Electrically-controlled enrichment catalytic membrane as well as preparation method and application thereof in water treatment
By using a copolymer coated layer with electroredox reversibility in electrochemical water treatment, the enrichment catalytic film is solved by combining nano-carbon tubes and titanium oxide conductive ceramic films, it is difficult to remove multiple coexisting organics in the prior art. The problem of pollutants has achieved efficient and energy-saving water treatment effects.
Patent Information
- Application Number
- CN202310606717.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-26
AI Technical Summary
Existing electrochemical water treatment technology is difficult to effectively remove a variety of coexisting hydrophobic organic pollutants, and there are problems of insufficient electrochemical activity and inconvenient operation.
The copolymer coating layer with electroredox reversibility is used to electrically control the enriched catalytic film, and the selective adsorption-oxidation process is realized by regulating the voltage, removing coexisting pollutants, and combining the combination of nano-carbon tubes and titanium oxide conductive ceramic films. , improve catalytic performance.
It realizes efficient selective removal of a variety of hydrophobic organic pollutants, improves treatment performance and current utilization efficiency, reduces energy consumption, is convenient to operate, and is suitable for electrochemical water treatment.
Smart Images

Figure CN119034507A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmental organic pollution remediation, and in particular to an electrically controlled enrichment catalytic membrane and a preparation method thereof and application in water treatment. Background Art
[0002] Electrocatalytic membranes have the advantages of green energy saving, reaction confinement, quantitative adjustment, and mass transfer enhancement, and are ideal candidates for achieving deep treatment. In particular, the catalytic degradation of pollutants in the pores is affected by the nanoconfinement effect, resulting in selectivity for oxidation products. However, studies have also shown that too small a space (e.g., less than 0.4 nm) is likely to become a barrier to the entry of target pollutant molecules, which is expected to inevitably have a significant adverse effect on the permeability and catalytic performance of the catalytic membrane. Regarding the fact that spatial confinement can significantly improve reaction kinetics and efficiency, it is necessary to explore the differences in the interaction between pollutant molecules and the electric field, and exploring the coupling of micro-nano reaction space and electrical energy through reactor design and system engineering will further help improve treatment performance.
[0003] For heterogeneous systems, oxidizing species are generated at the catalyst interface, and the scope of action is often limited to the near surface. Therefore, by regulating the adsorption process of pollutants, the selective enrichment and oxidation of micropollutants at the catalytic interface can be achieved. In terms of selective electro-separation membranes, the utility model patent with application number CN202022274054.0 takes metal or non-metal ions as the research object, and realizes selective separation and removal through redox reactions, acid-base reactions and other mechanisms. However, most organic matter does not have valence changes, and the above-mentioned selective mechanism cannot be applied. In terms of selective separation membranes, in addition to the very mature theoretical research on metal or salt ions, the Chinese invention patent with application number 202111668803.0 constructs a catalytic membrane suitable for separating and removing target pollutants from NOM, but the selective layer of the membrane is not conductive and cannot be applied to electrocatalytic membrane systems. In terms of selective separation electrochemical technology, the Chinese invention patent with application number 202111668803.0 realizes selective separation and removal through mechanisms such as electrostatics and hydrophilic-hydrophobic interactions. However, the corresponding mechanism used in membrane research must take into account a series of problems caused by membrane contamination, such as excessive consumption of oxidizing species, local amplified electric fields, micro- and nanoscale turbulence, and concentration polarization.
[0004] In summary, in view of the demand for deep wastewater treatment, the problems of electrochemical activity, universality of organic pollution, long-term operation and convenient operation of existing treatment technologies limit their practical application. Therefore, there is an urgent need for a catalytic membrane that can remove a variety of organic pollutants in the field of electrochemical water treatment. Summary of the invention
[0005] The purpose of the present invention is to solve the above technical problems and provide an electrically controlled enrichment catalytic membrane and its preparation method and application. The electrically controlled enrichment catalytic membrane provided by the present invention realizes the electrically controlled selective adsorption-oxidation of target pollutants under coexisting pollution, can selectively remove coexisting pollution through voltage regulation, and is energy-saving, environmentally friendly and easy to operate.
