A PTS process for graphite bearings for automobile water pumps
The brittleness of graphite bearings is solved by using nano-microcapsules prepared by using plant extracts and sodium alginate in graphite bearings and the silicon carbide layer is formed and the nano-microcapsules are loaded on carbon fibers. The rolling friction of nanobismuth copper powder is combined with the brittleness of graphite bearings and Fluidity issues improve lubrication and mechanical properties and extend service life.
Patent Information
- Application Number
- CN202411293452.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-14
AI Technical Summary
The graphite bearings of carbon graphite materials are not strong due to the properties of brittle materials, light powder quality and poor fluidity, which affect the mixing uniformity and wear resistance. Nanobodies particles are prone to fall off during friction wear, resulting in poor operating stability of friction pairs.
Plant extracts are used as core material and sodium alginate as wall material to prepare nano microcapsules, which adhere to the surface of graphite powder and carbon powder to form a silicon carbide layer, improving lubricating effect and mechanical properties; nanobiscus copper powder is used in graphene oxide Rolling friction forms on the surface to reduce friction factor; carbon fibers are used as carriers to load nano microcapsules to improve density and mechanical properties.
It improves the lubricating effect, mechanical properties and wear resistance of graphite bearings, extends service life, enhances friction stability and compactness, avoids powder bypass and agglomeration, and improves the density and dimensional stability of the bearings.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of graphite bearing production, in particular to a PTS process for graphite bearings for automobile water pumps. Background Art
[0002] The demand for carbon material parts in the automotive and home appliance industries is growing rapidly. The water pump, power tool and other industries have put forward higher requirements on the wear resistance and service life of carbon material parts. The development of high-quality, low-cost carbon material parts is the future development trend. The PTS (Press To Size) process of carbon graphite bearings refers to the use of carbon powder as raw material, through batching, kneading, crushing, granulation, molding, sintering, impregnation, processing and other processes, to prepare parts products that require little or no processing; it has high material utilization, high product stability, short process, and the graphite bearings for automotive water pumps have good wear resistance.
[0003] Carbon graphite material is a brittle material. The inherent strength of the prepared graphite bearings is not high, which limits the use of graphite bearings. In addition, the powder is light and has poor fluidity, which affects the uniformity of mixing and is prone to bridging, resulting in uneven material distribution, which in turn affects the performance of the graphite bearings. Impregnating the surface of the graphite bearing with nano-bismuth can improve the lubricity of the graphite bearing, but the nano-bismuth particles have poor ductility and are brittle. During the friction and wear process, the nano-bismuth particles precipitated in the friction contact area are easily detached from the wear surface, resulting in poor operating stability of the friction pair and affecting the wear resistance. Summary of the invention
[0004] The purpose of the present invention is to provide a PTS process for graphite bearings for automobile water pumps: plant extracts are used as core materials, sodium alginate is used as wall materials, and the formed nano-microcapsules adhere to the surfaces of graphite powder and carbon powder. When the graphite powder and carbon powder are piled up and bridged, and the friction force increases, the friction force generated causes the nano-microcapsules to rupture, releasing the plant extracts, which are filled into the gaps between the carbon powder particles of the bearing raw material, thereby improving the lubrication effect. In addition, during the high-temperature sintering process, the silicon element in the released plant extracts can react with the carbon element on the surface of the resin adhesive, graphite powder, and carbon powder to form a silicon carbide layer coated on the surface of the carbon powder, thereby improving the retention of the carbon phase in the graphite bearing and enhancing the mechanical properties of the graphite bearing; the nano-microcapsules are deposited on the surface of the carbon fiber. Carbon fiber is used as a carrier of nano-microcapsules and can load more nano-microcapsules. Carbon fiber is used as a reinforcing filler and has good fluidity during the sintering process. It can be filled into the pores of graphite powder and carbon powder to improve the density of the graphite bearing. Nano-bismuth copper powder is formed on the surface of graphene oxide to avoid agglomeration of the formed nano-bismuth copper powder, which leads to a decrease in lubricity. The formed nano-bismuth copper powder moves relative to each other between the friction pairs of the graphite bearing to form rolling friction, reduce the friction coefficient, reduce wear, and also play the role of micro-bearing and support. The nano-bismuth copper graphene oxide loaded with nano-bismuth copper is dispersed in unsaturated aldehyde ester to form a composite resin impregnating agent, which is filled into the surface of the graphite bearing and its pores to improve the density of the graphite bearing.
