Spectrum-adjustable aluminate matrix fluorescent powder as well as preparation method and application thereof
The spectrum of the aluminate matrix phosphor can be adjusted, and the excitation peak is purple or green light, and the emission peak is in the blue or far red light region, which solves the problem of insufficient excitation spectrum properties of the existing phosphor, and improves crop photosynthesis and solar energy Battery photoelectric conversion efficiency.
Patent Information
- Application Number
- CN202410905715.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-08
AI Technical Summary
The existing phosphors cannot meet the requirements of efficient pure blue light emission, pure red light emission and red blue dual emission in terms of excitation spectral properties, and cannot effectively improve crop photosynthesis efficiency and photoelectric conversion efficiency of solar cells.
The aluminate matrix phosphor using La1-xAl10.8-x-yMg0.10Si0.10+xO18:xEu2+, yCr3+ is used to adjust the values of x and y to achieve spectral control. The excitation peak is purple or green light and emits The peak is in the blue or far red light region, matching the response spectrum of crop chlorophyll and solar cells.
It realizes the simultaneous absorption of ultraviolet and green light, emits blue and far red light, improves the crop photosynthesis efficiency and the photoelectric conversion efficiency of solar cells, and extends the life of the photovoltaic power generation packaging film.
Smart Images

Figure CN118879322A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of luminescent materials, and in particular to a spectrum-adjustable aluminate-based phosphor and a preparation method and application thereof. Background Art
[0002] Light-conversion film, also known as light conversion film, refers to a film that uses optical principles to achieve spectrum conversion effects by adding light-conversion materials (such as phosphors) to the film. Light-conversion film has the advantages of high light absorption, green environmental protection, and good light transmittance, and is used in photovoltaic power generation and facility agriculture.
[0003] In photovoltaic power generation, solar cells have a weak spectral response to short-wave photons in sunlight and cannot effectively absorb and utilize this part of the photon spectrum. CN101699636A discloses a fluorescent film for solar cells, which has attracted widespread attention due to its obvious light conversion effect. The fluorescent film can convert light (ultraviolet light or part of visible light) with a low response efficiency to solar cells into long-wave light with a higher response efficiency, thereby improving the photoelectric conversion efficiency of solar cells.
[0004] However, in the actual manufacturing process of heterojunction modules, the most commonly used adhesive films in the industry are high-transmittance films and UV cut-off films. The initial power of modules using high-transmittance films is higher than that of modules using UV cut-off films, but the latter attenuates less. After UV exposure and attenuation, the power of the two is the same. HJT (Homojunction Solar Cell) cells, that is, heterojunction solar cells, are solar cells using crystalline silicon materials. The passivation layer of the cell is sensitive to ultraviolet rays, and the cell is prone to light aging. The components prepared with light-conversion films combine the advantages of both. The initial power is equivalent to that of modules using high-transmittance films, and its UV attenuation performance is equivalent to that of modules using UV cut-off films. Therefore, it is urgent to find a light-conversion material that converts the ultraviolet band into a blue light spectrum near the 440nm band, thereby improving the ultraviolet spectrum response efficiency of heterojunction cells, shielding ultraviolet light to protect the battery and increase battery life.
[0005] In terms of facility agriculture, blue light plays an important role in the early stages of crop growth. Exposure to blue light can not only help some seeds germinate, but also ensure the strong growth of their roots, stems and leaves. This is due to the fact that blue light can promote crops to produce more chlorophyll, helping seedlings to better absorb and utilize energy in photosynthesis, allowing crops to grow and mature faster. Far-red light can increase the chlorophyll content in crop leaves and improve the light absorption efficiency of photosynthetic pigments, thereby enhancing the ability of photosynthesis. At the same time, far-red light can also promote the synthesis of photosynthetic enzymes in crop leaves and increase the rate of photosynthesis. Therefore, an appropriate amount of far-red and blue light irradiation can improve the photosynthesis efficiency of crops and promote the synthesis and accumulation of photosynthetic products of crops.