[0006] In order to achieve the above-mentioned invention object, the specific technical scheme to be adopted by the present invention is as follows:
[0007] In the first aspect, the present invention provides an electrically controlled enrichment catalytic membrane. The electrically controlled enrichment catalytic membrane comprises a substrate layer and a copolymer coating layer having electrical redox reversibility. The substrate layer is a titanium oxide conductive ceramic membrane having a pore size of less than 1 micron. The material of the copolymer coating layer is an organic blended polymer TMA containing a nitro radical functional group. x -co-TMPMA (1-x) , 0<x<100, where x% represents the degree of oxidation.
[0008] Preferably, the value range of x is 18≤x≤84, and the copolymer TMA x -co-TMPMA (1-x) The degree of oxidation is 18 to 84%.
[0009] In a second aspect, the present invention provides a method for preparing the electrically controlled enrichment catalytic membrane described in the first aspect, and the preparation method is specifically as follows:
[0010] S1: 2-methyl-2-acrylic acid-2,2,6,6-tetramethyl-4-piperidinyl ester is dissolved in a nitrogen-blown deoxygenated N,N-dimethylformamide solution, and then azobisisobutyronitrile solution is added under anaerobic conditions to carry out polymerization reaction to obtain a polymer solution. The polymer solution is added to a 20-80wt.% methanol solution until a first precipitate appears, and then the first precipitate is filtered and freeze-dried to obtain a polymer PTMPMA.
[0011] S2: dissolving the polymer PTMPMA prepared in S1 in a tetrahydrofuran solution, wherein the concentration of the polymer PTMPMA is 1 to 3 g / mL, adding the solution to an oxidant after cooling and mixing evenly to obtain a mixed solution containing partially oxidized polymer PTMPMA; the oxidant is a tetrahydrofuran solution of m-chloroperbenzoic acid.
[0012] The mixed solution containing the partially oxidized polymer PTMPMA is added to a sodium hydroxide solution until a second precipitate appears, and then the second precipitate is separated and washed thoroughly, and then freeze-dried to obtain copolymers TMA with different oxidation degrees. x -co-TMPMA (1-x) .
[0013] S3: The copolymer TMA obtained in S2 x -co-TMPMA (1-x) and nano-carbon tubes are dissolved in N,N-dimethylformamide solution in a mass ratio of (1-4): (4-1) to obtain a precursor solution. The precursor solution is repeatedly spin-coated on the upper surface of the substrate film as a copolymer coating layer to obtain an electrically controlled enriched catalytic membrane.
[0014] Preferably, the concentration of 2-methyl-2-acrylic acid-2,2,6,6-tetramethyl-4-piperidinyl ester dissolved in N,N-dimethylformamide solution in S1 is 40-50 mmol. The concentration of azobisisobutyronitrile in the polymer solution is 2-4 g / L.
[0015] Preferably, the mass ratio of the polymer PTMPMA to m-chloroperbenzoic acid in the mixed solution containing the partially oxidized polymer PTMPMA in S2 is 10:(0.174-0.995). The concentration of the sodium hydroxide solution in S2 is 0.4-0.6M.
[0016] Preferably, the second precipitate is fully washed in S2 as follows: the second precipitate is dissolved in a tetrahydrofuran solution for washing, and then pure methanol, 20 wt.% methanol and deionized water are used in sequence to fully wash and remove the tetrahydrofuran solution.
[0017] Preferably, the volume of the precursor solution spin-coated in S3 is 0.2-2 mL.
[0018] Preferably, the base film is a titanium suboxide conductive ceramic film with a diameter of 0.5 to 5 cm and a thickness of 0.2 to 3 mm.
[0019] Preferably, the spin coating treatment is performed using a spin coater at a rotation speed of 30 r / min for 5 to 30 s and then at a rotation speed of 600 r / min for 30 to 90 s.
[0020] In a third aspect, the present invention provides an application of the electrically controlled enrichment catalytic membrane described in the first aspect in water treatment. Two electrically controlled enrichment catalytic membranes are arranged as filter membranes in an electrochemical water treatment device, and the two filter membranes are respectively connected to the positive and negative electrodes of the AC system, and the positive and negative electrodes are reversed within a cycle; the contaminated solution is controlled to flow through the two filter membranes in sequence, and the hydrophobic organic pollutants in the contaminated solution are adsorbed and oxidized and removed by adjusting the positive bias and negative bias parameters on the filter membranes.
[0021] Preferably, the hydrophobic organic pollutant is one or more of phenol, sulfamethoxazole or carbamazepine.
