;
[0044] S4, placing the preliminarily ground mixture in S3 in a jet mill for ultrafine grinding, wherein the grinding disc speed of the jet mill is 700 rpm, the grinding pressure is 0.5 MPa, and the air flow speed in the jet mill is 800 m / s;
[0045] S5, placing the ultrafinely crushed mixture in S4 in a blender and adding 50 parts of distilled water, and sequentially adding a dispersant, a stabilizer, a grinding aid, and a binder into the blender for dispersion and stirring to obtain a mixed solution, wherein the stirring time is 25 min, the stirring speed is 900 rpm, and the vacuum degree is 1500 Pa;
[0046] S6, placing the mixed solution obtained by the dispersion and stirring in S5 in a box-type dryer for drying to obtain preliminary dried particles, and placing the dried preliminary dried particles in a multi-layer screening machine for screening, wherein the multi-layer screening machine has 5 layers of screens and a mesh size of 400 meshes.
[0047] S7. The preliminary dried particles after screening in S6 are placed in an air flow screen for impurity removal, wherein the screening particle size of the air flow screen is 1 micron, and the preliminary dried particles after impurity removal are placed in an air flow mill for ultrafine grinding. After ultrafine grinding, they are introduced into a packaging bag for sealed packaging to obtain an ultrafine powder additive, and the grinding disc speed of the air flow mill is 700rmp, the grinding pressure is 0.5MPa, and the air flow speed in the air flow mill is 800m / s.
[0048] In S5, the dispersant, stabilizer, grinding aid, and binder are sieved through a sieve before being added into the mixer, and the mesh number of the sieve is 300 meshes.
[0049] In S1, after the cleaning is completed, the hexacyclic stone, nano-tourmaline, germanium stone, Bian stone, rare earth, and diatomaceous earth are rinsed with pure water for multiple times until the residual cleaning agent is removed.
[0050] In S1, the grinding disc speed of the jet mill is 5000 rpm, the grinding pressure is 0.4 MPa, and the speed of the air flow in the jet mill is 600 m / s.
[0051] Example 2
[0052] An ultrafine powder additive capable of inducing negative air ions, comprising an ultrafine powder additive body, wherein the ultrafine powder additive body comprises a base material, an additive material and an auxiliary material in a weight ratio of 60:15:25 when in use;
[0053] The base material includes the following raw materials in parts by weight: complex of platinum and palladium, hexacyclic stone, nano tourmaline, germanium stone, Bian stone, wheat rare earth, diatomite, tremolite, silver ion, thiosulfate;
[0054] The additives include the following raw materials in parts by weight: titanium dioxide, nano nickel powder, and wheat husk;
[0055] The auxiliary materials include the following raw materials in parts by weight: dispersant, stabilizer, grinding aid, binder, microcrystalline glass fiber, and nano silicon dioxide.
[0056] The base material includes the following raw materials in parts by mass: 50 parts of platinum and palladium complex, 60 parts of hexacyclic stone, 12 parts of nano tourmaline, 7 parts of germanium stone, 150 parts of Bian stone, 80 parts of wheat rare earth, 6 parts of diatomite, 3 parts of tremolite, 29 parts of silver ion, and 8 parts of thiosulfate;
[0057] The additives include the following raw materials in parts by weight: 6 parts of titanium dioxide, 3 parts of nano nickel powder, and 0.5 parts of wheat husk;
[0058] The auxiliary materials include the following raw materials in parts by weight: 0.8 parts of dispersant, 0.6 parts of stabilizer, 0.3 parts of grinding aid, 0.24 parts of binder, 0.95 parts of microcrystalline glass fiber, and 0.12 parts of nano silicon dioxide.
[0059] The carbon materials are carbon nanotubes and graphene, and the weight ratio of the carbon nanotubes to the graphene is 55:45.
[0060] The complex of platinum and palladium is platinum and palladium, and the weight ratio of platinum to palladium is 50:50.
