Thermal insulation polyurethane plastic and preparation method thereof

By using a combination of materials such as polyether polyol and modified composite fillers, polyurethane plastics with low thermal conductivity and high wear resistance are prepared, which solves the problems of high thermal conductivity and heat convection of existing thermal insulation plastics and achieves thermal insulation Performance improvements and energy savings.

CN118791694APending Publication Date: 2024-10-18ZHONGGUANG HUAXIN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411081965.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing thermal insulation plastics have high thermal conductivity, and when thin, there is a problem of heat convection, resulting in a decrease in thermal insulation effect and limiting its application.

Method used

Using a combination of polyether polyol, 2-fluorophenyl isocyanate, modified composite fillers, foam stabilizers, catalysts, foaming agents, water and antioxidants, the modified composite fillers are hollow glass microspheres, fluorosilicic acid A mixture of magnesium, ruthenium dioxide and hydromagnesite is used to prepare thermal insulation polyurethane plastic with low thermal conductivity, high wear resistance and strong tensile strength.

Benefits of technology

A polyurethane plastic with small thermal conductivity, excellent thermal insulation performance, high wear resistance and high tensile strength is realized, which is suitable for thermal insulation applications of building exterior walls and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004983988290000141
    Figure BDA0004983988290000141
  • Figure BDA0004983988290000151
    Figure BDA0004983988290000151
  • Figure BDA0004983988290000152
    Figure BDA0004983988290000152
Patent Text Reader

Abstract

The invention relates to a heat-preservation and heat-insulation polyurethane plastic and a preparation method thereof. The heat-preservation and heat-insulation polyurethane plastic contains polyether polyol, 2-fluorophenyl isocyanate, polyethylene glycol, a modified composite filler, a foam stabilizer, a catalyst, a foaming agent, water and an antioxidant. The modified composite filler is a mixture of hollow glass beads, magnesium fluosilicate, ruthenium dioxide and hydromagnesite. The modified composite filler is used for modification, the modified composite filler is introduced into the polyurethane system, and the prepared heat-preservation and heat-insulation polyurethane plastic has higher levels in heat-preservation and heat-insulation effect, wear resistance and tensile strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermal insulation, and in particular to a thermal insulation polyurethane plastic and a preparation method thereof. Background Art

[0002] Thermal insulation materials refer to materials that can block the transfer of heat energy, and can be divided into traditional thermal insulation materials and new thermal insulation materials. Traditional thermal insulation materials mainly include asbestos, silicate, glass fiber, rock wool, etc.; new thermal insulation materials mainly include vacuum panels, aerogels, foam plastics, etc. Compared with traditional thermal insulation materials, foam plastics have the advantages of light weight and easy construction. They are used on the exterior walls of buildings to block the hot summer air or cold winter air outside the building from entering the room, reducing the frequency of people using refrigeration or heating electrical equipment, thereby reducing energy consumption.

[0003] At present, the most commonly used thermal insulation foam plastics are polyurethane foam plastics, polyvinyl chloride foam plastics or polystyrene foam plastics. Existing thermal insulation plastics rely solely on the foamed pore structure to achieve thermal insulation. The thermal conductivity of current thermal insulation plastics is relatively high. When the thermal insulation plastics are thin, heat convection may still exist on both sides, resulting in reduced thermal insulation effects and other problems, which limits the application of thermal insulation.

[0004] Therefore, in view of the shortcomings of the prior art, it is necessary to provide a thermal insulation polyurethane plastic and a preparation method thereof to solve the shortcomings of the prior art. Summary of the invention

[0005] The purpose of the present invention is to avoid the shortcomings of the prior art and provide a heat-insulating polyurethane plastic having a small thermal conductivity and thus excellent heat-insulating performance, as well as high wear resistance and strong tensile strength.

[0006] The above-mentioned purpose of the present invention is achieved by the following technical measures:

[0007] Provided is a heat-insulating polyurethane plastic, which contains polyether polyol, 2-fluorophenyl isocyanate, polyethylene glycol, modified composite filler, foam stabilizer, catalyst, foaming agent, water and antioxidant.

[0008] The modified composite filler is a mixture of hollow glass microspheres, magnesium fluorosilicate, ruthenium dioxide and hydromagnesite.