[0005] The technical problems to be solved by the present invention are as follows: carbon graphite material is a brittle material, and the inherent strength of the prepared graphite bearings is not high, which limits the use of graphite bearings. In addition, the powder is light and has poor fluidity, which affects the uniformity of mixing and is prone to bridging, resulting in uneven material distribution, which in turn affects the performance of the graphite bearings. Impregnating the surface of the graphite bearing with nano-bismuth can improve the lubricity of the graphite bearing, but the nano-bismuth particles have poor ductility and are brittle. During the friction and wear process, the nano-bismuth particles precipitated in the friction contact area are easily detached from the wear surface, resulting in poor operating stability of the friction pair and affecting the wear resistance.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A PTS process for graphite bearings for automobile water pumps comprises the following steps:
[0008] S1. Graphite powder, carbon powder and composite adhesive are mixed, kneaded and crushed to obtain a mixture.
[0009] S2. Place the mixed material in a granulator for granulation and molding to obtain composite particles.
[0010] S3. Sintering and carbonizing the composite particles to obtain an initial graphite bearing.
[0011] S4. The initial graphite bearing is impregnated into a composite resin impregnating agent, taken out, cured, and processed to obtain a graphite bearing for an automobile water pump.
[0012] Furthermore, the mass ratio of graphite powder, carbon powder and composite adhesive is (70-80):(10-20):(6-8).
[0013] Furthermore, the particle size of graphite powder and carbon powder is 10-20 μm.
[0014] Furthermore, the kneading temperature is 70-90° C. and the time is 1-3 h.
[0015] Furthermore, the sintering carbonization temperature is 2000-2100° C., and the sintering carbonization time is 4-8 hours.
[0016] Furthermore, the graphite bearing for automobile water pump has a diameter of 40-50 mm and a thickness of 10-30 mm.
[0017] Furthermore, the curing temperature is 140-160° C., and the curing time is 20-30 min.
[0018] Furthermore, the composite adhesive is prepared by depositing nano-microcapsules on the surface of carbon fibers and then mixing with phenolic resin.
[0019] Furthermore, the carbon fiber has a diameter of 50-100 nm and a length of 5-10 μm.
[0020] Furthermore, the composite adhesive is specifically prepared by the following steps:
[0021] A1. Add nanocapsules to deionized water, stir evenly, add carbon fiber, KH550 and ethanol, stir and react at 40°C for 5 minutes, filter, wash with deionized water 3 times, and dry in an oven at 85°C for 10 minutes to obtain modified carbon fiber.
[0022] Among them, KH550 is used as a cross-linking agent. The silanol produced by hydrolysis can react with the hydroxyl groups on the surface of the nano-capsules, and the amino groups of KH550 react with the hydroxyl groups on the surface of the carbon fibers, so that the nano-capsules are deposited on the carbon fibers. During the sintering process, the plant extracts released from the nano-capsules loaded on the surface of the carbon fibers contain silicon elements that can react with the carbon elements on the surface of the carbon fibers, so that the carbon fibers and the carbon powder are combined through the silicon carbide layer of the solidified product of the plant extracts, so that the carbon fibers and the carbon powder raw materials are tightly combined, thereby improving the mechanical properties of the bearing.
[0023] Furthermore, the dosage ratio of nano-microcapsules, deionized water, carbon fiber, KH550, and ethanol is (0.2-0.3) g: (70-90) mL: (1-2) g: (0.3-0.7) g: (15-25) mL.
[0024] A2. The modified carbon fiber and liquid phenolic resin were mixed, stirred at 25°C for 30-45 minutes, and dried in an oven at 100°C for 10 minutes to remove moisture from the modified carbon fiber to obtain a composite adhesive.
[0025] Among them, the modified carbon fiber is mixed with liquid phenolic resin to form a composite adhesive, so that the modified carbon fiber adheres to the surface of graphite powder and carbon powder through the liquid phenolic resin to form a whole. During the melting process, the liquid phenolic resin can fill into the cracks and holes on the surface of multiple layers of graphite powder and carbon powder to form a stable and compact structure. Its dimensional stability further limits the large shrinkage that will occur during the sintering process.
[0026] Furthermore, the amount ratio of modified carbon fiber and liquid phenolic resin is (1-2) g: (25-35) mL.
[0027] Furthermore, the nano-microcapsules are prepared by using plant extracts as core materials and sodium alginate as wall materials; specifically, the nano-microcapsules are prepared by the following steps:
[0028] Sodium alginate was added into deionized water, stirred evenly at 50°C, and after it was completely dissolved, placed in a negative pressure oven at 50°C, and placed under negative pressure at -0.08MPa for 1h to remove internal bubbles, Tween 80 and plant extract were added, placed in a high-speed shearing machine, and sheared at 5000r / min for 15min, 2mL of 10mM calcium chloride solution was added, stirred and reacted for 10min to form nanocapsules, and dried at 50°C for 1h to dehydrate, thereby obtaining nano-microcapsules.