[0006] Therefore, the combination of green-to-red (GTR) and ultraviolet-to-blue (VTB) photoluminescent materials can optimize the overlap of chlorophyll's absorption capacity for red and blue light. These light-converting materials mixed with polyolefins or ethylene-vinyl acetate copolymer resins to make light-converting agricultural films can improve the photosynthetic efficiency of crops and have achieved significant economic and social benefits. GTR phosphors such as CaS:Eu 2+ , core-shell structure CaS:Eu 2+ @CaZnOS and Eu 2+ Doped nitride (CaAlSiN3:Eu 2+ and Sr2Si5N8:Eu 2+ ) have been reported as solar spectrum conversion materials. These materials convert the poorly absorbed green part of sunlight into red light, but due to their poor stability, their application is limited in some fields that require long-term stable operation. The absorption characteristics in the 300-380nm spectral region (ultraviolet, UV) are related to crops. In most cases, converting ultraviolet light into blue light plays an important role in photosynthesis. It can activate the photosynthetic activity of chlorophyll and other photosynthetic pigments and promote the activation of photosynthetic enzymes. However, to accurately convert ultraviolet and green light in the solar spectrum into blue and red light that is beneficial to the growth of crops, purple-to-red (VTB), purple / green-to-far-red (V / GTFR) and purple / green-to-blue / far-red (V / GTB / FR) phosphors with higher light conversion efficiency are needed.
[0007] Chinese patent application document CN110724531A discloses a spectrum-adjustable red and blue dual-emission europium-doped aluminate phosphor, which has the following chemical formula: CaY 2-x Al4SiO 12 :xEu, where x ranges from 0.001 to 0.05. The phosphor can emit blue light with a main peak of 420nm and red light with a main peak of 615nm under the excitation of ultraviolet light of 230 to 375nm; although the phosphor provided by this solution is single-doped, it can achieve red and blue dual emission and has adjustable characteristics, but it does not accurately correspond to crop chlorophyll b, β-carotene and P fr The absorption spectrum of photosensitive pigments does not correspond to the maximum response spectrum of perovskite and amorphous silicon solar photovoltaic cells, so it cannot effectively improve the photosynthesis efficiency of crops and promote crop production; it also cannot effectively absorb and utilize photons in sunlight, so the photoelectric conversion efficiency still needs to be improved.
[0008] Therefore, in order to address the problems existing in the prior art, the present invention provides a new phosphor with high luminous efficiency, which can absorb ultraviolet light and green light at the same time, emit blue light and far-red light, and can also be adjusted to emit pure blue light or far-red light. When applied to solar greenhouse film or light-converting film glass, it can promote crop photosynthesis and the establishment of light morphology; when applied to solar photovoltaic power generation, it can slow down the aging rate of photovoltaic power generation encapsulation film and improve the photoelectric conversion efficiency of solar cells. Summary of the invention
[0009] The technical problem to be solved by the present invention is to provide a spectrum-adjustable aluminate-based phosphor and its preparation and application. The purpose is to solve the problem that the excitation spectrum properties of existing phosphors on the market cannot meet the requirements of efficient pure blue light emission, pure red light emission and red and blue dual emission, and to provide a phosphor with a main excitation peak of purple or green light, an emission peak in the blue light or far-red light region, and a strong affinity with crop chlorophyll b, carotenoids and P fr Phosphors whose absorption spectra of photosensitive pigments overlap with the high-efficiency response spectra of perovskites and amorphous silicon solar photovoltaic cells can be used in fields such as solar greenhouses and solar photovoltaic power generation to promote crop photosynthesis and the establishment of light forms; or, to slow down the aging rate of photovoltaic power generation encapsulation films and improve the photoelectric conversion efficiency of solar cells.
[0010] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0011] In a first aspect, the present invention provides a spectrum-adjustable aluminate-based phosphor, the phosphor comprising a compound represented by the following formula (I):
[0012] La 1-x Al 10.8-x-y Mg 0.10 Si 0.10+x O 18 :xEu 2+ ,yCr 3+ (I)
[0013] In formula (I), 0≤x<0.08; 0≤y<0.2; x and y are not 0 at the same time.
