Phenylphosphonic acid organic compound, hole transport material, perovskite solar cell, preparation method of perovskite solar cell, and electric equipment
By using phenylphosphonic acid organic compounds as hole transport layer materials in perovskite solar cells, the problem of charge defects is solved, the open circuit voltage and photoelectric conversion efficiency of perovskite solar cells are improved, and the device stability is enhanced and hole transport properties.
Patent Information
- Application Number
- CN202410862613.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-28
AI Technical Summary
During the preparation process of perovskite solar cells, due to the evaporation of solvents and organic salts, charge defects are easily left at the lower interface and grain boundaries, reducing device performance and stability. The self-assembled monolayer does not have the defect passivation function, limiting the Design of hole transport layer.
Phenylphosphonic acid organic compounds are used as hole transport layer materials, forming chemical bonds with the metal oxide substrate through their phosphonic acid anchoring groups, passivating defects in the metal oxide and perovskite light-absorbing layers, and passing the phenyl Bridging with phosphine groups improves interfacial stability and hole transport properties.
The open circuit voltage and photoelectric conversion efficiency of perovskite solar cells are significantly improved, and the working stability and hole transport performance of the device are enhanced.
Smart Images

Figure CN118852249A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of perovskite solar cells, and specifically relates to a phenylphosphonic acid organic compound, a hole transport material, a perovskite solar cell and a preparation method thereof, and electrical equipment. Background Art
[0002] Perovskite solar cells (PSCs), as a new type of thin-film solar cells, are developing rapidly. PSCs have a wide range of material sources, simple processes, high photoelectric conversion efficiency, and broad development prospects. Currently, most efficient single-section or stacked PSCs use self-assembled monolayer (SAM) materials as hole transport layers, which have the advantages of low material consumption and low parasitic absorption.
[0003] However, during the preparation process of perovskite films, due to the evaporation of solvents and organic salts, a large number of charge defects are easily left at the lower interface and grain boundaries. These defects will become the centers of non-radiative recombination, reducing the device performance and stability of PSCs. However, these self-assembled monolayers do not have the function of defect passivation, which leaves a big obstacle for the rational design of more effective hole transport layers. Summary of the invention
[0004] The present application aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the purpose of the present application is to provide a phenylphosphine phosphonic acid organic compound, a hole transport material, a perovskite solar cell and a preparation method and an electrical device thereof. The open circuit voltage (V OC ) and photoelectric conversion efficiency (PCE) have been significantly improved.
[0005] In one aspect of the present application, the present application proposes a phenylphosphine phosphonic acid organic compound. According to an embodiment of the present application, the phenylphosphine phosphonic acid organic compound includes at least one of a compound as shown in Formula I and a compound as shown in Formula II:
[0006]
[0007]
[0008] Wherein, R1 includes a C1-C8 alkyl chain or at least one aryl chain; R2 includes a C1-C8 alkyl chain or at least one aryl chain, X - These include halide ions, sulfonate ions, benzenesulfonate ions, thiocyanate ions, tetrafluoroborate ions, hexafluorophosphate ions, formate ions, or acetate ions.
[0009] According to the phenylphosphine phosphonic acid organic compounds of the embodiments of the present application, first, the phosphonic acid in the phenylphosphine phosphonic acid organic compounds is an anchoring group, which can effectively anchor the phenylphosphine phosphonic acid organic compounds on the metal oxide substrate, thereby improving the coverage of the molecule on the metal oxide substrate. Second, the phosphoric acid in the phenylphosphine phosphonic acid organic compounds can be chemically bonded with the metal oxide in the metal oxide substrate, forming a layer of effective hole transport interface on the metal oxide substrate, and can passivate the defects on the metal oxide at the same time. Third, the phenylphosphine group in the phenylphosphine phosphonic acid organic compounds can bridge the perovskite light absorption layer and the metal oxide substrate respectively, effectively passivate the defects on the interface under the perovskite light absorption layer, improve the perovskite crystallization quality, enhance the interface stability, and enhance the working stability of the device. Fourth, the phenylphosphine phosphonic acid organic compounds introduce alkyl chains or aromatic groups as intermediate fragments, which can adjust the molecular flexibility, optimize the band structure, enhance the hole transport, and improve the carrier transport performance. Thus, the open circuit voltage (V OC ) and photoelectric conversion efficiency (PCE) have been significantly improved.
[0010] In addition, the phenylphosphonic acid organic compound according to the above embodiment of the present application may also have the following additional technical features:
[0011] In some embodiments of the present application, R1 includes a C1-C6 alkyl chain, an aryl chain or two aryl chains; R2 includes a C1-C4 alkyl chain; X - Including halide ions.