[0022] Preferably, the difference between the positive bias voltage and the negative bias voltage is in the range of 1.2 to 3.6V.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The present invention provides an electrically controlled enrichment catalytic membrane, which has a copolymer coating layer with electrical redox reversibility on the membrane surface and can be applied to an electrocatalytic membrane system. When the membrane electrode gains or loses electrons, the adsorption-oxidation process is realized respectively, thereby being able to efficiently remove hydrophobic organic pollutants.
[0025] (2) The electrically controlled enrichment catalytic membrane provided by the present invention is generally only applicable to a class of organic matter with very similar redox potentials and chemical structures, while the membrane provided by the present invention can remove different types of hydrophobic organic pollutants by regulating voltage. The adsorption amount of the three organic pollutants by the membrane containing the copolymer coating layer prepared in this embodiment is 1.31 to 2.13 times that of the control example. Therefore, the use of electrically controlled enrichment catalytic membranes to selectively remove organic pollutants by voltage regulation has great application potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The present invention provides a method for preparing an electrically controlled enriched catalytic membrane, wherein a is a flow chart for preparing a copolymer coating layer material; b is a schematic diagram for spin coating of a copolymer coating layer;
[0027] Figure 2 The scanning electron microscope images of the electrically controlled enriched catalytic membrane prepared in Example 2, wherein a is a scanning electron microscope image of the surface of the electrically controlled enriched catalytic membrane, and b is a scanning electron microscope image of the surface of the electrically controlled enriched catalytic membrane covered with carbon nanotubes;
[0028] Figure 3 This is a graph showing the pore size of the electrically controlled enriched catalytic membrane prepared in Example 2 measured by mercury pressure measurement;
[0029] Figure 4 The EPR result diagram of the electrically controlled enrichment catalytic membrane copolymer coating layer prepared in Examples 1 to 3 and the comparative example;
[0030] Figure 5 This is a CV curve diagram of the copolymer coating layer of the electrically controlled enriched catalyst membrane prepared in Example 2;
[0031] Figure 6 (a) removal performance and (b) separation coefficient of the membrane system for coexisting pollutants when different alternating currents are applied;
[0032] Figure 7 (a) Current utilization efficiency and (b) energy consumption of the membrane system for coexisting pollutants when different alternating currents are applied;
[0033] Figure 8 This is a graph showing the removal rate of organic pollutants by the electrically controlled enrichment catalytic membrane prepared in Example 2 and the comparative example as an electrode of an electrochemical water treatment device;
[0034] Fig. 9 This is a schematic diagram of the application of the electrically controlled enrichment catalytic membrane prepared in Example 2 in an electrochemical water treatment device. DETAILED DESCRIPTION
[0035] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific implementation mode of the present invention is described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below. The technical features in each embodiment of the present invention can be combined accordingly without conflicting with each other.
[0036] In order to further demonstrate the performance of the above-mentioned electrically controlled enrichment catalytic membrane of the present invention, the present invention further demonstrates its function and effect through examples.
[0037] Example 1
[0038] This example prepares an electrically controlled enrichment catalytic membrane containing a copolymer coating layer with an oxidation degree of 18%. The specific steps are described below:
[0039] (1) Synthetic polymer PTMPMA
[0040] Under heating conditions of 30-40°C, 10 g of 2-methyl-2-acrylic acid-2,2,6,6-tetramethyl-4-piperidinyl ester (TMPMA) was fully dissolved in 25 mL of nitrogen-deoxygenated N,N-dimethylformamide (DMF) to obtain a TMPMA concentration of 45.5 mmol. Subsequently, under anaerobic conditions (nitrogen was continuously introduced and the rotor was used for stirring), azobisisobutyronitrile solution (AIBN) was slowly added to the above solution in small amounts and multiple times to carry out polymerization reaction. The above polymerization reaction was carried out at 60°C for 16 hours to obtain a polymer solution. The concentration of AIBN in the polymer solution was 3 g / L.
[0041] The polymer solution was slowly added to 2000 mL of 20% (w / w) methanol solution through a syringe until the first precipitate appeared. The first precipitate was then filtered and freeze-dried to obtain a white polymer PTMPMA.
[0042] (2) Partial oxidation of polymer PTMPMA
[0043] 0.174 g of m-chloroperoxybenzoic acid (mCPBA) was dissolved in 3.75 mL of THF and stirred for 1 h to obtain an orange-yellow oxidant. 10 g of the polymer PTMPMA obtained in step (1) was dissolved in 5 mL of tetrahydrofuran (THF) and cooled in an ice bath, then added to the above oxidant and mixed evenly to obtain a mixed solution containing partially oxidized polymer PTMPMA, wherein the mass ratio of polymer PTMPMA to m-chloroperoxybenzoic acid was 10:0.174.