[0014] It can be understood that when y=0, formula (I) is simplified to: La 1-x Al 10.8-x Mg 0.10 Si 0.10+x O 18 :xEu 2+ When x=0, formula (I) is simplified as: LaAl 10.8-y Mg 0.10 Si 0.10 O 18 :yCr3+ .
[0015] Furthermore, the purple or green light excitation peak of the phosphor is the main excitation peak; its emission peak is in the blue or far-red region, which is consistent with crop chlorophyll b, carotenoids and P fr The absorption spectra of photosensitive pigments or the high-efficiency response spectra of perovskites and amorphous silicon solar photovoltaic cells overlap.
[0016] Further, when y=0 in formula (I), the excitation wavelength of the phosphor is 250-400 nm, and the emission wavelength is 400-500 nm in the blue light region;
[0017] When x=0 in formula (I), the main excitation wavelength of the phosphor is 200-300nm in the far ultraviolet region, 300-490nm in the blue-violet region, 490-600nm in the green region, and the emission wavelength is 600-900nm in the far red region;
[0018] When x≠0 and y≠0 in formula (I), the main excitation wavelength of the phosphor is 200-300nm in the far ultraviolet region, 300-490nm in the blue-violet region, 490-600nm in the green region, and the emission wavelength is 400-500nm in the blue region and 600-900nm in the far red region.
[0019] Furthermore, the phosphor is selected from one or more of the following compounds:
[0020] (1)La 0.97 Al 10.97 Mg 0.10 Si 0.13 O 18 :0.03Eu 2+ ;
[0021] (2)La 0.95 Al 10.95 Mg 0.10 Si 0.15 O 18 :0.05Eu 2+ ;
[0022] (3) LaAl 10.73 Mg 0.10 Si 0.10 O 18 :0.07Cr 3+ ;
[0023] (4) LaAl 10.68 Mg 0.10 Si 0.10 O 18 :0.12Cr 3+ ;
[0024] (5)La 0.97 Al 10.70 Si 0.13 Mg 0.10 O 18 :0.03Eu 2+ ,0.07Cr 3+ ;
[0025] (6)La 0.97 Al 10.65 Si 0.13 Mg 0.10 O 18 :0.03Eu 2+ ,0.12Cr 3+ .
[0026] In a second aspect, the present invention provides a method for preparing the spectrum-adjustable aluminate-based phosphor as described above, the preparation method comprising the following steps:
[0027] (1) weighing raw materials of each element according to the atomic stoichiometric ratio of each element, uniformly mixing them, and then ball milling to obtain a solid mixture;
[0028] (2) The obtained solid mixture is calcined in a carbon reducing atmosphere, cooled to room temperature and then fully ground to obtain the obtained solid mixture; the calcination temperature is 1400-1600°C, and the calcination time is 6-10 hours. The calcination temperature is more preferably 1500-1600°C.
[0029] Furthermore, the conditions for ball milling in step (1) are as follows: ball to material ratio is 1:1, ball milling time is 25 to 35 minutes, and speed is 180 to 200 rpm. Preferably, the ball milling time is 30 minutes and speed is 200 rpm.
[0030] Furthermore, in step (1), the raw material of the Al element is aluminum hydroxide.
[0031] Furthermore, in step (1), the raw material of the La element is lanthanum oxide.
[0032] Furthermore, in step (1), the raw material of the Mg element is magnesium oxide.
[0033] Furthermore, in step (1), the raw material of the Eu element is europium oxide.
[0034] Furthermore, in step (1), the raw material of the Cr element is chromium oxide.
[0035] Furthermore, in step (1), the raw material of Si element is silicic acid.
[0036] Furthermore, the carbon reducing atmosphere in step (2) is a CO or H2 atmosphere.
[0037] In a third aspect, the present invention further provides the use of the spectrum-adjustable aluminate-based phosphor as described above or the spectrum-adjustable aluminate-based phosphor prepared by the preparation method as described above.
[0038] Furthermore, the application is to use the phosphor in solar greenhouse covering materials to provide an optimal action spectrum close to crop growth to promote crop growth. Alternatively, the phosphor is used in solar photovoltaic power generation to improve the photoelectric conversion efficiency of solar cells.