[0012] In some embodiments of the present application, the phenylphosphonic acid organic compound includes at least one of the following compounds:
[0013]
[0014]
[0015] In the second aspect of the present application, the present application proposes a hole transport material. According to the embodiment of the present application, the hole transport material includes the phenylphosphonic acid organic compound described in the above embodiment. Thus, the hole transport material can be effectively anchored on the metal oxide substrate to improve the coverage of the molecule on the metal oxide substrate; can effectively form a hole transport interface on the metal oxide substrate, and can effectively passivate the defects on the metal oxide; can effectively passivate the defects on the interface under the perovskite light absorption layer, and improve the perovskite crystal quality; can effectively adjust the molecular flexibility, optimize the band structure, enhance hole transport, and improve the carrier transport performance.
[0016] In the third aspect of the present application, the present application proposes a perovskite solar cell. According to an embodiment of the present application, the perovskite solar cell includes a hole transport layer, and the hole transport layer includes the hole transport material described in the above embodiment. Thus, by introducing a phenylphosphine phosphonic acid organic compound into the hole transport layer of the perovskite solar cell, the open circuit voltage (V OC ) and photoelectric conversion efficiency (PCE).
[0017] In addition, the perovskite solar cell according to the above embodiment of the present application may also have the following additional technical features:
[0018] In some embodiments of the present application, the thickness of the hole transport layer is 1 nm-10 nm; and / or, the hole transport layer is a SAM layer.
[0019] In some embodiments of the present application, the perovskite solar cell further includes a metal oxide substrate, a perovskite light absorbing layer, an electron transport layer and an electrode layer, and the metal oxide substrate, the hole transport layer, the perovskite light absorbing layer, the electron transport layer and the electrode layer are stacked in sequence.
[0020] In some embodiments of the present application, the thickness of the perovskite light absorbing layer is 100 nm-3 μm; and / or the thickness of the electron transport layer is 1 nm-100 nm.
[0021] In some embodiments of the present application, the perovskite light-absorbing layer includes an ABX3 type perovskite material, wherein the A ions include at least one of cesium ions, rubidium ions, potassium ions, methylamine ions, formamidine ions, methylenediamine ions, benzamidine cations, and guanidinium cations, the B ions include at least one of divalent lead ions and divalent tin ions, and the X ions include at least one of fluoride ions, chloride ions, bromide ions, iodide ions, thiocyanate ions, tetrafluoroborate ions, hexafluorophosphate ions, formate ions, and acetate ions; and / or the electron transport layer includes tin dioxide, At least one of titanium dioxide, [6,6]-phenyl-C71-butyric acid isomethyl ester, C60 and C60 derivatives; and / or, the electrode layer comprises at least one of ITO, IZO, IWO, FTO, ICO, AZO, BZO, gold, silver, copper, aluminum, and carbon; and / or, the metal oxide substrate comprises a transparent conductive oxide layer, and the transparent conductive oxide layer comprises at least one of ITO, IZO, IWO, FTO, ICO, AZO, and BZO; optionally, the metal oxide substrate further comprises TiO2, NiO x , Al2O3 or SiO2.
[0022] In a fourth aspect of the present application, the present application proposes a method for preparing a perovskite solar cell. According to an embodiment of the present application, the method comprises:
[0023] Mixing the hole transport material of the above embodiment with a solvent to form a mixed solution;
[0024] The mixed solution is spin-coated on the surface of the metal oxide substrate, and heated and annealed, thereby forming a hole transport layer on the surface of the metal oxide substrate.
[0025] According to the method for preparing a perovskite solar cell according to the embodiment of the present application, by introducing a phenylphosphine phosphonic acid organic compound into the hole transport layer of the perovskite solar cell, the open circuit voltage (V OC ) and photoelectric conversion efficiency (PCE).
[0026] In addition, the method for preparing a perovskite solar cell according to the above embodiment of the present application may also have the following additional technical features:
[0027] In some embodiments of the present application, the concentration of the hole transport material in the mixed solution is 0.1 mg / mL-4.0 mg / mL.
[0028] In the fifth aspect of the present application, the present application proposes an electrical device. According to an embodiment of the present application, the electrical device has the perovskite solar cell as described above. Therefore, the electrical device has all the advantages of the perovskite solar cell, which will not be repeated here.
[0029] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0031] Figure 1 Schematic diagram of the structure of a perovskite solar cell according to an embodiment of the present application.
[0032] Reference numerals:
[0033] 100-metal oxide substrate, 200-hole transport layer, 300-perovskite light absorption layer, 400-electron transport layer, 500-electrode layer. DETAILED DESCRIPTION
[0034] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limiting the present application.