[0009] In parts by weight,

[0010] Polyether polyol: 40 parts;

[0011] 2-Fluorophenyl isocyanate: 20 to 30 parts;

[0012] Polyethylene glycol: 5 to 10 parts;

[0013] Modified composite filler: 15 to 20 parts;

[0014] Foam stabilizer: 10 to 20 parts;

[0015] Catalyst: 1 to 3 parts;

[0016] Foaming agent: 10 to 15 parts;

[0017] Water: 1 to 3 parts;

[0018] Antioxidant: 0.1 to 0.3 parts;

[0019] In the modified composite filler, in parts by weight,

[0020] Hollow glass microspheres: 100 parts;

[0021] Ruthenium dioxide: 10 to 20 parts;

[0022] Magnesium fluorosilicate: 4 to 8 parts;

[0023] Hydromagnesite: 5 to 10 parts.

[0024] Further, in parts by weight,

[0025] Polyether polyol: 40 parts;

[0026] 2-Fluorophenyl isocyanate: 26 parts;

[0027] Polyethylene glycol: 7 parts;

[0028] Modified composite filler: 17.7 parts;

[0029] Foam stabilizer: 15 parts;

[0030] Catalyst: 2.3 parts;

[0031] Foaming agent: 12 parts;

[0032] Water: 2.5 parts;

[0033] Antioxidant: 0.22 parts;

[0034] In the modified composite filler, in parts by weight,

[0035] Hollow glass microspheres: 100 parts;

[0036] Ruthenium dioxide: 16 parts;

[0037] Magnesium fluorosilicate: 6 parts;

[0038] Hydromagnesite: 7 parts.

[0039] Preferably, the modified composite filler is prepared by mixing 800-1000 mesh hydromagnesite, ruthenium dioxide, magnesium fluorosilicate and 500-1000 mesh hollow glass microspheres to obtain the modified composite filler.

[0040] Preferably, the catalyst is any one of dibutyltin dilaurate, stannous octoate, and triethylenediamine.

[0041] Preferably, the foam stabilizer is foam stabilizer AK8801 or silicone oil.

[0042] Preferably, the foaming agent is azodicarbonamide or cyclopentane.

[0043] Preferably, the antioxidant is polysorbate 80.

[0044] Another object of the present invention is to avoid the shortcomings of the prior art and provide a method for preparing a thermal insulation polyurethane plastic. The method for preparing the thermal insulation polyurethane plastic is simple, and the prepared thermal insulation polyurethane plastic has a small thermal conductivity and thus excellent thermal insulation performance, and also has high wear resistance and strong tensile strength.

[0045] A method for preparing the above-mentioned thermal insulation polyurethane plastic is provided, comprising the following steps:

[0046] S1, mixing polyether polyol, polyethylene glycol, foam stabilizer, modified composite filler, catalyst, water and antioxidant, and entering S2;

[0047] S2, add 2-fluorophenyl isocyanate, stir and mix to obtain an intermediate, and proceed to S3;

[0048] S3, adding a blowing agent to the intermediate to foam it to obtain a polyurethane foam semi-finished product;

[0049] S4, ripening the polyurethane foam semi-finished product to obtain the thermal insulation polyurethane plastic.

[0050] The preparation method of the present invention comprises the following steps:

[0051] S1, stirring polyether polyol, polyethylene glycol, foam stabilizer, modified composite filler, catalyst, water and antioxidant at a stirring speed of 100r / min to 120r / min for 15min to 30min, and then entering S2;

[0052] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1000 r / min to 1200 r / min, stir for 15 min to 30 min to obtain an intermediate, and enter S3;

[0053] S3, adding a foaming agent to the intermediate, stirring for 7s to 10s, and then foaming to obtain a polyurethane foam semi-finished product;

[0054] S4, curing the polyurethane foam semi-finished product at a curing temperature of 105° C. to 115° C. for a curing time of 18 h to 36 h to obtain the thermal insulation polyurethane plastic.

[0055] The present invention discloses a thermal insulation polyurethane plastic and a preparation method thereof, wherein the thermal insulation polyurethane plastic contains polyether polyol, 2-fluorophenyl isocyanate, polyethylene glycol, modified composite filler, foam stabilizer, catalyst, foaming agent, water and antioxidant; the modified composite filler is a mixture of hollow glass microspheres, magnesium fluorosilicate, ruthenium dioxide and hydromagnesite. The present invention uses the modified composite filler for modification, introduces the modified composite filler into the polyurethane system of the present invention, and the prepared thermal insulation polyurethane plastic has a higher level in terms of thermal insulation effect, wear resistance and tensile strength. DETAILED DESCRIPTION

[0056] The technical solution of the present invention is further described in conjunction with the following examples. Unless otherwise specified, the raw materials used in the following examples are all commercially available products.