[0044] The above solution containing partially oxidized polymer PTMPMA is slowly added dropwise to 50 mL of 0.5 M sodium hydroxide solution (NaOH) until a second precipitate appears. The second precipitate is filtered and dissolved again in 7.5 mL of THF to fully wash away the oxidant m-chloroperbenzoic acid (mCPBA). Then, 125 mL of pure methanol, 20% (w / w) methanol and deionized water are used to fully wash away THF. The washed precipitate is vacuum filtered and freeze-dried, and the degree of oxidation is determined by a UV spectrophotometer to obtain a polymer with an oxidation degree of 18%, which is recorded as TMA. 18 -co-TMPMA 82 .
[0045] (3) Preparation of electrically controlled enrichment catalytic membrane
[0046] 5 mg of carbon nanotubes (CNT) and 5 mg of TMA prepared in step (2) were added. 18 -co-TMPMA 82 The powder was dissolved in 1 mL of DMF and ultrasonicated in an ice bath for 1 h to obtain a precursor solution. 1 mL of the precursor solution was repeatedly spin-coated as a copolymer coating layer on the surface of a sub-titanium oxide conductive ceramic membrane with a diameter of 2.5 cm and a thickness of 1.5 mm. The spin coating process was performed using a spin coater at a speed of 30 r / min for 10 s and then at a speed of 600 r / min for 60 s. After drying, an electrically controlled enriched catalytic membrane was obtained.
[0047] like Figure 1 a and Figure 1 b shows that the electrically controlled enriched catalytic membrane provided by the present invention uses a high-speed spin coating method to partially oxidize the TMPMA polymer (TMA) x -co-TMPMA 1-x ) is coated on a sub-titanium oxide ceramic membrane with a diameter of 2.5 cm and a thickness of 1.5 mm.
[0048] Example 2
[0049] This example prepares an electrically controlled enrichment catalytic membrane containing a copolymer coating layer with an oxidation degree of 51%. The specific steps are described below:
[0050] (1) Synthetic polymer PTMPMA
[0051] Under heating conditions of 30-40°C, 10 g of 2-methyl-2-acrylic acid-2,2,6,6-tetramethyl-4-piperidinyl ester (TMPMA) was fully dissolved in 25 mL of nitrogen-deoxygenated N,N-dimethylformamide (DMF) to obtain a TMPMA concentration of 45.5 mmol. Subsequently, under anaerobic conditions (nitrogen was continuously introduced and the rotor was used for stirring), azobisisobutyronitrile solution (AIBN) was slowly added to the above solution in small amounts and multiple times to carry out polymerization reaction. The above polymerization reaction was carried out at 60°C for 16 hours to obtain a polymer solution. The concentration of AIBN in the polymer solution was 3 g / L.
[0052] The polymer solution was slowly added to 2000 mL of 20% (w / w) methanol solution through a syringe until the first precipitate appeared, and then the first precipitate was filtered and freeze-dried to obtain a white polymer PTMPMA. The yield of the polymer PTMPMA was 81.03%.
[0053] (2) Partial oxidation of polymer PTMPMA
[0054] 0.585 g of m-chloroperbenzoic acid (mCPBA) was dissolved in 3.75 mL of THF and stirred for 1 h to obtain an orange-yellow oxidant. 10 g of the polymer PTMPMA obtained in step (1) was dissolved in 5 mL of tetrahydrofuran (THF) and cooled in an ice bath, then added to the above oxidant and mixed evenly to obtain a mixed solution containing partially oxidized polymer PTMPMA, wherein the mass ratio of polymer PTMPMA to m-chloroperbenzoic acid was 10:0.585.
[0055] The above solution containing partially oxidized polymer PTMPMA is slowly added dropwise to 50 mL of 0.5 M sodium hydroxide solution (NaOH) until a second precipitate appears. The second precipitate is filtered and dissolved again in 7.5 mL of THF to fully wash away the oxidant m-chloroperbenzoic acid (mCPBA). Then, 125 mL of pure methanol, 20% (w / w) methanol and deionized water are used to fully wash away THF. The washed precipitate is vacuum filtered and freeze-dried, and the degree of oxidation is determined by a UV spectrophotometer to obtain a polymer with an oxidation degree of 51%, which is recorded as TMA. 51 -co-TMPMA 49 .