[0035] This application is proposed by the inventor based on the following issues:
[0036] In the related art, efficient single-section or stacked PSCs mostly use self-assembled monolayer (SAM) materials as hole transport layers, which have the advantages of low material consumption and small parasitic absorption. However, during the preparation process of the perovskite film, due to the evaporation of solvents and organic salts, a large number of charge defects are easily left at the lower interface and grain boundaries. These defects will become the centers of non-radiative recombination, reducing the device performance and stability of PSCs. However, these self-assembled monolayers do not have the function of defect passivation, which leaves a big obstacle for the rational design of more effective hole transport layers.
[0037] In view of this, in one aspect of the present application, the present application proposes a phenylphosphine phosphonic acid organic compound. According to an embodiment of the present application, the phenylphosphine phosphonic acid organic compound includes at least one of a compound as shown in Formula I and a compound as shown in Formula II:
[0038]
[0039] Wherein, R1 includes a C1-C8 alkyl chain or at least one aryl chain; R2 includes a C1-C8 alkyl chain or at least one aryl chain, X - These include halide ions, sulfonate ions, benzenesulfonate ions, thiocyanate ions, tetrafluoroborate ions, hexafluorophosphate ions, formate ions, or acetate ions.
[0040] According to the phenylphosphine phosphonic acid organic compounds of the embodiments of the present application, first, the phosphonic acid in the phenylphosphine phosphonic acid organic compounds is an anchoring group, which can effectively anchor the phenylphosphine phosphonic acid organic compounds on the metal oxide substrate, thereby improving the coverage of the molecule on the metal oxide substrate. Second, the phosphonic acid in the phenylphosphine phosphonic acid organic compounds can be chemically bonded with the metal oxide in the metal oxide substrate, forming a layer of effective hole transport interface on the metal oxide substrate, and can passivate the defects on the metal oxide at the same time. Third, the phenylphosphine group in the phenylphosphine phosphonic acid organic compounds can bridge the perovskite light absorption layer and the metal oxide substrate respectively, effectively passivate the defects on the interface under the perovskite light absorption layer, improve the perovskite crystallization quality, enhance the interface stability, and enhance the working stability of the device. Fourth, the phenylphosphine phosphonic acid organic compounds introduce alkyl chains or aromatic groups as intermediate fragments, which can adjust the molecular flexibility, optimize the band structure, enhance the hole transport, and improve the carrier transport performance. Thus, the open circuit voltage (V OC ) and photoelectric conversion efficiency (PCE) have been significantly improved.
[0041] It should be noted that the metal oxide substrate includes a transparent conductive oxide layer, and the transparent conductive oxide layer includes at least one of ITO, IZO, IWO, FTO, ICO, AZO, and BZO.
[0042] According to some specific embodiments of the present application, R1 includes a C1-C6 alkyl chain, one aryl chain or two aryl chains; R2 includes a C1-C4 alkyl chain; X - Including halogen ions. The phenylphosphonic acid organic compound obtained can further effectively anchor on the metal oxide substrate, improve the coverage of the molecule on the metal oxide substrate; can further effectively form a hole transmission interface on the metal oxide substrate, and can further effectively passivate the defects on the metal oxide; can further effectively passivate the defects on the interface under the perovskite light absorption layer, and improve the perovskite crystal quality; can further effectively adjust the molecular flexibility, optimize the band structure, enhance hole transmission, and improve the carrier transmission performance.
[0043] According to some further specific embodiments of the present application, the above-mentioned phenylphosphonic acid organic compound includes at least one of the following compounds:
[0044]
[0045]
[0046] The phenylphosphonic acid organic compounds shown in H1, H2, H3, H4, H5, H6, H7, and H8 above can further effectively anchor on the metal oxide substrate, thereby increasing the coverage of the molecules on the metal oxide substrate; can further effectively form a hole transport interface on the metal oxide substrate, and can further effectively passivate the defects on the metal oxide; can further effectively passivate the defects on the interface under the perovskite light-absorbing layer, thereby improving the crystallization quality of the perovskite; can further effectively adjust the molecular flexibility, optimize the energy band structure, enhance hole transport, and improve the carrier transport performance.
[0047] The preparation method of the above-mentioned phenylphosphine phosphonic acid organic compound is not particularly limited. As a specific embodiment, the preparation method of the phenylphosphine phosphonic acid organic compound shown in formula I is as follows:
[0048] Step 1: reacting the diphenylphosphine represented by formula M1 and the dibromoalkyl or dibromoaryl represented by formula M2 under the conditions of a strong base and a phase transfer catalyst to prepare a compound represented by formula M3;
[0049] Step 2: reacting the compound represented by formula M3 and the phosphate represented by formula M4 under alkaline conditions to prepare the compound represented by formula M5;
[0050] Step 3: hydrolyze the compound represented by formula M5 through a hydrolysis reaction to prepare the compound represented by formula I.