[0029] Among them, plant extract is used as core material and sodium alginate is used as wall material. Calcium ions in calcium chloride solution replace sodium ions to form calcium alginate wall material and evenly wrap the plant extract to form nano microcapsules. Under the action of phenolic resin adhesive, the nano microcapsules adhere to the surface of graphite powder and carbon powder, tightly bonding the graphite powder and carbon powder together to form an overall structure. During the mixing process, when the graphite powder and carbon powder accumulate and bridge, the friction force increases, the friction force generated causes the nano microcapsules to rupture, releasing the plant extract, which fills the gaps between the carbon powder particles of the bearing raw material, thereby improving the lubrication effect.
[0030] Furthermore, the dosage ratio of sodium alginate, deionized water, Tween 80, and plant extract is (0.3-0.7) g: (20-30) mL: (0.01-0.03) g: (2-2.6) g.
[0031] Furthermore, the plant extract is specifically prepared by the following steps:
[0032] The East Asian feather moss is washed with water, dried, and ground into powder in a grinder. The East Asian feather moss powder is added to deionized water, stirred at 80°C for 6 hours, filtered, and the solution is collected. Petroleum ether is added to the solution for degreasing. The solution is shaken, allowed to stand, separated, and the upper petroleum ether solution is removed, and then heated at 80°C to evaporate until it becomes viscous to obtain a plant extract.
[0033] Furthermore, the dosage ratio of the East Asian sclerocaria powder and deionized water is (1-2) g: (40-50) mL.
[0034] Furthermore, the composite resin impregnating agent is prepared by mixing the loaded nano-bismuth copper graphene oxide with unsaturated aldehyde ester, and is specifically prepared by the following steps: mixing the loaded nano-bismuth copper graphene oxide and the unsaturated aldehyde ester, stirring for 30-45 minutes at 25°C, vacuuming and pressurizing to 8.8MPa, maintaining for 5 hours and then taking out to obtain the composite resin impregnating agent.
[0035] Among them, the nano-bismuth copper on the surface of the loaded nano-bismuth copper oxide graphene contains a large number of hydroxyl groups, which can be dispersed in unsaturated aldehyde esters to form a composite resin impregnant, which is filled into the surface of the graphite bearing and its pores to improve the density of the graphite bearing.
[0036] Furthermore, the amount ratio of loaded nano-bismuth copper oxide graphene and unsaturated aldehyde ester is (0.6-1) g: (20-30) mL.
[0037] Furthermore, the nano-bismuth copper-loaded graphene oxide is prepared by a mixed reaction of a bismuth-copper composite emulsion and graphene oxide.
[0038] The bismuth-copper composite emulsion and graphene oxide were mixed and stirred evenly, allowed to stand for 10 minutes, and then stirred and reacted at 30° C. for 1 hour. The mixture was filtered, washed with deionized water for 3 times, and dried in an oven at 70° C. for 10 minutes to obtain nano-bismuth-copper-loaded graphene oxide.
[0039] The bismuth-copper composite emulsion is mixed with graphene oxide, and the bismuth ions and copper ions in the bismuth-copper composite emulsion can combine with the carboxyl and hydroxyl groups on the surface of the graphene oxide, so that the bismuth-copper composite emulsion is deposited on the surface of the graphene oxide. Hydrazine hydrate is used as a reducing agent, and the copper ions are reduced to copper atoms, and the copper atoms gather to form atomic clusters. Further, under the action of hydrazine hydrate, the bismuth ions are reduced to bismuth atoms, and the copper atomic clusters continuously absorb new bismuth atoms to become crystal nuclei, and the crystal nuclei further grow, so as to form 40-50nm nano-bismuth-copper powder on the surface of the graphene oxide, avoid the agglomeration of the formed nano-bismuth-copper powder, which leads to a decrease in lubricity, and the formed nano-bismuth-copper powder moves relative to each other between the friction pairs of the graphite bearing, forming rolling friction, reducing the friction coefficient, reducing wear, and also playing the role of micro-bearing and support.
[0040] Furthermore, the dosage ratio of bismuth-copper composite emulsion and graphene oxide is (8-12) mL: (0.1-0.3) g.
[0041] Further, the bismuth-copper composite emulsion is specifically prepared by the following steps:
[0042] Dodecylphenol polyoxyethylene ether, n-pentanol, cyclohexane and deionized water are mixed and stirred to obtain a mixed emulsion, bismuth nitrate and copper nitrate are added to the mixed emulsion, and stirred to obtain phase A at 25°C, hydrazine hydrate is mixed with the mixed emulsion, and stirred to obtain phase B at 25°C, and phase A is mixed with phase B to obtain a bismuth-copper composite emulsion.
[0043] Furthermore, the volume ratio of dodecylphenol polyoxyethylene ether, n-pentanol, cyclohexane and deionized water is (1-3):(0.5-1.5):(5-7):(25-35).
[0044] Furthermore, the dosage ratio of bismuth nitrate, copper nitrate and mixed emulsion is (2-2.2) g: (1.6-2) g: (80-120) mL.
[0045] Furthermore, the dosage ratio of hydrazine hydrate and mixed emulsion is (1-1.4) g: (8-12) mL.