[0056] (3) Preparation of electrically controlled enrichment catalytic membrane
[0057] 5 mg of carbon nanotubes (CNT) and 5 mg of TMA prepared in step (2) were added. 51 -co-TMPMA49 The powder was dissolved in 1 mL of DMF and ultrasonicated in an ice bath for 1 h to obtain a precursor solution. 1 mL of the precursor solution was repeatedly spin-coated as a copolymer coating layer on the surface of a sub-titanium oxide conductive ceramic membrane with a diameter of 2.5 cm and a thickness of 1.5 mm. The spin coating process was performed using a spin coater at a speed of 30 r / min for 10 s and then at a speed of 600 r / min for 60 s. After drying, an electrically controlled enriched catalytic membrane was obtained.
[0058] Example 3
[0059] This example prepares an electrically controlled enrichment catalytic membrane containing a copolymer coating layer with an oxidation degree of 84%. The specific steps are described below:
[0060] (1) Synthetic polymer PTMPMA
[0061] Under heating conditions of 30-40°C, 10 g of 2-methyl-2-acrylic acid-2,2,6,6-tetramethyl-4-piperidinyl ester (TMPMA) was fully dissolved in 25 mL of nitrogen-deoxygenated N,N-dimethylformamide (DMF) to obtain a TMPMA concentration of 45.5 mmol. Subsequently, under anaerobic conditions (nitrogen was continuously introduced and the rotor was used for stirring), azobisisobutyronitrile solution (AIBN) was slowly added to the above solution in small amounts and multiple times to carry out polymerization reaction. The above polymerization reaction was carried out at 60°C for 16 hours to obtain a polymer solution. The concentration of AIBN in the polymer solution was 3 g / L.
[0062] The polymer solution was slowly added to 2000 mL of 20% (w / w) methanol solution through a syringe until the first precipitate appeared. The first precipitate was then filtered and freeze-dried to obtain a white polymer PTMPMA.
[0063] (2) Partial oxidation of polymer PTMPMA
[0064] 0.995 g of m-chloroperbenzoic acid (mCPBA) was dissolved in 3.75 mL of THF and stirred for 1 h to obtain an orange-yellow oxidant. 10 g of the polymer PTMPMA obtained in step (1) was dissolved in 5 mL of tetrahydrofuran (THF) and cooled in an ice bath, then added to the above oxidant and mixed evenly to obtain a mixed solution containing partially oxidized polymer PTMPMA, wherein the mass ratio of polymer PTMPMA to m-chloroperbenzoic acid was 10:0.995.
[0065] The above solution containing partially oxidized polymer PTMPMA is slowly added dropwise to 50 mL of 0.5 M sodium hydroxide solution (NaOH) until a second precipitate appears. The second precipitate is filtered and dissolved again in 7.5 mL of THF to fully wash away the oxidant m-chloroperbenzoic acid (mCPBA). Then, 125 mL of pure methanol, 20% (w / w) methanol and deionized water are used to fully wash away THF. The washed precipitate is vacuum filtered and freeze-dried, and the degree of oxidation is determined by a UV spectrophotometer to obtain a polymer with an oxidation degree of 51%, which is recorded as TMA. 84 -co-TMPMA 16 .
[0066] (3) Preparation of electrically controlled enrichment catalytic membrane
[0067] 5 mg of carbon nanotubes (CNT) and 5 mg of TMA prepared in step (2) were added. 84 -co-TMPMA 16 The powder was dissolved in 1 mL of DMF and ultrasonicated in an ice bath for 1 h to obtain a precursor solution. 1 mL of the precursor solution was repeatedly spin-coated as a copolymer coating layer on the surface of a sub-titanium oxide conductive ceramic membrane with a diameter of 2.5 cm and a thickness of 1.5 mm. The spin coating process was performed using a spin coater at a speed of 30 r / min for 10 s and then at a speed of 600 r / min for 60 s. After drying, an electrically controlled enriched catalytic membrane was obtained.