[0051] in,
[0052]
[0053] Formula M2, R1 is selected from a C1-8 alkyl chain or at least one aryl chain;
[0054]
[0055] According to some specific embodiments of the present application, the molar ratio of the diphenylphosphine represented by Formula M1 to the dibromo compound represented by Formula M2 can be 1:(2-10).
[0056] According to some further specific embodiments of the present application, the reaction temperature of step one can be 50 degrees Celsius-90 degrees Celsius.
[0057] According to some other specific embodiments of the present application, in step 2, the molar ratio of the compound represented by formula M3 to the phosphate represented by formula M4 can be 1:(10-40).
[0058] According to some other specific embodiments of the present application, the reaction temperature of step 2 can be 120 degrees Celsius to 160 degrees Celsius.
[0059] The preparation method of the phenylphosphine phosphonic acid organic compound shown in formula II is similar to the preparation method of the phenylphosphine phosphonic acid organic compound shown in formula I, specifically, comprising:
[0060] Step 1: reacting the bromotriphenylphosphine salt represented by formula N1 and the phosphate represented by formula N2 under alkaline conditions to prepare a compound represented by formula N3;
[0061] Step 2: hydrolyze the compound represented by formula N3 through a hydrolysis reaction to prepare a compound represented by formula II.
[0062] in, R2 includes a C1-C8 alkyl chain or at least one aryl chain, X - These include halide ions, sulfonate ions, benzenesulfonate ions, thiocyanate ions, tetrafluoroborate ions, hexafluorophosphate ions, formate ions, or acetate ions.
[0063]
[0064] In the second aspect of the present application, the present application proposes a hole transport material. According to the embodiment of the present application, the hole transport material includes the phenylphosphonic acid organic compound described in the above embodiment. Thus, the hole transport material can be effectively anchored on the metal oxide substrate to improve the coverage of the molecule on the metal oxide substrate; can effectively form a hole transport interface on the metal oxide substrate, and can effectively passivate the defects on the metal oxide; can effectively passivate the defects on the interface under the perovskite light absorption layer, and improve the perovskite crystal quality; can effectively adjust the molecular flexibility, optimize the band structure, enhance hole transport, and improve the carrier transport performance.
[0065] In the third aspect of the present application, the present application provides a perovskite solar cell. According to the embodiments of the present application, referring to the attached Figure 1 The perovskite solar cell includes a hole transport layer 200, and the hole transport layer 200 includes the hole transport material described in the above embodiment. Therefore, by introducing phenylphosphine phosphonic acid organic compounds into the hole transport layer of the perovskite solar cell, the open circuit voltage (V OC ) and photoelectric conversion efficiency (PCE).
[0066] According to some specific embodiments of the present application, the thickness of the above-mentioned hole transport layer can be 1nm-10nm, for example, it can be 1nm, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, etc. By limiting the thickness of the hole transport layer within the above-mentioned range, the ability of the hole transport layer to transport holes can be further enhanced, and at the same time, it can further ensure that it passivates the defects on the lower interface of the perovskite light absorbing layer, thereby improving the crystallization quality of the perovskite.
[0067] According to some further specific embodiments of the present application, the hole transport layer is a SAM layer, ie, a self-assembled monolayer.
[0068] Further, see Attachment Figure 1 The perovskite solar cell further comprises a metal oxide substrate 100, a perovskite light absorbing layer 300, an electron transport layer 400 and an electrode layer 500. The metal oxide substrate 100, the hole transport layer 200, the perovskite light absorbing layer 300, the electron transport layer 400 and the electrode layer 500 are sequentially stacked.
[0069] The working process of perovskite solar cells mainly includes: the generation and separation of excitons, the transmission of free carriers, the collection of carriers and the generation of current. The specific process is as follows: In perovskite solar cells, sunlight is absorbed by the perovskite light-absorbing layer, and the perovskite light-absorbing layer absorbs photons to generate excitons. Since the perovskite light-absorbing layer has a lower Coulomb force binding, the excitons are then separated into free electrons and holes. The separated free carriers are transmitted in the perovskite light-absorbing layer and transmitted out through the transport layer. The electron transport layer plays the role of transmitting electrons and blocking holes, and the hole transport layer plays the role of transmitting holes and blocking electrons. The electrons and holes transmitted through the transport layer are collected by the electrodes to form current and voltage respectively.