[0046] Furthermore, compared with the prior art, the present invention has the following beneficial effects:
[0047] (1) In the technical scheme of the present invention, plant extract is used as the core material and sodium alginate is used as the wall material. Under the action of phenolic resin adhesive, the obtained nano-microcapsules adhere to the surface of graphite powder and carbon powder, tightly bonding the graphite powder and carbon powder together to form an integral structure. In the mixing process, when the graphite powder and carbon powder are piled up and bridged, the friction force increases. The friction force generated causes the nano-microcapsules to rupture, releasing the plant extract, which is filled into the gaps between the carbon powder particles of the bearing raw material, thereby improving the lubrication effect and making the carbon powder particles have better fluidity, avoiding the accumulation and agglomeration of graphite powder and carbon powder, resulting in poor mechanical strength of the prepared graphite bearing. The graphite powder and carbon powder mixture is granulated, and its small size structure can also improve the powder fluidity, so that the carbon powder is evenly filled and the mechanical properties are improved.
[0048] (2) In the technical solution of the present invention, the mixture of graphite powder and carbon powder is granulated and formed to obtain composite particles. During the high-temperature sintering process, the silicon element in the plant extract released can react with the carbon element in the phenolic resin binder, and the silicon element can also react with the carbon element on the surface of the graphite powder and carbon powder to form a silicon carbide layer coated on the surface of the carbon powder, which has the function of preventing impurities from penetrating into the graphite powder and carbon powder and affecting the mechanical properties of the bearing, and can also improve the retention of the carbon phase in the graphite bearing and enhance the mechanical properties of the graphite bearing; and the silicon carbide coating has excellent antioxidant properties, wear resistance and lubrication properties, which can effectively prevent the oxidation of the graphite material at high temperature, thereby extending the service life of the graphite bearing.
[0049] (3) In the technical solution of the present invention, nano-capsules are deposited on the surface of carbon fibers. Carbon fibers serve as carriers of nano-capsules and can carry more nano-capsules. Carbon fibers serve as reinforcing fillers and have good fluidity during the sintering process, and can be filled into the pores of graphite powder and carbon powder to improve the density of graphite bearings. During the sintering process, the silicon element contained in the plant extract released by the nano-capsules loaded on the surface of the carbon fibers can also react with the carbon element on the surface of the carbon fibers, so that the carbon fibers are combined with the graphite powder and carbon powder through the silicon carbide layer of the solidified product of the plant extract, so that the carbon fibers are tightly combined with the carbon powder raw materials, thereby improving the mechanical properties of the bearings. Phenolic resin serves as an adhesive and can be filled into the cracks and holes on the surface of the multi-layer graphite during the melting process to form a stable and compact structure. Its dimensional stability further limits the large shrinkage that occurs during the sintering process. After carbonization, the phenolic resin forms a smooth glassy carbon layer with a diameter of 200-500nm. Glassy carbon can effectively avoid the formation of internal pores. The bearing mixture formed after sintering has good density and mechanical properties and can maintain a stable dimensional structure.
[0050] (4) In the technical solution of the present invention, nano-bismuth has good lubrication properties, and a single nano-bismuth particle can significantly improve the friction reduction and anti-wear properties of the base oil. A microemulsion method is used to form a 40-50 nm nano-bismuth copper powder on the surface of graphene oxide to avoid agglomeration of the formed nano-bismuth copper powder, which leads to a decrease in lubricity. The formed nano-bismuth copper powder moves relative to the friction pair of the graphite bearing to form rolling friction, reduce the friction coefficient, reduce wear, and also play a role as a micro-bearing and support. In addition, during the friction and wear process of the graphite bearing, due to the effects of deformation, extrusion and frictional heat, the nano-bismuth copper powder melts, precipitates and spreads on the contact surface of the friction pair of the graphite bearing, which can effectively improve the friction and wear properties of the graphite bearing material.