[0039] Furthermore, the application is specifically to add the phosphor as a raw material to the preparation process of agricultural plastic greenhouse film or laminated glass or encapsulation film for solar photovoltaic power generation, so that the prepared light-converting agricultural film or light-converting film laminated glass or light-converting film for solar photovoltaic power generation has photoluminescent properties.
[0040] Furthermore, the raw materials for preparing the glass include glass glue and the fluorescent powder, and the mass of the fluorescent powder is 0.1% to 1.0% of the mass of the glass glue. The glass glue generally adopts glass resin, such as UV-photosensitive liquid resin.
[0041] The present invention has the following beneficial effects:
[0042] (1) The aluminate-based phosphor provided by the present invention can realize spectrum controllability, can absorb ultraviolet light and green light at the same time, emit blue light and far-red light, and can also be adjusted to be a pure blue light emitting phosphor or a far-red light emitting phosphor.
[0043] The emission peak of the phosphor of the present invention is in the blue light or far red light region, and the dual emission peaks are 440nm and 730nm, which are consistent with the absorption peak of crop chlorophyll (a, b) in the blue region and P fr The absorption peak of the pigment is very consistent. The fluorescent powder of the present invention takes the purple light or green light excitation peak as the main excitation peak, and the excitation spectrum is located in the blue-purple region and the green light region. It is applied to the greenhouse film of the greenhouse of the facility agriculture, and can effectively convert the ultraviolet light and green light that are less absorbed by the green crops into the blue light and P required for photosynthesis. fr Pigments efficiently absorb far-red light, promoting crop photosynthesis and the formation of light forms. Pure blue light emitting phosphors, whose excitation peaks and emission peaks overlap with the high-efficiency response spectra of perovskite and amorphous silicon solar photovoltaic cells, can efficiently convert ultraviolet light into blue light. They are used in the manufacture of encapsulation films for solar photovoltaic cells, which can not only slow down the aging rate of polymer films, but also improve the photoelectric conversion efficiency of solar cells.
[0044] Therefore, the fluorescent powder provided by the present invention can be used for crop growth lighting to provide an optimal action spectrum close to crop growth to promote crop growth, and can also be used for solar photovoltaic power generation to improve the photoelectric conversion efficiency of solar cells, and has a wide range of applications.
[0045] (2) The phosphor preparation method provided in the present application is simple and can be obtained by using existing phosphor preparation equipment, and is suitable for large-scale, industrialized production. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is the X-ray powder diffraction pattern of the phosphor of Example 1 of the present invention.
[0047] Figure 2 The X-ray powder diffraction pattern of the phosphor of Example 3 of the present invention is
[0048] Figure 3 The X-ray powder diffraction pattern of the phosphor of Inventive Example 5 is
[0049] Figure 4 This is the emission spectrum of the phosphor in Example 1 of the present invention (excitation wavelength 308 nm, monitoring wavelength 440 nm).
[0050] Figure 5 This is the emission spectrum of the phosphor of Invention Example 3 (excitation wavelength 519 nm, monitoring wavelength 730 nm).
[0051] Figure 6 This is the emission spectrum of the phosphor of Inventive Example 5 (excitation wavelength 308 nm, monitoring wavelength 440 nm).
[0052] Figure 7 This is the emission spectrum of the phosphor of Inventive Example 5 (excitation wavelength 519 nm, monitoring wavelength 713 nm).
[0053] Figure 8 The emission spectrum of the phosphor in Example 1 of the present invention is compared with the absorption spectrum of chlorophyll b and carotene of crops.
[0054] Fig. 9 The emission spectrum of the phosphor in Example 3 of the present invention is similar to that of the crop phytochrome P fr Comparison of absorption spectra.
[0055] Fig.10 The emission spectrum of the phosphor in Example 5 of the present invention is similar to that of carotene and crop phytochrome P fr Comparison of absorption spectra.
[0056] Fig.11 The figure is a comparison between the emission spectrum of the phosphor of Example 1 of the present invention and the effect curve of the perovskite solar cell.
[0057] Fig.12 The figure is a comparison between the emission spectrum of the phosphor of Example 1 of the present invention and the effect curve of an amorphous silicon solar cell.