[0070] In the embodiments of the present application, the perovskite light-absorbing layer serves as a light-absorbing layer that can convert photons into holes and electrons, and its material can be selected from conventional materials in the art, which are not limited here, and can be selected according to actual needs by those skilled in the art. As some specific examples, the material of the above-mentioned perovskite light-absorbing layer can be an ABX3-type perovskite material, wherein the A ion can be at least one of cesium ions, rubidium ions, potassium ions, methylamine ions, formamidine ions, methylenediamine ions, benzamidine cations, and guanidine cations, the B ion can be at least one of divalent lead ions and divalent tin ions, and the X ion can be at least one of fluoride ions, chloride ions, bromide ions, iodide ions, thiocyanate ions, tetrafluoroborate ions, hexafluorophosphate ions, formate ions, and acetate ions.
[0071] According to some further specific embodiments of the present application, the thickness of the above-mentioned perovskite light absorbing layer can be 100nm-3μm, for example, it can be 100nm, 300nm, 500nm, 800nm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, etc., thereby further ensuring the ability of the perovskite light absorbing layer to convert photons into holes and electrons.
[0072] In the embodiments of the present application, the electron transport layer is a transport layer that can effectively transport electrons, and its material can be selected from conventional materials in the field, which is not limited here, and those skilled in the art can select according to actual needs. As some specific examples, the material of the electron transport layer includes at least one of tin dioxide, titanium dioxide, [6,6]-phenyl-C71-butyric acid isomethyl ester, C60 and C60 derivatives.
[0073] According to some other specific embodiments of the present application, the thickness of the above-mentioned electron transport layer can be 1nm-100nm, for example, it can be 1nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, etc., thereby further ensuring the ability of the electron transport layer to transport electrons.
[0074] In the embodiments of the present application, the material of the electrode layer is not particularly limited. As some specific examples, the electrode layer includes at least one of indium tin oxide, indium zinc oxide, zinc aluminum oxide, silver nanowires, gold, silver, copper, aluminum, and carbon.
[0075] According to some further specific embodiments of the present application, the metal oxide substrate includes a transparent conductive oxide layer and a substrate (such as glass). The material of the transparent conductive oxide layer is not particularly limited. As some specific examples, the transparent conductive oxide layer includes at least one of ITO, IZO, IWO, FTO, ICO, AZO, and BZO. Optionally, the metal oxide substrate also includes TiO2, NiO x , Al2O3 or SiO2.
[0076] In the embodiments of the present application, the perovskite solar cell may be a single-layer cell or a stacked cell. When the stacked cell is a perovskite / crystalline silicon stacked cell, a full perovskite stacked cell, a perovskite / organic stacked cell, or a perovskite / CIGS stacked cell.
[0077] In a fourth aspect of the present application, the present application proposes a method for preparing a perovskite solar cell. According to an embodiment of the present application, the method comprises:
[0078] Mixing the hole transport material of the above embodiment with a solvent to form a mixed solution;
[0079] The mixed solution is spin-coated on the surface of the metal oxide substrate, and heated and annealed, thereby forming a hole transport layer on the surface of the metal oxide substrate.
[0080] According to some specific embodiments of the present application, the concentration of the above-mentioned hole transport material in the above-mentioned mixed solution is 0.1 mg / mL-4.0 mg / mL, for example, it can be 0.1 mg / mL, 0.2 mg / mL, 0.5 mg / mL, 0.8 mg / mL, 1 mg / mL, 1.5 mg / mL, 2 mg / mL, 2.5 mg / mL, 3.5 mg / mL, 4.0 mg / mL, etc. By limiting the concentration of the hole transport material in the above-mentioned mixed solution to the above-mentioned range, the hole transport material can be more effectively anchored on the metal oxide substrate, thereby improving the coverage of the hole transport material on the metal oxide substrate; a hole transport interface can be further effectively formed on the metal oxide substrate, and defects on the metal oxide can be further effectively passivated; defects on the interface below the perovskite light absorption layer can be further effectively passivated, thereby improving the crystallization quality of the perovskite; the flexibility of the hole transport material can be further effectively adjusted, the band structure can be optimized, hole transport can be enhanced, and the carrier transport performance can be improved.
[0081] According to some further specific embodiments of the present application, the mixed solution is spin-coated at a rotation speed of 3000 rpm-5000 rpm for 20s-40s, for example, at a rotation speed of 4000 rpm for 30s.
[0082] According to some specific embodiments of the present application, the metal oxide substrate after spin coating the mixed solution is placed on a hot plate at 90° C.-110° C. for heating and annealing for 5 min-15 min, for example, placed on a hot plate at 100° C. for heating and annealing for 10 min.
[0083] In the embodiments of the present application, the specific type of the above-mentioned solvent is not particularly limited. As some preferred schemes, the above-mentioned solvent is at least one of chloroform, chlorobenzene, ethyl acetate, tetrahydrofuran, dichloroethane, isopropanol, acetone, ethanol, N,N-dimethylformamide and 2-methoxyethanol.