[0051] (5) In the technical solution of the present invention, the nano-bismuth copper loaded on the surface of the graphene oxide contains a large number of hydroxyl groups, which can be dispersed in unsaturated aldehyde esters to form a composite resin impregnant, which is filled into the surface of the graphite bearing and its pores to improve the density of the graphite bearing. The nano-bismuth copper loaded on the graphene oxide is bonded to the surface of the graphite bearing through the nano-bismuth copper to form a sandwich structure. The nano-bismuth copper serves as a lubricating component, which can make the layers of the sandwich structure move back and forth, and the resulting micro-ball effect has a good lubrication effect. DETAILED DESCRIPTION
[0052] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] The raw materials used in the embodiments of the present invention are as follows: sodium alginate (chemically pure, Nanjing Tongying Biotechnology Co., Ltd.); calcium chloride solution (chemically pure, Weifang Ruidesheng Chemical Co., Ltd.); Tween 80 (chemically pure, Shanghai Zhongfeng Biotechnology Co., Ltd.); KH550 (Jinan Yongyue Chemical Co., Ltd., effective ingredient content 98%); liquid phenolic resin (BR2130, Henan Boren Building Materials Co., Ltd.); dodecylphenol polyoxyethylene ether (purity CP, Tianjin Chengfeng Chemical Reagent Factory); n-pentanol, cyclohexane (purity AR, Tianjin Damao Chemical Reagent Factory); bismuth nitrate (purity AR, Tianjin Komio Chemical Reagent Co., Ltd.); copper nitrate (purity AR, Tianjin Bodi Chemical Co., Ltd.); hydrazine hydrate (purity AR, 80%, Tianjin Damao Chemical Reagent Factory); graphene oxide (purity 99%, Shandong Jinan Huifengda Chemical Co., Ltd.); graphite powder, carbon powder (Zhuozhou Yourong New Material Technology Co., Ltd., industrial grade).
[0054] The unsaturated aldehyde ester is selected from the polymer of p-phenylphenol, p-tert-butylphenol and formaldehyde, and its CAS number is 52469-00-8.
[0055] The plant extract is specifically prepared by the following steps:
[0056] The East Asian hard feather moss was washed with water, dried, and ground into powder in a grinder. 1.5 g of the East Asian hard feather moss powder was added to 45 mL of deionized water, stirred at 80°C for 6 h, filtered, and the solution was collected. Petroleum ether was added to the solution for degreasing. After shaking, standing, and separating to remove the upper petroleum ether solution, it was heated at 80°C to evaporate until it became viscous to obtain a plant extract.
[0057] Example 1
[0058] The composite adhesive is specifically prepared by the following steps:
[0059] A1. Add 0.5 g of sodium alginate to 25 mL of deionized water, stir evenly at 50°C, and after it is completely dissolved, place it in a negative pressure oven at 50°C and press at -0.08 MPa for 1 hour to remove internal bubbles, add 0.02 g of Tween 80 and 2.3 g of plant extract, place it in a high-speed shearing machine, shear at 5000 r / min for 15 minutes, add 2 mL of 10 mM calcium chloride solution, stir and react for 10 minutes to form nanocapsules, and dry it at 50°C for 1 hour to dehydrate and obtain nano-microcapsules.
[0060] A2. Add 0.2g of nano-microcapsules to 80mL of deionized water, stir evenly, add 1.5g of carbon fiber, 0.5g of KH550 and 20mL of ethanol, stir and react at 40°C for 5min, filter, wash with deionized water 3 times, and dry in an oven at 85°C for 10min to obtain modified carbon fiber.
[0061] A3. 1.5 g of modified carbon fiber and 30 mL of liquid phenolic resin were mixed, stirred at 25 ° C for 40 min, and dried in an oven at 100 ° C for 10 min to remove moisture from the modified carbon fiber to obtain a composite adhesive.
[0062] Comparative Example 1
[0063] The difference between this comparative example and Example 1 is that no carbon fiber is added, and the remaining steps and raw materials are the same as Example 1.
[0064] A1. Add 0.5 g of sodium alginate to 25 mL of deionized water, stir evenly at 50°C, and after it is completely dissolved, place it in a negative pressure oven at 50°C and press at -0.08 MPa for 1 hour to remove internal bubbles, add 0.02 g of Tween 80 and 2.3 g of plant extract, place it in a high-speed shearing machine, shear at 5000 r / min for 15 minutes, add 2 mL of 10 mM calcium chloride solution, stir and react for 10 minutes to form nanocapsules, and dry it at 50°C for 1 hour to dehydrate and obtain nano-microcapsules.
[0065] A2. 1.5 g of nanocapsules and 30 mL of liquid phenolic resin were mixed, stirred at 25 ° C for 40 min, and dried in an oven at 100 ° C for 10 min to remove moisture from the modified carbon fiber to obtain a composite adhesive.
[0066] Comparative Example 2
[0067] The difference between this comparative example and Example 1 is that no nano-microcapsules are added, and the remaining steps and raw materials are the same as those of Example 1.
[0068] 1.5 g of carbon fiber and 30 mL of liquid phenolic resin were mixed, stirred at 25° C. for 40 min, and dried in an oven at 100° C. for 10 min to remove moisture from the modified carbon fiber to obtain a composite adhesive.
[0069] Example 2
[0070] The composite resin impregnating agent is specifically prepared by the following steps:
[0071] B1. Mix dodecylphenol polyoxyethylene ether, n-pentanol, cyclohexane and deionized water, stir evenly to obtain a mixed emulsion, add 2.1g bismuth nitrate and 1.8g copper nitrate to 100mL of the mixed emulsion, stir evenly at 25°C to obtain phase A, mix 1.2g hydrazine hydrate with 10mL of the mixed emulsion, stir evenly at 25°C to obtain phase B, mix phase A with phase B to obtain a bismuth-copper composite emulsion.