[0057] Example 1

[0058] A heat-insulating polyurethane plastic contains polyether polyol, 2-fluorophenyl isocyanate, polyethylene glycol, modified composite filler, foam stabilizer, catalyst, foaming agent, water and antioxidant; the modified composite filler is a mixture of hollow glass microspheres, magnesium fluorosilicate, ruthenium dioxide and hydromagnesite.

[0059] In parts by weight,

[0060] Polyether polyol: 40 parts;

[0061] 2-Fluorophenyl isocyanate: 30 parts;

[0062] Polyethylene glycol: 10 parts;

[0063] Modified composite filler: 20 parts;

[0064] Foam stabilizer: 20 parts;

[0065] Catalyst: 3 parts;

[0066] Foaming agent: 10 parts;

[0067] Water: 1 part;

[0068] Antioxidant: 0.1 part;

[0069] In the modified composite filler, by weight,

[0070] Hollow glass microspheres: 100 parts;

[0071] Ruthenium dioxide: 20 parts;

[0072] Magnesium fluorosilicate: 8 parts;

[0073] Hydromagnesite: 10 parts.

[0074] The preparation method of the modified composite filler is to mix 800-1000 mesh hydromagnesite, ruthenium dioxide, magnesium fluorosilicate and 500-1000 mesh hollow glass microspheres to obtain the modified composite filler.

[0075] The catalyst is dibutyltin dilaurate, the foam stabilizer is silicone oil, the foaming agent is azodicarbonamide, and the antioxidant is polysorbate-80.

[0076] The preparation method of the heat-insulating polyurethane plastic comprises the following steps:

[0077] S1, stirring polyether polyol, polyethylene glycol, foam stabilizer, modified composite filler, catalyst, water and antioxidant at a stirring speed of 100 r / min for 15 min, and then entering S2;

[0078] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1000 r / min, stir for 15 min, and enter S3;

[0079] S3, adding a foaming agent to the intermediate, stirring for 10 seconds, and then foaming to obtain a polyurethane foam semi-finished product;

[0080] S4. The polyurethane foam semi-finished product is cured at a temperature of 105° C. for 18 hours to obtain a heat-insulating polyurethane plastic.

[0081] Example 2

[0082] A heat-insulating polyurethane plastic contains polyether polyol, 2-fluorophenyl isocyanate, polyethylene glycol, modified composite filler, foam stabilizer, catalyst, foaming agent, water and antioxidant; the modified composite filler is a mixture of hollow glass microspheres, magnesium fluorosilicate, ruthenium dioxide and hydromagnesite.

[0083] In parts by weight,

[0084] Polyether polyol: 40 parts;

[0085] 2-Fluorophenyl isocyanate: 20 parts;

[0086] Polyethylene glycol: 5 parts;

[0087] Modified composite filler: 15 parts;

[0088] Foam stabilizer: 10 parts;

[0089] Catalyst: 1 part;

[0090] Foaming agent: 15 parts;

[0091] Water: 3 parts;

[0092] Antioxidant: 0.3 parts;

[0093] In the modified composite filler, by weight,

[0094] Hollow glass microspheres: 100 parts;

[0095] Ruthenium dioxide: 10 parts;

[0096] Magnesium fluorosilicate: 4 parts;

[0097] Hydromagnesite: 5 parts.

[0098] The preparation method of the modified composite filler is to mix 800-1000 mesh hydromagnesite, ruthenium dioxide, magnesium fluorosilicate and 500-1000 mesh hollow glass microspheres to obtain the modified composite filler.

[0099] The catalyst is stannous octoate, the foam stabilizer is foam stabilizer AK8801, the foaming agent is cyclopentane, and the antioxidant is polysorbate-80.

[0100] The preparation method of the heat-insulating polyurethane plastic comprises the following steps:

[0101] S1, stirring polyether polyol, polyethylene glycol, foam stabilizer, modified composite filler, catalyst, water and antioxidant at a stirring speed of 120r / min for 30min, and then entering S2;

[0102] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1200 r / min, stir for 30 min, and enter S3;

[0103] S3, adding a blowing agent to the intermediate, stirring for 7 seconds, and then foaming to obtain a polyurethane foam semi-finished product;

[0104] S4. The polyurethane foam semi-finished product is cured at a temperature of 115° C. for 36 hours to obtain a heat-insulating polyurethane plastic.