[0084] The metal oxide substrate includes a transparent conductive oxide layer and a substrate (eg, glass).
[0085] Furthermore, the above method also includes:
[0086] forming a perovskite light absorbing layer on a surface of the hole transport layer away from the metal oxide substrate;
[0087] forming an electron transport layer on a surface of the perovskite light absorbing layer away from the hole transport layer;
[0088] An electrode layer is formed on a surface of the electron transport layer away from the perovskite light absorbing layer.
[0089] In the embodiments of the present application, the preparation method of the perovskite absorption layer is not particularly limited, and a conventional preparation method in the art can be used, and the person skilled in the art can select according to actual needs. As some specific examples, the preparation method of the above-mentioned perovskite absorption layer can be to first prepare a perovskite precursor solution, and then prepare a perovskite film by dip coating, spin coating, blade coating, slit coating, rod coating or inkjet printing.
[0090] In the embodiments of the present application, the preparation method of the electron transport layer is not particularly limited, and a conventional preparation method in the art can be used, and those skilled in the art can select according to actual needs. As some specific examples, the electron transport layer can be prepared by vacuum evaporation, magnetron sputtering, atomic layer deposition, electrochemical deposition, molecular beam evaporation, solvent-dissolved dip coating, spin coating, blade coating, slit coating, rod coating or inkjet printing.
[0091] In the fifth aspect of the present application, the present application proposes an electrical device. According to an embodiment of the present application, the electrical device has the above perovskite solar cell. Therefore, the electrical device has all the advantages of the perovskite solar cell, which will not be repeated here.
[0092] Specifically, electrical equipment may include lighting elements, display elements, mobile devices, etc., and may specifically include street lights, signal indicators, insect killer lamps, electric fans, electric toys, electric tools, battery vehicles, electric vehicles, ships, spacecraft, etc., among which electric toys may include fixed or mobile electric toys, for example, game consoles, electric car toys, electric ship toys and electric airplane toys, etc., and spacecraft may include airplanes, rockets, space shuttles and spacecraft, etc.; photovoltaic power generation systems may include large-scale ground photovoltaic power generation systems, distributed photovoltaic power generation and building integrated photovoltaic power generation systems, etc.
[0093] The embodiments of the present application are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. In addition, unless otherwise explicitly stated, all reagents used in the following embodiments are commercially available or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.
[0094] Example 1
[0095] (1) A method for preparing a hole transport material H1 is provided, comprising the following steps:
[0096] Synthesis step 1: Add 1,2-dibromoethane (5mmol), diphenylphosphine (2mmol), tetrabutylammonium bromide (0.7mmol), and 50% potassium hydroxide aqueous solution (50mmol) to a 150mL dry three-necked round-bottom flask in sequence. Heat and stir at 70°C for 24h under N2 atmosphere. After the reaction is completed, cool to room temperature, add dichloromethane and deionized water. Extract repeatedly with dichloromethane 3-4 times, and collect the organic phase in a conical flask. The combined organic layer is dried over anhydrous sodium sulfate, and the organic phase is dried under reduced pressure and then separated and purified by silica gel column chromatography (the volume ratio of petroleum ether and dichloromethane is 3:1) to obtain intermediate 2.
[0097] Synthesis step 2: Add intermediate 2 (2 mmol) and triethyl phosphite (10 mL, 60 mmol) to a 100 mL dry three-necked round-bottom flask, heat to 140 ° C and stir for 12 h under N2 atmosphere. After the reaction is completed, cool to room temperature, extract repeatedly with dichloromethane 3-4 times, and collect the organic phase in a conical flask. The combined organic layer is dried over anhydrous sodium sulfate, and the organic phase is dried under reduced pressure and separated and purified by silica gel column chromatography (the volume ratio of dichloromethane to ethyl acetate is 30:1) to obtain intermediate 3.
[0098] Synthesis step 3: Add intermediate 3 (1.0 mmol) and 20 mL of dichloromethane to a 50 mL dry round-bottom flask to dissolve, slowly drop 2 mL of trimethylsilyl bromide, and stir at room temperature for 9 h. After the reaction is completed, remove the solvent under reduced pressure and add 50 mL of methanol. Then add 60 mL of water dropwise until the solution becomes turbid, stir at room temperature for 12 h, filter and wash with deionized water, and dry to obtain hole transport material H1.
[0099] By referring to the above method and replacing the raw materials, different hole transport materials H2, H3, H4, H5, H6, H7, and H8 can be prepared, which will not be described in detail here.