[0061] A preparation process of an ultrafine powder additive capable of inducing negative air ions comprises the following steps:
[0062] S1. Place hexacyclic stone, nano tourmaline, germanium stone, Bian stone, rare earth, diatomite, tremolite, nano nickel powder, microcrystalline glass fiber, and nano silicon dioxide in a stirring cleaning machine and add 55 parts of a water-based cleaning agent for cleaning. After cleaning, place them in a dryer for drying. The drying time is 45 minutes. The working pressure of the dryer is 0.8 MPa. After drying, place them in a jet mill for preliminary crushing.
[0063] S2, the crushed six ring stone, nano tourmaline, germanium stone, Bian stone, rare earth, diatomite, tremolite, nano nickel powder, microcrystalline glass fiber, nano silicon dioxide are placed in a blender, and titanium dioxide, silver ions, thiosulfate, silver ions, thiosulfate are added into the blender in sequence to mix to obtain a mixture, and the mixing time is 25min, the stirring speed is 650rpm, and the vacuum degree is 1900Pa;
[0064] S3, placing the mixed material in S2 in a ball mill for preliminary grinding, and gradually adding wheat husks to continue grinding, wherein the grinding time is 18 minutes, and the grinding speed is 150 r / min;
[0065] S4, placing the preliminarily ground mixture in S3 in a jet mill for ultrafine grinding, wherein the grinding disc speed of the jet mill is 750 rpm, the grinding pressure is 0.55 MPa, and the air flow speed in the jet mill is 850 m / s;
[0066] S5, placing the ultrafinely crushed mixture in S4 in a blender and adding 55 parts of distilled water, and sequentially adding a dispersant, a stabilizer, a grinding aid, and a binder into the blender for dispersion and stirring to obtain a mixed solution, wherein the stirring time is 30 min, the stirring speed is 950 rpm, and the vacuum degree is 1700 Pa;
[0067] S6, placing the mixed solution obtained by the dispersion and stirring in S5 in a box-type dryer for drying to obtain preliminary dried particles, and placing the dried preliminary dried particles in a multi-layer screening machine for screening, wherein the multi-layer screening machine has 5 layers of screens and a mesh size of 450 meshes.
[0068] S7. The preliminary dried particles after screening in S6 are placed in an air flow screen for impurity removal, wherein the screening particle size of the air flow screen is 3 microns, and the preliminary dried particles after impurity removal are placed in an air flow mill for ultrafine grinding. After ultrafine grinding, they are introduced into a packaging bag for sealed packaging to obtain an ultrafine powder additive, and the grinding disc speed of the air flow mill is 750rmp, the grinding pressure is 0.55MPa, and the air flow speed in the air flow mill is 8500m / s.
[0069] In S5, the dispersant, stabilizer, grinding aid, and binder are sieved through a sieve before being added into the mixer, and the mesh number of the sieve is 350 meshes.
[0070] In S1, after the cleaning is completed, the hexacyclic stone, nano-tourmaline, germanium stone, Bian stone, rare earth, and diatomaceous earth are rinsed with pure water for multiple times until the residual cleaning agent is removed.
[0071] In S1, the grinding disc speed of the jet mill is 600 rpm, the grinding pressure is 0.45 MPa, and the speed of the air flow in the jet mill is 650 m / s.
[0072] Example 3
[0073] An ultrafine powder additive capable of inducing negative air ions, comprising an ultrafine powder additive body, wherein the ultrafine powder additive body comprises a base material, an additive material and an auxiliary material in a weight ratio of 32.5:86.5:75.5 when in use;
[0074] The base material includes the following raw materials in parts by weight: complex of platinum and palladium, hexacyclic stone, nano tourmaline, germanium stone, Bian stone, wheat rare earth, diatomite, tremolite, silver ion, thiosulfate;
[0075] The additives include the following raw materials in parts by weight: titanium dioxide, nano nickel powder, and wheat husk;
[0076] The auxiliary materials include the following raw materials in parts by weight: dispersant, stabilizer, grinding aid, binder, microcrystalline glass fiber, and nano silicon dioxide.