[0105] Example 3

[0106] A heat-insulating polyurethane plastic contains polyether polyol, 2-fluorophenyl isocyanate, polyethylene glycol, modified composite filler, foam stabilizer, catalyst, foaming agent, water and antioxidant; the modified composite filler is a mixture of hollow glass microspheres, magnesium fluorosilicate, ruthenium dioxide and hydromagnesite.

[0107] In parts by weight,

[0108] Polyether polyol: 40 parts;

[0109] 2-Fluorophenyl isocyanate: 26 parts;

[0110] Polyethylene glycol: 7 parts;

[0111] Modified composite filler: 17.7 parts;

[0112] Foam stabilizer: 15 parts;

[0113] Catalyst: 2.3 parts;

[0114] Foaming agent: 12 parts;

[0115] Water: 2.5 parts;

[0116] Antioxidant: 0.22 parts;

[0117] In the modified composite filler, by weight,

[0118] Hollow glass microspheres: 100 parts;

[0119] Ruthenium dioxide: 16 parts;

[0120] Magnesium fluorosilicate: 6 parts;

[0121] Hydromagnesite: 7 parts.

[0122] The preparation method of the modified composite filler is to mix 800-1000 mesh hydromagnesite, ruthenium dioxide, magnesium fluorosilicate and 500-1000 mesh hollow glass microspheres to obtain the modified composite filler.

[0123] The catalyst is triethylenediamine, the foam stabilizer is silicone oil, the foaming agent is cyclopentane, and the antioxidant is polysorbate-80.

[0124] The preparation method of the heat-insulating polyurethane plastic comprises the following steps:

[0125] S1, stirring polyether polyol, polyethylene glycol, foam stabilizer, modified composite filler, catalyst, water and antioxidant at a stirring speed of 110r / min for 20min, and then entering S2;

[0126] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1100 r / min, stir for 20 min, and enter S3;

[0127] S3, adding a foaming agent to the intermediate, stirring for 8 seconds, and then foaming to obtain a polyurethane foam semi-finished product;

[0128] S4. The polyurethane foam semi-finished product is cured at a temperature of 110° C. for 24 hours to obtain a heat-insulating polyurethane plastic.

[0129] Example 4

[0130] A heat-insulating polyurethane plastic contains polyether polyol, 2-fluorophenyl isocyanate, polyethylene glycol, modified composite filler, foam stabilizer, catalyst, foaming agent, water and antioxidant; the modified composite filler is a mixture of hollow glass microspheres, magnesium fluorosilicate, ruthenium dioxide and hydromagnesite.

[0131] In parts by weight,

[0132] Polyether polyol: 40 parts;

[0133] 2-Fluorophenyl isocyanate: 25 parts;

[0134] Polyethylene glycol: 6.5 parts;

[0135] Modified composite filler: 18 parts;

[0136] Foam stabilizer: 18 parts;

[0137] Catalyst: 2 parts;

[0138] Foaming agent: 14 parts;

[0139] Water: 1.5 parts;

[0140] Antioxidant: 0.25 parts;

[0141] In the modified composite filler, by weight,

[0142] Hollow glass microspheres: 100 parts;

[0143] Ruthenium dioxide: 18 parts;

[0144] Magnesium fluorosilicate: 7 parts;

[0145] Hydromagnesite: 6 parts.

[0146] The preparation method of the modified composite filler is to mix 800-1000 mesh hydromagnesite, ruthenium dioxide, magnesium fluorosilicate and 500-1000 mesh hollow glass microspheres to obtain the modified composite filler.

[0147] The catalyst is triethylenediamine, the foam stabilizer is silicone oil, the foaming agent is cyclopentane, and the antioxidant is polysorbate-80.

[0148] The preparation method of the heat-insulating polyurethane plastic comprises the following steps:

[0149] S1, stirring polyether polyol, polyethylene glycol, foam stabilizer, modified composite filler, catalyst, water and antioxidant at a stirring speed of 110r / min for 20min, and then entering S2;

[0150] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1000 r / min, stir for 25 min, and enter S3;

[0151] S3, adding a blowing agent to the intermediate, stirring for 9 seconds, and then foaming to obtain a polyurethane foam semi-finished product;

[0152] S4. The polyurethane foam semi-finished product is cured at a temperature of 112° C. for 24 hours to obtain a heat-insulating polyurethane plastic.

[0153] Comparative Example 1

[0154] A thermal insulation polyurethane plastic, the other features of which are the same as those of Example 3, except that the weight portion of the modified composite filler is 10 parts.