[0068] Example 4
[0069] In order to evaluate the performance of the electrically controlled enrichment catalytic membrane provided by the present invention, this example uses the electrically controlled enrichment catalytic membrane prepared in Example 2 as the positive electrode and negative electrode materials in the electrochemical water treatment device, such as Fig. 9 As shown. Phenol, sulfamethoxazole (SMX) and carbamazepine (CBZ) were used as hydrophobic organic pollutants for removal experiments. The specific steps are as follows:
[0070] A mixed solution containing 10 mg / L of SMX, phenol, and CBZ was added as a contaminated solution to the electrochemical water treatment device, wherein the relevant information in the contaminated solution is shown in Table 1. The electrically controlled enrichment catalytic membrane prepared in Example 2 was used as the positive and negative electrode materials in the electrochemical water treatment device, the electrolyte was 100 mM sodium sulfate, the reference electrode was Ag / AgCl, and an alternating current system was used, that is, the applied voltage was periodically reversed between negative bias and positive bias, as shown in Table 2. The difference between positive and negative bias ΔE = [E +-E-]) are 1.2, 2.4 and 3.6V respectively. This setting is based on the theoretical values of the adsorption, direct oxidation of electrodes and indirect oxidation of free radicals of the three pollutants, and can ensure that the side reaction of hydrolysis and hydrogen production does not occur. The pulse period is 0.01(s), and the difference between the positive and negative bias voltages is 1.2V, 2.4V, and 3.6V respectively. The measured dissolved oxygen content is 6.4-8.8mg / L.
[0071] Table 1 Pollutant related information
[0072]
[0073] Table 2 Theoretical oxidation reactions of the alternating current applied to the catalytic membrane and various pollutant systems
[0074]
[0075] Oxidation reaction of pollutants at the electrode: direct oxidation (DO); indirect oxidation (IDO)
[0076] The separation factor (SF) of the electrically controlled enrichment catalytic membrane to remove organic pollutants from the polluted solution is calculated by the following formula:
[0077]
[0078] The current utilization efficiency (%) of the electrically controlled enriched catalytic membrane to remove organic pollutants per mole of mass is calculated by the following formula:
[0079]
[0080] Where n is the molar number of the corresponding pollutant, F is the Faraday constant, z is the number of electron transfers involved in the removal of the corresponding pollutant; and i is the current value recorded by the electrochemical workstation.
[0081] The energy consumption (EC, %) required for each mole of pollution removal is calculated by the following formula:
[0082]
[0083] Where Ewe is the working electrode potential and Ece is the counter electrode potential.
[0084] Comparative Example
[0085] This comparative example prepares an electrically controlled enrichment catalytic membrane containing a copolymer coating layer that has not been partially oxidized. The specific steps are described below:
[0086] (1) Synthetic polymer PTMPMA
[0087] Under heating conditions of 30-40°C, 10 g of 2-methyl-2-acrylic acid-2,2,6,6-tetramethyl-4-piperidinyl ester (TMPMA) was fully dissolved in 25 mL of nitrogen-deoxygenated N,N-dimethylformamide (DMF) to obtain a TMPMA concentration of 45.5 mmol. Subsequently, under anaerobic conditions (nitrogen was continuously introduced and the rotor was used for stirring), azobisisobutyronitrile solution (AIBN) was slowly added to the above solution in small amounts and multiple times to carry out polymerization reaction. The above polymerization reaction was carried out at 60°C for 16 hours to obtain a polymer solution. The concentration of AIBN in the polymer solution was 3 g / L.
[0088] The polymer solution was slowly added to 2000 mL of 20% (w / w) methanol solution through a syringe until the first precipitate appeared. The first precipitate was then filtered and freeze-dried to obtain a white polymer PTMPMA as a copolymer coating layer that was not partially oxidized.
[0089] (2) Preparation of electrically controlled enrichment catalytic membrane
[0090] Dissolve 5 mg of carbon nanotubes (CNT) and 5 mg of the polymer PTMPMA powder prepared in step (1) in 1 mL of DMF, and ultrasonicate in an ice bath for 1 h to obtain a precursor solution. Spin-coat 1 mL of the precursor solution as a copolymer coating layer on the upper surface of a titanium oxide conductive ceramic membrane with a diameter of 2.5 cm and a thickness of 1.5 mm. Spin-coating is performed using a spin coater at a speed of 30 r / min for 10 s and then at a speed of 600 r / min for 60 s. After drying, an electrically controlled enriched catalytic membrane is obtained.