[0072] B2. Mix 10 mL of bismuth-copper composite emulsion and 0.2 g of graphene oxide, stir evenly, let stand for 10 minutes, stir and react at 30°C for 1 hour, filter, wash with deionized water 3 times, and dry in an oven at 70°C for 10 minutes to obtain nano-bismuth-copper loaded graphene oxide.
[0073] B3. Mix 0.8 g of nano-bismuth copper-loaded graphene oxide and 25 mL of unsaturated aldehyde ester, stir at 25°C for 40 min, evacuate and pressurize to 8.8 MPa, maintain for 5 h and then take out to obtain a composite resin impregnating agent.
[0074] Comparative Example 3
[0075] The difference between this comparative example and Example 2 is that the nano-bismuth copper-loaded graphene oxide is replaced by graphene oxide, and the remaining steps are synchronized with Example 2.
[0076] 0.8 g of graphene oxide and 25 mL of unsaturated aldehyde ester were mixed, stirred at 25° C. for 40 min, vacuumed and pressurized to 8.8 MPa, maintained for 5 h, and then taken out to obtain a composite resin impregnating agent.
[0077] Comparative Example 4
[0078] The difference between this comparative example and Example 2 is that graphene oxide is not added, and the remaining steps are synchronized with Example 2.
[0079] B1. Mix dodecylphenol polyoxyethylene ether, n-pentanol, cyclohexane and deionized water, stir evenly to obtain a mixed emulsion, add 2.1g bismuth nitrate and 1.8g copper nitrate to 100mL of the mixed emulsion, stir evenly at 25°C to obtain phase A, mix 1.2g hydrazine hydrate with 10mL of the mixed emulsion, stir evenly at 25°C to obtain phase B, mix phase A with phase B, stir and react at 30°C for 1h, filter, wash with deionized water 3 times, and dry in an oven at 70°C for 10min to obtain nano bismuth copper.
[0080] B3. Mix 0.8 g of nano-bismuth copper and 25 mL of unsaturated aldehyde ester, stir at 25°C for 40 min, evacuate and pressurize to 8.8 MPa, maintain for 5 h and then take out to obtain a composite resin impregnating agent.
[0081] Example 3
[0082] A PTS process for graphite bearings for automobile water pumps comprises the following steps:
[0083] S1. Graphite powder, carbon powder and composite binder are mixed, kneaded at 80°C for 2h, and then crushed to obtain a mixture, wherein the mass ratio of graphite powder, carbon powder and composite binder is 70:10:6, and the particle size of graphite powder and carbon powder is 15μm.
[0084] S2. Place the mixed material in a granulator for granulation and molding to obtain composite particles.
[0085] S3. Sintering and carbonizing the composite particles to obtain an initial graphite bearing, the sintering and carbonizing temperature is 2050° C., and the sintering and carbonizing time is 6 hours.
[0086] S4. 8 g of the initial graphite bearing was immersed in 80 mL of the composite resin impregnating agent, taken out, cured at 150° C. for 25 min, and processed to obtain a graphite bearing for an automobile water pump.
[0087] Example 4
[0088] A PTS process for graphite bearings for automobile water pumps comprises the following steps:
[0089] S1. Graphite powder, carbon powder and composite binder are mixed, kneaded at 80° C. for 2 h, and then crushed to obtain a mixture, wherein the mass ratio of graphite powder, carbon powder and composite binder is 75:15:7, and the particle size of graphite powder and carbon powder is 15 μm.
[0090] S2. Place the mixed material in a granulator for granulation and molding to obtain composite particles.
[0091] S3. Sintering and carbonizing the composite particles to obtain an initial graphite bearing, the sintering and carbonizing temperature is 2050° C., and the sintering and carbonizing time is 6 hours.
[0092] S4. 10 g of the initial graphite bearing was immersed in 100 mL of the composite resin impregnating agent, taken out, cured at 150° C. for 25 min, and processed to obtain a graphite bearing for an automobile water pump.
[0093] Example 5
[0094] A PTS process for graphite bearings for automobile water pumps comprises the following steps:
[0095] S1. Graphite powder, carbon powder and composite binder are mixed, kneaded at 80° C. for 2 h, and then crushed to obtain a mixture, wherein the mass ratio of graphite powder, carbon powder and composite binder is 80:20:8, and the particle size of graphite powder and carbon powder is 15 μm.
[0096] S2. Place the mixed material in a granulator for granulation and molding to obtain composite particles.
[0097] S3. Sintering and carbonizing the composite particles to obtain an initial graphite bearing, the sintering and carbonizing temperature is 2050° C., and the sintering and carbonizing time is 6 hours.
[0098] S4. 12 g of the initial graphite bearing was immersed in 120 mL of the composite resin impregnating agent, taken out, cured at 150° C. for 25 min, and processed to obtain a graphite bearing for an automobile water pump.