[0155] Comparative Example 2

[0156] A thermal insulation polyurethane plastic, the other features of which are the same as those of Example 3, except that the weight portion of the modified composite filler is 25 parts.

[0157] Comparative Example 3

[0158] A heat-insulating polyurethane plastic, the other features of which are the same as those of Example 3, except that the composition of the modified composite filler is different. In the modified composite filler, in parts by weight,

[0159] Hollow glass microspheres: 100 parts;

[0160] Ruthenium dioxide: 5 parts;

[0161] Magnesium fluorosilicate: 10 parts;

[0162] Hydromagnesite: 20 parts.

[0163] Comparative Example 4

[0164] A thermal insulation polyurethane plastic, the other features of which are the same as those of Example 3, except that no modified composite filler is added and the weight portion of 2-fluorophenyl isocyanate is 43.7 parts.

[0165] The preparation method of the heat-insulating polyurethane plastic comprises the following steps:

[0166] S1, stirring polyether polyol, polyethylene glycol, foam stabilizer, catalyst, water and antioxidant at a stirring speed of 110r / min for 20min, and then entering S2;

[0167] S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1100 r / min, stir for 20 min, and enter S3;

[0168] S3, adding a foaming agent to the intermediate, stirring for 8 seconds, and then foaming to obtain a polyurethane foam semi-finished product;

[0169] S4. The polyurethane foam semi-finished product is cured at a temperature of 110° C. for 24 hours to obtain a heat-insulating polyurethane plastic.

[0170] Comparative Example 5

[0171] A heat-insulating polyurethane plastic, the other features of which are the same as those of Example 3, except that the composition of the modified composite filler is different. In the modified composite filler, in parts by weight,

[0172] Hollow glass microspheres: 100 parts;

[0173] Ruthenium dioxide: 22 parts;

[0174] Hydromagnesite: 7 parts.

[0175] Comparative Example 6

[0176] A heat-insulating polyurethane plastic, the other features of which are the same as those of Example 3, except that the composition of the modified composite filler is different. In the modified composite filler, in parts by weight,

[0177] Hollow glass microspheres: 100 parts;

[0178] Ruthenium dioxide: 23 parts;

[0179] Magnesium fluorosilicate: 6 parts.

[0180] Comparative Example 7

[0181] A heat-insulating polyurethane plastic, the other features of which are the same as those of Example 3, except that the composition of the modified composite filler is different. In the modified composite filler, in parts by weight,

[0182] Ruthenium dioxide: 16 parts;

[0183] Magnesium fluorosilicate: 6 parts;

[0184] Hydromagnesite: 7 parts.

[0185] Comparative Example 8

[0186] A thermal insulation polyurethane plastic, the other features of which are the same as those of Example 3, except that 2-fluorophenyl isocyanate is replaced by isocyanate.

[0187] Effect example

[0188] The thermal insulation polyurethane plastics obtained in Examples 1 to 4 and Comparative Examples 1 to 8 of the present invention were subjected to performance tests, wherein the thermal conductivity was tested according to the standard GB / T10295-2008, the wear resistance was tested according to the DIN 53516 standard, the tensile strength at room temperature and the tensile strength at -170°C were tested according to 1SO1926, the average pore diameter was tested according to GB / T 8810-2005, and the closed cell rate was tested according to ASTMD2856-94. The test results are shown in Tables 1 and 2:

[0189] Table 1. Test results of thermal insulation polyurethane plastic performance of Examples 1-4

[0190]

[0191]

[0192] Table 2. Test results of thermal insulation polyurethane plastics of comparative examples 1-8

[0193]

[0194] It can be seen from the data in Table 1 and Table 2 that, compared with the thermal insulation polyurethane plastic of the comparative example, the thermal conductivity of the thermal insulation polyurethane plastic of Examples 1 to 4 of the present invention is significantly lower than that of Comparative Examples 1 to 8, and is within the range of 0.017W / m·K to 0.019W / m·K, and its closed cell rate is not less than 95.9%, so the thermal insulation performance of the present invention is excellent. The wear resistance of the thermal insulation polyurethane plastic of the present invention is not more than 303mm 3 , its material is harder than the comparative example, so its wear resistance is superior. The tensile strength of the present invention is not less than 5.94MPa at room temperature and not less than 5.01MPa at -170°C. It can be seen that even at -170°C, the tensile strength can still maintain a high strength, so its tensile strength is high and the mechanical properties are good. It can be seen from the foaming density and the average diameter of the pores of the present invention that the thermal insulation polyurethane plastic of the present invention has more pore data and a small pore diameter.