[0058] Fig.13The real-time spectrum of sunlight converted by the light-converting laminated glass in Example 5 of the present invention. DETAILED DESCRIPTION
[0059] As used herein:
[0060] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0061] When a parameter is expressed as a range, a preferred range, or a range limited by a series of upper preferred values and lower preferred values, it should be understood that all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value are specifically disclosed, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0062] In these examples, parts and percentages are by mass unless otherwise indicated.
[0063] "Weight parts" / "mass parts" refers to the basic measurement unit that indicates the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g, 2g, etc. If we say that the mass parts of component A are a parts and the mass parts of component B are b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Or, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass parts of all components is not limited to 100 parts.
[0064] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0065] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing the specific embodiments and are not intended to limit the present invention. In the embodiments, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0066] The present invention provides a spectrum-adjustable aluminate-based phosphor, which comprises a compound represented by the following formula (I): La 1-x Al 10.8-x-y Mg 0.10 Si 0.10+x O 18 :xEu 2+ ,yCr 3+ (I)
[0067] In formula (I), 0≤x<0.08; 0≤y<0.2; x and y are not 0 at the same time.
[0068] The phosphor can be prepared by the following method:
[0069] (1) Raw materials are weighed according to the stoichiometric ratio of Al(OH)3, La2O3, Eu2O3, MgO, H2SiO3, and Cr2O3, mixed in a specific ratio, and then ball-milled to obtain a solid mixture; wherein the ball-milling conditions are as follows: the ball-milling time is 25 to 35 minutes, and the speed is 180 to 200 rpm. The ball-milling time is generally 30 minutes, and the speed is 200 rpm.
[0070] (2) calcining the solid mixture in a carbon reducing atmosphere, wherein the carbon reducing atmosphere is a CO or H2 atmosphere; the calcination temperature is 1400°C to 1600°C, and the calcination time is 6 to 10 hours. Then, the mixture is naturally cooled to room temperature and fully ground to obtain the product.
[0071] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Preferred embodiments of the present invention are provided in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0072] Example 1La 0.97 Al 10.97 Mg 0.10 Si 0.13 O 18 :0.03Eu 2+ Phosphor
[0073] This embodiment provides a method for preparing a phosphor, comprising the following steps:
[0074] (1) The raw materials are weighed according to the stoichiometric ratio, specifically as follows: 0.2844 g of lanthanum oxide (La2O3), 1.5121 g of aluminum hydroxide (Al(OH)3), 0.0095 g of europium oxide (Eu2O3), 0.0073 g of magnesium oxide (MgO), 0.0188 g of silicic acid (H2SiO3) and 0.0890 g of boric acid (H3BO3) are mixed and ball-milled to obtain a mixed powder; the ball-milling time is 30 min, and the speed is 200 rpm.
[0075] (2) The mixed powder was poured into an alumina crucible and calcined in a carbon reducing atmosphere in a box-type high temperature furnace at 1400°C for 10 h. The carbon reducing atmosphere was H2 atmosphere. The mixture was cooled to room temperature and ground thoroughly to obtain La 0.97 Al 10.97 Mg 0.10 Si 0.13 O 18 :0.03Eu 2+ Blue phosphor.
[0076] Example 2La 0.95 Al 10.95 Mg 0.10 Si 0.15 O 18 :0.05Eu 2+ Phosphor
[0077] This embodiment provides a method for preparing a phosphor, comprising the following steps:
[0078] (1) The raw materials are weighed according to the stoichiometric ratio, specifically as follows: 0.2786 g of lanthanum oxide (La2O3), 1.5093 g of aluminum hydroxide (Al(OH)3), 0.0158 g of europium oxide (Eu2O3), 0.0073 g of magnesium oxide (MgO), 0.0217 g of silicic acid (H2SiO3) and 0.0890 g of boric acid (H3BO3) are mixed and ball-milled to obtain a mixed powder; the ball-milling time is 30 min, and the speed is 200 rpm.