[0077] The base material includes the following raw materials in parts by mass: 80 parts of platinum and palladium complex, 80 parts of hexacyclic stone, 15 parts of nano tourmaline, 10 parts of germanium stone, 210 parts of Bian stone, 100 parts of wheat rare earth, 8 parts of diatomite, 8 parts of tremolite, 50 parts of silver ion, and 10 parts of thiosulfate;
[0078] The additives include the following raw materials in parts by weight: 8 parts of titanium dioxide, 8 parts of nano nickel powder, and 0.8 parts of wheat husk;
[0079] The auxiliary materials include the following raw materials in parts by weight: 1 part of dispersant, 0.8 part of stabilizer, 0.5 part of grinding aid, 0.4 part of binder, 1.5 parts of microcrystalline glass fiber, and 1.4 parts of nano silicon dioxide.
[0080] The carbon materials are carbon nanotubes and graphene, and the weight ratio of the carbon nanotubes to the graphene is 60:65.
[0081] The complex of platinum and palladium is platinum and palladium, and the weight ratio of platinum to palladium is 60:65.
[0082] A preparation process of an ultrafine powder additive capable of inducing negative air ions comprises the following steps:
[0083] S1. Place hexacyclic stone, nano tourmaline, germanium stone, Bian stone, rare earth, diatomite, tremolite, nano nickel powder, microcrystalline glass fiber, and nano silicon dioxide in a stirring cleaning machine and add 60 parts of a water-based cleaning agent for cleaning. After cleaning, place them in a dryer for drying. The drying time is 60 minutes. The working pressure of the dryer is 1MPa. After drying, place them in a jet mill for preliminary crushing.
[0084] S2, the crushed six ring stone, nano tourmaline, germanium stone, Bian stone, rare earth, diatomite, tremolite, nano nickel powder, microcrystalline glass fiber, nano silicon dioxide are placed in a blender, and titanium dioxide, silver ions, thiosulfate, silver ions, thiosulfate are added into the blender in sequence to mix to obtain a mixture, and the mixing time is 30min, the stirring speed is 700rpm, and the vacuum degree is 2000Pa;
[0085] S3, placing the mixed material in S2 in a ball mill for preliminary grinding, and gradually adding wheat husks to continue grinding, wherein the grinding time is 20 minutes and the grinding speed is 200 r / min;
[0086] S4, placing the preliminarily ground mixture in S3 in a jet mill for ultrafine grinding, wherein the grinding disc speed of the jet mill is 800 rpm, the grinding pressure is 0.6 MPa, and the air flow speed in the jet mill is 1000 m / s;
[0087] S5, placing the ultrafinely crushed mixture in S4 in a blender and adding 60 parts of distilled water, and sequentially adding a dispersant, a stabilizer, a grinding aid, and a binder into the blender for dispersion and stirring to obtain a mixed solution, wherein the stirring time is 35 min, the stirring speed is 1000 rpm, and the vacuum degree is 1900 Pa;
[0088] S6, placing the mixed solution obtained by the dispersion and stirring in S5 in a box-type dryer for drying to obtain preliminary dried particles, and placing the dried preliminary dried particles in a multi-layer screening machine for screening, wherein the multi-layer screening machine has 5 layers of screens and a mesh size of 500 meshes.
[0089] S7. The preliminary dried particles after screening in S6 are placed in an air flow screen for impurity removal, wherein the screening particle size of the air flow screen is 1-5 microns, and the preliminary dried particles after impurity removal are placed in an air flow mill for ultrafine grinding. After ultrafine grinding, the particles are introduced into a packaging bag for sealed packaging to obtain an ultrafine powder additive, and the grinding disc speed of the air flow mill is 800rmp, the grinding pressure is 0.6MPa, and the air flow speed in the air flow mill is 1000m / s.
[0090] In S5, the dispersant, stabilizer, grinding aid, and binder are sieved through a sieve before being added into the mixer, and the mesh number of the sieve is 400 meshes.