[0091] The following is an analysis of the experimental results:
[0092] Figure 2 a and Figure 2 b are scanning electron microscope images of the surface of the electrically controlled enriched catalytic membrane prepared in Example 2 and the surface carbon nanotubes covering the membrane. Figure 3 The pore size of the electrically controlled enriched catalyst membrane prepared in Example 2 is measured by mercury pressure method, where CM is a catalyst membrane without a copolymer coating layer, and PTMA-CM is an electrically controlled enriched catalyst membrane with a copolymer coating layer spin-coated thereon prepared in Example 2. Figure 2 a. Figure 2 b and Figure 3 It can be seen that the pore size of the electrically controlled enrichment catalytic membrane substrate prepared in Example 2 is slightly smaller than 1 μm, the copolymer coating layer has little effect on the pore size of the substrate membrane, and the carbon nanotubes serve as cross-linking agents and cover the surface of the membrane.
[0093] Figure 4The EPR structures of the electrically controlled enriched catalytic membranes containing copolymer coating layers with different oxidation degrees prepared in Examples 1 to 3 and Comparative Examples are shown. The EPR results show that stable N=O· free radicals are observed, and the signal intensity related to the spin density of free radicals increases with the increase of the oxidation degree, and the hydrophobicity increases, and the adsorption capacity for hydrophobic pollutants increases.
[0094] Figure 5 The CV curve results show that the nitro radicals and NO functional groups on the copolymer coating layer in the electrically controlled enriched catalytic membrane prepared in Example 2 have redox reversibility.
[0095] Figure 6 a Figure 6 b are the removal performance and separation coefficient of three coexisting organic pollutants under different voltage differences. The results show that under the coexistence of three pollutants, when the electrode membrane is not powered (OC), CBZ has a larger removal amount (separation coefficient is 1.645) than the other two pollutants, indicating that when there is no power, the electrically controlled enrichment catalytic membrane preferentially adsorbs CBZ. SMX has a larger removal amount at 1.2 and 2.4V (separation coefficient is 1.243-1.859), and phenol (Phenol) at 3.6V (separation coefficient is 2.145). Therefore, the target organic pollutant in the coexisting pollution system can be selectively removed by voltage regulation.
[0096] Figure 7 a and Figure 7 b is the calculation diagram of the current utilization efficiency and unit energy consumption of the electric control enrichment catalytic membrane system for removing specific organic pollutants per mole. Taking SMX as an example, the removal of SMX at a potential difference of 2.4V, the utilization efficiency and unit energy consumption of the applied alternating current of [-0.1, 2.3]V are 1.8×10 -2 % and 0.02564 kWh / mol; the utilization efficiency and unit energy consumption of the applied [-0.5, 1.9] V AC were 9.6×10 -2 % and 0.02964 kWh / mol. Under the same potential difference, compared with applying [-0.1, 2.3] V AC, the catalytic membrane system with a negative bias of -0.5 V and a positive bias of 1.9 V ([-0.5, 1.9] V) AC has a higher removal rate, higher current utilization efficiency and lower unit energy consumption, so the treatment cost is lower.
[0097] according to Figure 8 It can be seen that when the alternating current [-0.5, 1.9] V is applied, the adsorption amount of the three pollutants by the membrane containing the copolymer coating layer prepared in Example 2 is 1.31 to 2.13 times that of the control example, that is, the enrichment multiple is 1.31 to 2.13. This shows that the electrically controlled enrichment membrane provided by the present invention can efficiently remove organic pollutants in polluted water.
[0098] The above-described embodiment is only a preferred solution of the present invention, but it is not intended to limit the present invention. A person skilled in the relevant technical field may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.
Claims
1. An electrically controlled enrichment catalytic membrane, characterized in that: The electrically controlled enrichment catalytic membrane comprises a base layer and a copolymer coating layer with electrical redox reversibility; the base layer is a titanium oxide conductive ceramic membrane with a pore size of less than 1 micron; the material of the copolymer coating layer is an organic blended polymer TMA containing a nitro radical functional group x -co-TMPMA (1-x) , 0<x<100, where x% represents the degree of oxidation.
2. The electrically controlled enrichment catalytic membrane according to claim 1, characterized in that: The value range of x is 18≤x≤84, and the copolymer TMA x -co-TMPMA (1-x) The degree of oxidation is 18 to 84%.