[0079] (2) The mixed powder was poured into an alumina crucible and calcined in a carbon reducing atmosphere in a box-type high temperature furnace at 1600°C for 6 hours. The carbon reducing atmosphere was CO atmosphere. The mixture was cooled to room temperature and ground thoroughly to obtain La 0.95 Al 10.95 Mg 0.10 Si 0.15 O 18 :0.05Eu 2+ Phosphor.
[0080] Example 3 LaAl 10.73 Mg 0.10 Si 0.10 O 18 :0.07Cr 3+ Phosphor
[0081] This embodiment provides a method for preparing a phosphor, comprising the following steps:
[0082] (1) The raw materials are weighed according to the stoichiometric ratio, specifically as follows: 0.2932 g of lanthanum oxide (La2O3), 1.5065 g of aluminum hydroxide (Al(OH)3), 0.0096 g of chromium oxide (Cr2O3), 0.0145 g of silicate (H2SiO3), 0.0073 g of magnesium oxide (MgO) and 0.0890 g of boric acid (H3BO3) are mixed and ball-milled to obtain a mixed powder; the ball-milling time is 30 min, and the speed is 200 rpm.
[0083] (2) The mixed powder was poured into an alumina crucible and calcined in a carbon reducing atmosphere in a box-type high temperature furnace at 1500°C for 10 h. The carbon reducing atmosphere was H2 atmosphere. The mixture was cooled to room temperature and ground thoroughly to obtain LaAl 10.73 Mg 0.10 Si 0.10 O 18 :0.07Cr 3+ Phosphor.
[0084] Example 4 LaAl 10.68 Mg 0.10 Si 0.10 O 18 :0.12Cr 3+ Phosphor
[0085] This embodiment provides a method for preparing a phosphor, comprising the following steps:
[0086] (1) The raw materials are weighed according to the stoichiometric ratio, specifically as follows: 0.2932 g of lanthanum oxide (La2O3), 1.4995 g of aluminum hydroxide (Al(OH)3), 0.0164 g of chromium oxide (Cr2O3), 0.0145 g of silicate (H2SiO3), 0.0073 g of magnesium oxide (MgO) and 0.0890 g of boric acid (H3BO3) are mixed and ball-milled to obtain a mixed powder; the ball-milling time is 30 min, and the speed is 200 rpm.
[0087] (2) The mixed powder was poured into an alumina crucible, calcined in a carbon reducing atmosphere in a box-type high-temperature furnace at 1500°C for 10 h, cooled to room temperature, and fully ground to obtain LaAl 10.68 Mg 0.10 Si0.10 O 18 :0.12Cr 3+ Phosphor.
[0088] Example 5La 0.97 Al 10.70 Mg 0.10 Si 0.13 O 18 :0.03Eu 2+ ,0.07Cr 3+ Phosphor
[0089] This embodiment provides a method for preparing a phosphor, comprising the following steps:
[0090] (1) The raw materials are weighed according to the stoichiometric ratio, specifically as follows: 0.2844 g of lanthanum oxide (La2O3), 1.5023 g of aluminum hydroxide (Al(OH)3), 0.0096 g of chromium oxide (Cr2O3), 0.0095 g of europium oxide (Eu2O3), 0.0188 g of silicic acid (H2SiO3), 0.0073 g of magnesium oxide (MgO) and 0.0890 g of boric acid (H3BO3) are mixed and ball-milled to obtain a mixed powder; the ball-milling time is 30 min, and the speed is 200 rpm.
[0091] (2) The mixed powder was poured into an alumina crucible, calcined in a carbon reducing atmosphere in a box-type high-temperature furnace at 1500°C for 10 h, cooled to room temperature, and fully ground to obtain La 0.97 Al 10.70 Si 0.13 Mg 0.10 O 18 :0.03Eu 2+ ,0.07Cr 3+ Phosphor.