[0091] In S1, after the cleaning is completed, the hexacyclic stone, nano-tourmaline, germanium stone, Bian stone, rare earth, and diatomaceous earth are rinsed with pure water for multiple times until the residual cleaning agent is removed.
[0092] In S1, the grinding disc speed of the jet mill is 700 rpm, the grinding pressure is 0.5 MPa, and the speed of the air flow in the jet mill is 800 m / s.
[0093] Three portions of ultrafine powder additives in Examples 1-3 and one portion of ordinary ultrafine powder additive were placed in a constant temperature and humidity test chamber, where there should be no pollutants such as dust, smoke, and chemical gases, and the negative ion concentration in the air was measured by a negative ion detector, and the final test results are as follows:
[0094] The following table is a comparison of the ability of ultrafine powder additives to induce negative ions in the air
[0095]
[0096] In the present invention, nano-tourmaline, tremolite, nano-nickel powder and wheat husk are added in the process of preparing the ultrafine powder additive, so that the discharge effect between the ultrafine powder additive and air molecules can be enhanced, thereby increasing the generation of negative ions. In addition, microcrystalline glass fiber and nano-silicon dioxide are added to increase the photoelectric effect of the ultrafine powder additive, further increasing the generation of negative ions, thereby enhancing the inducing negative ion effect of the ultrafine powder additive.
[0097] By adding platinum and palladium complexes, the negative ions can be stabilized, further enhancing the stability of the ultrafine powder additive and ensuring the stability of the ultrafine powder additive during use. By adding titanium dioxide during the preparation of the ultrafine powder additive, the ability of the ultrafine powder additive to induce negative ions in the air can be further enhanced.
[0098] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An ultrafine powder additive capable of inducing negative air ions, comprising an ultrafine powder additive body, It is characterized in that The ultrafine powder additive body includes a base material, an additive material and an auxiliary material in a weight ratio of (60±2.5-30±2.5): (15±1.5-85±1.5): (25±0.5-75±0.5) when used; The base material includes the following raw materials in parts by weight: a complex of platinum and palladium, hexacyclic stone, nano-tourmaline, germanium stone, Bian stone, wheat rare earth, diatomite, tremolite, silver ions, and thiosulfate; The additives include the following raw materials in parts by weight: titanium dioxide, nano nickel powder, and wheat husk; The auxiliary materials include the following raw materials in parts by weight: dispersant, stabilizer, grinding aid, binder, microcrystalline glass fiber and nano silicon dioxide.
2. The ultrafine powder additive capable of inducing negative air ions according to claim 1, It is characterized in that The base material includes the following raw materials in parts by weight: 15-80 parts of platinum and palladium complexes, 50-80 parts of hexacyclic stone, 10-15 parts of nano-tourmaline, 5-10 parts of germanium stone, 100-210 parts of Bian stone, 20-100 parts of wheat rare earth, 5-8 parts of diatomite, 1-8 parts of tremolite, 20-50 parts of silver ions, and 5-10 parts of thiosulfate; The additive comprises the following raw materials in parts by weight: 4-8 parts of titanium dioxide, 1-8 parts of nano nickel powder, and 0.2-0.8 parts of wheat husk; The auxiliary materials include the following raw materials in parts by weight: 0.5-1 part of dispersant, 0.1-0.8 part of stabilizer, 0.1-0.5 part of grinding aid, 0.1-0.4 part of binder, 0.8-1.5 part of microcrystalline glass fiber, and 0.2-1.4 part of nano silicon dioxide.
3. The ultrafine powder additive capable of inducing negative air ions according to claim 1, It is characterized in that The carbon material is carbon nanotubes and graphene, and the weight ratio of the carbon nanotubes to the graphene is (40-60): (35-65).
4. The ultrafine powder additive capable of inducing negative air ions according to claim 1, It is characterized in that The platinum and palladium complex is platinum and palladium, and the weight ratio of platinum to palladium is (40-60): (35-65).