[0100] (2) A method for preparing a perovskite solar cell is provided below, comprising the following steps:
[0101] Step 1: Spin-coat a 0.5 mg / mL H1 solution (solvent is isopropanol) on a clean ITO transparent conductive substrate at 4000 rpm for 30 seconds. Place the ITO glass coated with the H1 solution on a hot plate at 100°C for 10 minutes to form a hole transport layer with a thickness of about 2.5 nm.
[0102] Step 2: Dissolve 622.36 mg of lead iodide, 10.73 mg of iodomethylamine, 17.53 mg of cesium iodide and 208.94 mg of iodomethylamine perovskite material in 1 mL of a mixed solvent of N,N-dimethylformamide and dimethyl sulfoxide (4:1 v:v), and stir at room temperature until completely dissolved to obtain a perovskite precursor solution.
[0103] Step 3: In a nitrogen glove box, take 60 μL of perovskite precursor solution and drop it onto the clean ITO conductive glass. Spin-coat at 500 rpm and 4000 rpm for 5 s and 35 s respectively. After 25 s, slowly drop 400 μL of anisole. Then place the ITO glass on a hot stage and heat and anneal at 150 °C for 15 min to form a perovskite light-absorbing layer of about 500 nm.
[0104] Step 4: Transfer the ITO conductive glass with the perovskite light-absorbing layer to the vacuum coating instrument and wait until the vacuum degree is 3*10 -4 C60 was evaporated at 500 Pa to obtain an electron transport layer with a thickness of about 30 nm.
[0105] Step 5: Transfer the ITO conductive glass with the hole transport layer, perovskite light absorption layer and electron transport layer to the glove box, scrape out the negative electrode area, and then transfer it to the vacuum coating instrument and wait until the vacuum degree is 6*10 -4 A silver electrode was evaporated at 100 nm in thickness to obtain an electrode layer.
[0106] Example 2
[0107] The preparation method of Example 2 is substantially the same as that of Example 1, except that:
[0108] When H1 is replaced by H2, the thickness of the formed hole transport layer is about 3 nm.
[0109] Example 3
[0110] The preparation method of Example 3 is substantially the same as that of Example 1, except that H1 is replaced by H3, and the thickness of the formed hole transport layer is about 4 nm.
[0111] Example 4
[0112] The preparation method of Example 4 is substantially the same as that of Example 1, except that H1 is replaced by H4, and the thickness of the formed hole transport layer is about 2.5 nm.
[0113] Example 5
[0114] The preparation method of Example 5 is substantially the same as that of Example 1, except that H1 is replaced by H5, and the thickness of the formed hole transport layer is about 4 nm.
[0115] Example 6
[0116] The preparation method of Example 6 is substantially the same as that of Example 1, except that H1 is replaced by H6, and the thickness of the formed hole transport layer is about 2.5 nm.
[0117] Example 7
[0118] The preparation method of Example 7 is substantially the same as that of Example 1, except that H1 is replaced by H7, and the thickness of the formed hole transport layer is about 2.5 nm.
[0119] Example 8
[0120] The preparation method of Example 8 is substantially the same as that of Example 1, except that H1 is replaced by H8, and the thickness of the formed hole transport layer is about 2.5 nm.
[0121] Example 9
[0122] The preparation method of Example 9 is substantially the same as that of Example 1, except that the concentration of the H1 solution is replaced from 0.5 mg / mL to 0.1 mg / mL.
[0123] Example 10
[0124] The preparation method of Example 10 is substantially the same as that of Example 1, except that the concentration of the H1 solution is replaced from 0.5 mg / mL to 1 mg / mL.
[0125] Embodiment 11
[0126] The preparation method of Example 11 is substantially the same as that of Example 1, except that the concentration of the H1 solution is replaced from 0.5 mg / mL to 2 mg / mL.
[0127] Example 12
[0128] The preparation method of Example 12 is substantially the same as that of Example 1, except that the concentration of the H1 solution is replaced from 0.5 mg / mL to 4 mg / mL.
[0129] Comparative Example 1
[0130] The preparation method of this comparative example is substantially the same as that of Example 1, except that H1 is replaced by [2-(9H-carbazole-9-yl)ethyl]phosphonic acid.
[0131] The perovskite solar cells prepared in Examples 1 to 12 and Comparative Example 1 were tested using a simulated light source system, and the relevant performance test results are shown in Table 1.