[0195] In summary, the thermal insulation polyurethane plastic of the present invention is modified by using a modified composite filler using a mixture of hollow glass microspheres, magnesium fluorosilicate, ruthenium dioxide and hydromagnesite as raw materials, and the modified composite filler is introduced into the polyurethane system of the present invention. The prepared thermal insulation polyurethane plastic has higher levels in terms of thermal insulation effect, wear resistance and tensile strength.

[0196] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A thermal insulation polyurethane plastic, characterized in that: Contains polyether polyol, 2-fluorophenyl isocyanate, polyethylene glycol, modified composite filler, foam stabilizer, catalyst, foaming agent, water and antioxidant; The modified composite filler is a mixture of hollow glass microspheres, magnesium fluorosilicate, ruthenium dioxide and hydromagnesite.

2. The thermal insulation polyurethane plastic according to claim 1, characterized in that: In parts by weight, Polyether polyol: 40 parts; 2-Fluorophenyl isocyanate: 20 to 30 parts; Polyethylene glycol: 5 to 10 parts; Modified composite filler: 15 to 20 parts; Foam stabilizer: 10 to 20 parts; Catalyst: 1 to 3 parts; Foaming agent: 10 to 15 parts; Water: 1 to 3 parts; Antioxidant: 0.1 to 0.3 parts; In the modified composite filler, by weight, Hollow glass microspheres: 100 parts; Ruthenium dioxide: 10 to 20 parts; Magnesium fluorosilicate: 4 to 8 parts; Hydromagnesite: 5 to 10 parts.

3. The thermal insulation polyurethane plastic according to claim 2, characterized in that: In parts by weight, Polyether polyol: 40 parts; 2-Fluorophenyl isocyanate: 26 parts; Polyethylene glycol: 7 parts; Modified composite filler: 17.7 parts; Foam stabilizer: 15 parts; Catalyst: 2.3 parts; Foaming agent: 12 parts; Water: 2.5 parts; Antioxidant: 0.22 parts; In the modified composite filler, by weight, Hollow glass microspheres: 100 parts; Ruthenium dioxide: 16 parts; Magnesium fluorosilicate: 6 parts; Hydromagnesite: 7 parts.

4. The thermal insulation polyurethane plastic according to claim 1, characterized in that: The preparation method of the modified composite filler is to mix 800-1000 mesh hydromagnesite, ruthenium dioxide, magnesium fluorosilicate and 500-1000 mesh hollow glass microspheres to obtain the modified composite filler.

5. The thermal insulation polyurethane plastic according to claim 1, characterized in that: The catalyst is any one of dibutyltin dilaurate, stannous octoate and triethylenediamine.

6. The thermal insulation polyurethane plastic according to claim 1, characterized in that: The foam stabilizer is foam stabilizer AK8801 or silicone oil.

7. The thermal insulation polyurethane plastic according to claim 1, characterized in that: The foaming agent is azodicarbonamide or cyclopentane.

8. The thermal insulation polyurethane plastic according to claim 1, characterized in that: The antioxidant is polysorbate-80.

9. A method for preparing the thermal insulation polyurethane plastic according to any one of claims 1 to 8, characterized in that: The steps include: S1, mixing polyether polyol, polyethylene glycol, foam stabilizer, modified composite filler, catalyst, water and antioxidant, and entering S2; S2, add 2-fluorophenyl isocyanate, stir and mix to obtain an intermediate, and proceed to S3; S3, adding a blowing agent to the intermediate to foam it to obtain a polyurethane foam semi-finished product; S4, ripening the polyurethane foam semi-finished product to obtain the thermal insulation polyurethane plastic.

10. The preparation method according to claim 9, characterized in that: The steps include: S1, stirring polyether polyol, polyethylene glycol, foam stabilizer, modified composite filler, catalyst, water and antioxidant at a stirring speed of 100r / min to 120r / min for 15min to 30min, and then entering S2; S2, add 2-fluorophenyl isocyanate, stir at a stirring speed of 1000 r / min to 1200 r / min, stir for 15 min to 30 min to obtain an intermediate, and enter S3; S3, adding a foaming agent to the intermediate, stirring for 7s to 10s, and then foaming to obtain a polyurethane foam semi-finished product; S4, curing the polyurethane foam semi-finished product at a curing temperature of 105° C. to 115° C. for a curing time of 18 h to 36 h to obtain the thermal insulation polyurethane plastic.