3. A method for preparing an electrically controlled enrichment catalytic membrane according to claim 1 or 2, characterized in that: The preparation method is as follows: S1: dissolving 2-methyl-2-acrylic acid-2,2,6,6-tetramethyl-4-piperidinyl ester in a nitrogen-blown deoxygenated N,N-dimethylformamide solution, and then adding an azobisisobutyronitrile solution under anaerobic conditions to carry out polymerization reaction to obtain a polymer solution; adding the polymer solution to a 20-80wt.% methanol solution until a first precipitate appears, and then filtering the first precipitate and freeze-drying it to obtain a polymer PTMPMA; S2: dissolving the polymer PTMPMA prepared in S1 in a tetrahydrofuran solution, wherein the concentration of the polymer PTMPMA is 1 to 3 g / mL, cooling and adding the solution to an oxidant and mixing evenly to obtain a mixed solution containing partially oxidized polymer PTMPMA; the oxidant is a tetrahydrofuran solution of m-chloroperbenzoic acid; The mixed solution containing the partially oxidized polymer PTMPMA is added to a sodium hydroxide solution until a second precipitate appears, and then the second precipitate is separated and washed sufficiently, and then freeze-dried to obtain copolymers TMA with different oxidation degrees. x -co-TMPMA (1-x) ; S3: The copolymer TMA obtained in S2 x -co-TMPMA (1-x) and carbon nanotubes are dissolved in N,N-dimethylformamide solution in a mass ratio of (1-4):(4-1) to obtain a precursor solution; The precursor solution is used as a copolymer coating layer and is repeatedly spin-coated on the upper surface of the substrate membrane to obtain an electrically controlled enriched catalytic membrane.
4. The method for preparing the electrically controlled enrichment catalytic membrane according to claim 3, characterized in that: The concentration of 2-methyl-2-acrylic acid-2,2,6,6-tetramethyl-4-piperidinyl ester dissolved in N,N-dimethylformamide solution in S1 is 40-50 mmol; the concentration of azobisisobutyronitrile in the polymer solution is 2-4 g / L.
5. The method for preparing the electrically controlled enrichment catalytic membrane according to claim 3, characterized in that: The mass ratio of the polymer PTMPMA to m-chloroperbenzoic acid in the mixed solution containing partially oxidized polymer PTMPMA in the S2 is 10:(0.174-0.995); the concentration of the sodium hydroxide solution in the S2 is 0.4-0.6M.
6. The method for preparing the electrically controlled enrichment catalytic membrane according to claim 3, characterized in that: The second precipitate is fully washed in S2 by dissolving the second precipitate in a tetrahydrofuran solution for washing, and then fully washed with pure methanol, 20 wt.% methanol and deionized water in sequence to remove the tetrahydrofuran solution.
7. The method for preparing the electrically controlled enrichment catalytic membrane according to claim 3, characterized in that: The volume of the precursor solution spin-coated in S3 is 0.2-2 mL.
8. The method for preparing the electrically controlled enrichment catalytic membrane according to claim 3, characterized in that: The base film is a titanium suboxide conductive ceramic film with a diameter of 0.5 to 5 cm and a thickness of 0.2 to 3 mm.
9. The method for preparing the electrically controlled enrichment catalytic membrane according to claim 3, characterized in that: The spin coating treatment uses a spin coater, with a rotation speed of 30 r / min for 5 to 30 s and then a rotation speed of 600 r / min for 30 to 90 s.
10. An application of the electrically controlled enrichment catalytic membrane according to claim 1 or 2 in water treatment, characterized in that: Two of the electrically controlled enrichment catalytic membranes are arranged as filter membranes in an electrochemical water treatment device, and the two filter membranes are respectively connected to the positive and negative electrodes of an alternating current system; the polluted solution is controlled to flow through the two filter membranes in sequence, and the hydrophobic organic pollutants in the polluted solution are adsorbed and oxidized and removed by adjusting the positive bias and negative bias parameters on the filter membranes; preferably, the hydrophobic organic pollutants are one or more of phenol, sulfamethoxazole or carbamazepine; preferably, the difference between the positive and negative bias voltages is in the range of 1.2 to 3.6V.
Citation Information
Patent Citations
Antimicrobial polymers and coatings
CN102131836A
Triazine ring covalent organic polymer and electrode material, as well as preparation method and application thereof
CN108976417A
Treatment technology for degrading antibiotic wastewater by electrochemistry and membrane filtration coupling system
CN110498491A
Polymer electrolyte membrane, method of preparing the same and fuel cell including the same
US20070190385A1
Electroactivated film with polymer GEL electrolyte
WO2009143314A2
Cited By
Electrochemical water treatment method based on TEMPO modified ceramic membrane
CN120117710A
TEMPO-CNT composite membrane based on layer-by-layer assembly, preparation method and application
CN121974447A
Tempos-cnt composite membrane based on layer-by-layer assembly, preparation method and application
CN121974447B