[0099] Comparative Example 5
[0100] The difference between this comparative example and Example 4 is that the composite adhesive is replaced by the material prepared in Comparative Example 1, and the remaining steps are synchronized with Example 4.
[0101] Comparative Example 6
[0102] The difference between this comparative example and Example 4 is that the composite adhesive is replaced by the material prepared in Comparative Example 2, and the remaining steps are synchronized with Example 4.
[0103] Comparative Example 7
[0104] The difference between this comparative example and Example 4 is that the composite resin impregnating agent is replaced by the material prepared in Comparative Example 3, and the remaining steps are synchronized with Example 4.
[0105] Comparative Example 8
[0106] The difference between this comparative example and Example 4 is that the composite resin impregnating agent is replaced by that of Comparative Example 4, and the remaining steps are synchronized with Example 4.
[0107] The performance of the graphite bearings for automobile water pumps prepared in Examples 3-5 and Comparative Examples 5-8 is now tested;
[0108] Shore hardness: It is used to characterize the hardness of the sample, using a Shore hardness tester, referring to ASTM D1039-1999 standard test method - conventional test method for hard materials to Shore hardness gauge.
[0109] Compressive strength: The compressive strength performance of the graphite bearing for automobile water pump prepared above was tested according to GB / T13465.3-2002 "Test method for compressive strength of impermeable graphite materials", and the test was specifically conducted using a pressure testing machine.
[0110] Flexural strength: The flexural strength performance of the graphite bearing for automobile water pump prepared above was tested according to BJ / T8133.8-1999 standard to characterize the ultimate fracture stress per unit area of the sample when subjected to bending moment. The test was carried out on a general universal material testing machine.
[0111] Friction and wear performance test of bearings: The friction coefficient was tested using MPX-2000 friction and wear testing machine.
[0112] Heat resistance: GB3215-824.4.1 standard was used to test the heat resistance of graphite solid rolling bearings. The test results are shown in Table 1 below.
[0113] Table 1: Test results
[0114] project Shore hardness / HS Compressive strength / MPa Flexural strength / MPa Friction coefficient / μ Open porosity / % Example 3 93.5 216.5 78.9 0.12 0.356 Example 4 94.2 217.3 79.5 0.10 0.269 Example 5 94.1 216.8 79.1 0.13 0.328 Comparative Example 5 80.2 202.4 70.6 0.14 0.481 Comparative Example 6 75.9 185.6 66.4 0.15 0.625 Comparative Example 7 90.9 210.3 72.5 0.35 0.385 Comparative Example 8 92.7 213.5 73.7 0.37 0.359
[0115] It can be seen from the test results in Table 1 that in Comparative Example 5, the composite adhesive prepared without adding carbon fiber is used to adhere graphite powder and carbon powder to prepare graphite bearings, and its mechanical properties and density decrease. This may be because carbon fiber, as a reinforcing filler, has good fluidity during the sintering process and can be filled into the pores of graphite powder and carbon powder to improve the density of the graphite bearing. The carbon fiber is combined with the graphite powder and carbon powder through the solidified silicon carbide layer of the plant extract, so that the carbon fiber and the carbon powder raw material are closely combined, thereby improving the mechanical properties of the bearing; Comparative Example 6 does not add the composite adhesive prepared with nano-microcapsules, and is used to adhere graphite powder and carbon powder. The mechanical properties of graphite bearings prepared by adding graphite powder and carbon powder decreased. This may be because when the friction of graphite powder and carbon powder increases, the nano-microcapsules break and release plant extracts, which fill the gaps between the carbon powder particles of the bearing raw material, improving the lubrication effect, making the carbon powder particles have better fluidity, avoiding the accumulation of graphite powder and carbon powder, resulting in poor mechanical strength of the prepared graphite bearings, and during the high-temperature sintering process, the silicon element in the released plant extracts can react with the carbon element on the surface of graphite powder and carbon powder to form a silicon carbide layer covering the surface of the carbon powder, thereby enhancing the mechanical properties of the graphite bearings.
[0116] In Comparative Example 7, the composite resin impregnating agent prepared by graphene oxide loaded with nano-bismuth copper is replaced, and the graphite bearing is impregnated with the composite resin impregnating agent, and the friction performance thereof is decreased. This may be because the nano-bismuth copper powder moves relative to each other between the friction pairs of the graphite bearing, forming rolling friction, reducing the friction coefficient, reducing wear, and also playing the role of micro-bearing and support; in Comparative Example 8, the composite resin impregnating agent prepared by graphene oxide is not added, and the graphite bearing is impregnated with the composite resin impregnating agent, and the friction performance thereof is decreased. This may be because the nano-bismuth copper graphene oxide loaded with nano-bismuth copper is attached to the surface of the graphite bearing through nano-bismuth copper to form a sandwich structure. Nano-bismuth copper serves as a lubricating component, which can make the layers of the sandwich structure move back and forth, and the resulting micro-ball effect has a better lubrication effect.