[0132] Table 1
[0133]
[0134]
[0135] It can be seen from Table 1 that compared with Comparative Example 1, the open circuit voltage (V OC ) and photoelectric conversion efficiency (PCE) are significantly improved. Embodiments 1-8 benefit from the combination of phenylphosphine in phenylphosphine phosphonic acid organic compounds with uncoordinated lead, and the combination of anchoring groups with metal oxides, so that the phenylphosphine phosphonic acid organic compounds in the hole transport layer bridge the perovskite light absorption layer and the metal oxide substrate respectively, thereby improving the hole transport capacity of the hole transport layer; at the same time, by passivating the lower interface defects of the perovskite, the perovskite crystal quality is improved. Thereby, the battery performance of the perovskite solar cells of Embodiments 1-8 is significantly improved. It can also be seen from Table 1 that the comprehensive performance of the perovskite solar cells of Embodiments 1 and 10 is excellent compared with Embodiments 9, 11-12. It can be seen that the concentration of H1 is preferably 0.5mg / mL-1mg / mL.
[0136] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0137] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A phenylphosphonic acid organic compound, characterized in that: Including at least one of the compound shown in formula I and the compound shown in formula II: Wherein, R1 includes a C1-C8 alkyl chain or at least one aryl chain; R2 includes a C1-C8 alkyl chain or at least one aryl chain, X - These include halide ions, sulfonate ions, benzenesulfonate ions, thiocyanate ions, tetrafluoroborate ions, hexafluorophosphate ions, formate ions, or acetate ions.
2. The phenylphosphonic acid organic compound according to claim 1, characterized in that: R1 includes a C1-C6 alkyl chain, an aryl chain or two aryl chains; R2 includes a C1-C4 alkyl chain; X - Including halide ions.
3. The phenylphosphonic acid organic compound according to claim 1, characterized in that: Includes at least one of the following compounds:
4. A hole transport material, characterized in that The invention comprises the phenylphosphonic acid organic compound described in any one of claims 1 to 3.
5. A perovskite solar cell, characterized in that: The invention comprises a hole transport layer, wherein the hole transport layer comprises the hole transport material according to claim 4.
6. The perovskite solar cell according to claim 5, characterized in that: The thickness of the hole transport layer is 1nm-10nm; And / or, the hole transport layer is a SAM layer.
7. The perovskite solar cell according to claim 5 or 6, characterized in that: It also includes a metal oxide substrate, a perovskite light-absorbing layer, an electron transport layer and an electrode layer. The metal oxide substrate, the hole transport layer, the perovskite light-absorbing layer, the electron transport layer and the electrode layer are stacked in sequence.
8. The perovskite solar cell according to claim 7, characterized in that: The thickness of the perovskite light absorbing layer is 100nm-3μm; And / or, the thickness of the electron transport layer is 1 nm-100 nm.
9. The perovskite solar cell according to claim 7, characterized in that: The perovskite light-absorbing layer comprises an ABX3 type perovskite material, wherein the A ions comprise at least one of cesium ions, rubidium ions, potassium ions, methylamine ions, formamidine ions, methylenediamine ions, benzamidine cations, and guanidinium cations, the B ions comprise at least one of divalent lead ions and divalent tin ions, and the X ions comprise at least one of fluoride ions, chloride ions, bromide ions, iodide ions, thiocyanate ions, tetrafluoroborate ions, hexafluorophosphate ions, formate ions, and acetate ions; and / or, the electron transport layer comprises at least one of tin dioxide, titanium dioxide, [6,6]-phenyl-C71-butyric acid isomethyl ester, C60 and a C60 derivative; And / or, the electrode layer includes at least one of ITO, IZO, IWO, FTO, ICO, AZO, BZO, gold, silver, copper, aluminum, and carbon; And / or, the metal oxide substrate includes ITO, IZO, IWO, FTO, ICO, AZO, BZO, TiO2, NiO x , Al2O3 or SiO2.
10. A method for preparing a perovskite solar cell, characterized in that: include: Mixing the hole transport material according to claim 4 with a solvent to form a mixed solution; The mixed solution is spin-coated and heated for annealing to form a hole transport layer.
11. The method according to claim 10, characterized in that The concentration of the hole transport material in the mixed solution is 0.1 mg / mL-4.0 mg / mL.
12. An electrical equipment, characterized in that: A perovskite solar cell according to any one of claims 5 to 9 or a perovskite solar cell prepared by the method according to claim 10 or 11.
Citation Information
Patent Citations
Preparation method of palladium complex and conjugated aromatic polymer
CN102424694A
Hole transport material, solar cell and preparation method thereof, and photovoltaic module
CN118076202A
Perovskite solar cell and preparation method thereof
CN118201445A
Layered carboxy end terminated organophosphorus inorganic polymers
US4235990A
Transition metal catalysts based on inorganic-organic polymers, manufacture and use thereof
WO1997035661A1
Cited By
Perovskite solar cell module self-assembled monomolecular hole transport material and preparation method thereof
CN119504856A
Perovskite solar cell module self-assembled monomolecular hole transport material and preparation method thereof
CN119504856B