5. A process for preparing an ultrafine powder additive capable of inducing negative air ions according to any one of claims 1 to 4, It is characterized in that The following steps are involved: S1. Place hexacyclic stone, nano tourmaline, germanium stone, Bian stone, rare earth, diatomite, tremolite, nano nickel powder, microcrystalline glass fiber, and nano silicon dioxide in a stirring cleaning machine and add 50-60 parts of a water-based cleaning agent for cleaning. After cleaning, place them in a dryer for drying. The drying time is 40-60 minutes. The working pressure of the dryer is 0.5-1MPa. After drying, place them in a jet mill for preliminary crushing. S2, the crushed six ring stone, nano tourmaline, germanium stone, Bian stone, rare earth, diatomite, tremolite, nano nickel powder, microcrystalline glass fiber, nano silicon dioxide are placed in a blender, and titanium dioxide, silver ions, thiosulfate, silver ions, thiosulfate are added to the blender in sequence to mix to obtain a mixture, and the mixing time is 20-30min, the stirring speed is 600-700rpm, and the vacuum degree is 1800-2000Pa; S3, placing the mixed material in S2 in a ball mill for preliminary grinding, and gradually adding wheat husks to continue grinding, wherein the grinding time is 15-20 minutes, and the grinding speed is 100-200 r / min; S4, placing the preliminarily ground mixed material in S3 in a jet mill for ultrafine grinding, wherein the grinding disc speed of the jet mill is 700-800 rpm, the grinding pressure is 0.5-0.6 MPa, and the air flow speed in the jet mill is 800-1000 m / s; S5, placing the ultrafinely crushed mixture in S4 in a blender and adding 50-60 parts of distilled water, and sequentially adding a dispersant, a stabilizer, a grinding aid, and a binder into the blender for dispersion and stirring to obtain a mixed solution, wherein the stirring time is 25-35 min, the stirring speed is 900-1000 rpm, and the vacuum degree is 1500-1900 Pa; S6, placing the mixed solution obtained by the dispersion and stirring in S5 in a box-type dryer for drying to obtain preliminary dried particles, and placing the preliminary dried particles after drying in a multi-layer screening machine for screening, wherein the multi-layer screening machine has 5 layers of screens, and the mesh number of the screen is 400-500 meshes S7. The preliminary dried particles after screening in S6 are placed in an air flow screen for impurity removal, wherein the screening particle size of the air flow screen is 1-5 microns, and the preliminary dried particles after impurity removal are placed in an air flow mill for ultrafine grinding. After ultrafine grinding, the particles are introduced into a packaging bag for sealed packaging to obtain an ultrafine powder additive, and the grinding disc speed of the air flow mill is 700-800rmp, the grinding pressure is 0.5-0.6MPa, and the air flow speed in the air flow mill is 800-1000m / s.
6. A process for preparing an ultrafine powder additive capable of inducing negative air ions according to claim 5, Features In S5, the dispersant, stabilizer, grinding aid and binder are sieved through a sieve before being added into the mixer, and the mesh number of the sieve is 300-400 meshes.
7. The preparation process of the ultrafine powder additive capable of inducing negative air ions according to claim 5, Features In S1, after the cleaning is completed, the hexacyclic stone, nano-tourmaline, germanium stone, Bian stone, rare earth, and diatomaceous earth are rinsed multiple times with pure water until the residual cleaning agent is removed.
8. The preparation process of the ultrafine powder additive capable of inducing negative air ions according to claim 5, Features In the S1, the grinding disc speed of the air flow mill is 500-700rmp, the grinding pressure is 0.4-0.5MPa, and the air flow speed in the air flow mill is 600-800m / s.
Citation Information
Patent Citations
Preparation method of ecological synthetic stone
CN103420639A
Anion putty powder and preparation method thereof
CN107383982A
Multifunctional negative ion energy sheet and preparation method thereof
CN111533545A
Inorganic antimicrobial agent
JP2000198708A
Negative ion generation oxygen catalyst composition, coating method therefor and fitting article
JP2006021167A
Cited By
Negative ion diaphragm and preparation method thereof
CN119552591A
A negative ion diaphragm and a method for manufacturing the same
CN119552591B