[0117] The data in Table 1 show that the graphite bearings for automobile water pumps prepared in Examples 3-5 meet the test performance requirements, while the graphite bearings for automobile water pumps prepared in Comparative Examples 5-8 do not meet the performance requirements, indicating that the graphite bearings for automobile water pumps prepared in the present invention have good mechanical properties and wear resistance.
[0118] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0119] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A PTS process for graphite bearings for automobile water pumps, characterized in that: The following steps are involved: S1. The graphite powder, carbon powder, and composite binder are mixed, kneaded, and crushed to obtain a mixture; The composite adhesive is prepared by depositing nano-microcapsules on the surface of carbon fibers and then mixing with phenolic resin; The nano-microcapsules are made of plant extracts as core materials and sodium alginate as wall materials; The plant extract is specifically prepared by the following steps: washing the East Asian hard feather moss with water, drying it, and grinding it in a grinder to powder, adding the East Asian hard feather moss powder to deionized water, stirring it at 80° C. for 6 hours, filtering it, collecting the solution, adding petroleum ether to the solution for degreasing, shaking, standing it, separating and removing the upper petroleum ether solution, and heating it at 80° C. to evaporate it to a viscous state to obtain the plant extract; The amount ratio of the East Asian sclerocaria powder and deionized water is (1-2) g: (40-50) mL; The nano-microcapsules are specifically prepared by the following steps: Sodium alginate was added to deionized water, stirred evenly at 50°C, and after it was completely dissolved, placed in a negative pressure oven at 50°C, and negatively pressurized at -0.08MPa for 1h to remove internal bubbles, Tween 80 and plant extract were added, placed in a high-speed shearing machine, sheared at 5000r / min for 15min, 2mL of 10mM calcium chloride solution was added, stirred and reacted for 10min to form nanocapsules, and dried at 50°C for 1h to dehydrate, thereby obtaining nano-microcapsules; The dosage ratio of the sodium alginate, deionized water, Tween 80 and plant extract is (0.3-0.7) g: (20-30) mL: (0.01-0.03) g: (2-2.6) g; S2. placing the mixture in a granulator for granulation and molding to obtain composite particles; S3. The composite particles are sintered and carbonized to obtain an initial graphite bearing; S4. The initial graphite bearing is impregnated into a composite resin impregnating agent, removed, cured, and processed to obtain a graphite bearing for an automotive water pump; The composite impregnating agent is prepared by mixing nano-bismuth copper-loaded graphene oxide with unsaturated aldehyde ester; The nano-bismuth-copper-loaded graphene oxide is prepared by a mixed reaction of a bismuth-copper composite emulsion and graphene oxide.
2. The PTS process for graphite bearings for automobile water pumps according to claim 1 is characterized in that: The particle size of the graphite powder and carbon powder is 10-20 μm; the kneading temperature is 70-90° C., and the kneading time is 1-3 hours.
3. The PTS process for graphite bearings for automobile water pumps according to claim 1 is characterized in that: The carbon fiber has a diameter of 50-100 nm and a length of 5-10 μm.
4. The PTS process for graphite bearings for automobile water pumps according to claim 1 is characterized in that: The graphene oxide has a particle size of 0.1-1 μm and an interlayer distance of 10-20 nm; the unsaturated aldehyde ester is selected from a polymer of p-phenylphenol, p-tert-butylphenol and formaldehyde, and has a CAS number of 52469-00-8.
5. The PTS process for graphite bearings for automobile water pumps according to claim 1 is characterized in that: The bismuth-copper composite emulsion is specifically prepared by the following steps: Dodecylphenol polyoxyethylene ether, n-pentanol, cyclohexane and deionized water are mixed and stirred to obtain a mixed emulsion, bismuth nitrate and copper nitrate are added to the mixed emulsion, and stirred to obtain phase A at 25°C, hydrazine hydrate is mixed with the mixed emulsion, and stirred to obtain phase B at 25°C, and phase A is mixed with phase B to obtain a bismuth-copper composite emulsion.
6. The PTS process for graphite bearings for automobile water pumps according to claim 5 is characterized in that: The volume ratio of the dodecylphenol polyoxyethylene ether, n-pentanol, cyclohexane and deionized water is (1-3):(0.5-1.5):(5-7):(25-35).
7. The PTS process for graphite bearings for automobile water pumps according to claim 1 is characterized in that: The sintering and carbonization temperature is 2000-2100° C., and the sintering and carbonization time is 4-8 hours.
8. The PTS process for graphite bearings for automobile water pumps according to claim 1 is characterized in that: The graphite bearing for automobile water pump has a diameter of 40-50 mm and a thickness of 10-30 mm.