[0092] Example 6La 0.97 Al 10.65 Mg 0.10 Si 0.13 O 18 :0.03Eu 2+ ,0.12Cr 3+ Phosphor
[0093] This embodiment provides a method for preparing a blue phosphor, comprising the following steps:
[0094] (1) The raw materials are weighed according to the stoichiometric ratio, specifically as follows: 0.2844 g of lanthanum oxide (La2O3), 1.4953 g of aluminum hydroxide (Al(OH)3), 0.0164 g of chromium oxide (Cr2O3), 0.0095 g of europium oxide (Eu2O3), 0.0188 g of silicic acid (H2SiO3), 0.0073 g of magnesium oxide (MgO) and 0.0890 g of boric acid (H3BO3) are mixed and ball-milled to obtain a mixed powder; the ball-milling time is 30 min, and the speed is 200 rpm.
[0095] (2) The mixed powder was poured into an alumina crucible, calcined in a carbon reducing atmosphere in a box-type high-temperature furnace at 1500°C for 10 h, cooled to room temperature, and fully ground to obtain La 0.97 Al 10.65 Si 0.13 Mg 0.10 O 18 :0.03Eu 2+ ,0.12Cr 3+ Phosphor.
[0096] Example 7 Preparation of light-converting laminated glass
[0097] Formula and preparation method of light-converting film laminated glass: Add the phosphor to the UV-photosensitive liquid resin in a certain proportion, mix and ultrasonicate for 1 hour, and then fill the liquid resin containing the phosphor between two glass sheets. The size of the glass sheet is 30mm×30mm and the thickness is 3mm. The spacing between the parallel glass sheets is controlled at 0.5mm. The synthesized glass combination is exposed to sunlight until the resin is completely polymerized to obtain the luminous laminated glass.
[0098] The phosphor of this embodiment adopts the La prepared in Example 5. 0.97 Al 10.70 Mg 0.10 Si 0.13 O 18 :0.03Eu 2+ ,0.07Cr 3+ Phosphor: The mass of the phosphor is generally 0.1% to 1.0% of the mass of the liquid resin. In this embodiment, the mass ratio of the phosphor to the liquid resin is 1:100 (1%).
[0099] It is understandable that agricultural greenhouse film can also be prepared according to the formula of plastic film: the raw materials for preparing agricultural greenhouse film generally include 99.6 to 99.99 parts by mass of resin and 0.01 to 0.4 parts by mass of the fluorescent powder prepared in the above embodiment.
[0100] In order to further verify the feasibility of the method of the present invention and the performance of the prepared phosphor, the phosphor prepared in the above embodiment was subjected to the following performance characterization and testing:
[0101] 1. XRD test
[0102] The test method is: using a Japanese Rigaku XRD diffractometer to test the phosphor prepared in the above embodiment, and the results are as follows:
[0103] The X-ray powder diffraction pattern of the phosphor prepared in Example 1 of the present invention is as follows: Figure 1 As shown;
[0104] The phosphor prepared in Example 3 of the present invention has an X-ray powder diffraction pattern as shown in Figure 2 As shown;
[0105] The phosphor prepared in Example 5 of the present invention has an X-ray powder diffraction pattern as shown in Figure 3 shown.
[0106] Depend on Figure 1-3 It can be seen from the XRD diagram that the phosphor synthesized by the present invention is pure phase and free of impurities.
[0107] 2. Excitation spectrum and emission spectrum
[0108] The test method is: using Hitachi F-4700 fluorescence spectrum tester to test the phosphor prepared in the above embodiment, the results are as follows:
[0109] The excitation spectrum and emission spectrum of the phosphor prepared in Example 1 of the present invention are as follows: Figure 4 shown.
[0110] The excitation spectrum and emission spectrum of the phosphor prepared in Example 3 of the present invention are as follows: Figure 5 shown.
[0111] The excitation spectrum and emission spectrum of the phosphor prepared in Example 5 of the present invention are as follows: Figure 6 , as shown in 7.
[0112] Depend on Figure 4-7 The spectrum shows that the aluminate-based phosphor provided by the present invention can realize spectral controllability, and the purple or green light excitation peak of the phosphor is the main excitation peak; its emission peak is in the blue or far-red region, which is consistent with crop chlorophyll b, carotenoids and P fr The absorption spectra of photosensitive pigments or the maximum response spectra of perovskite and amorphous silicon solar photovoltaic cells overlap.
[0113] Specifically,
[0114] (1) The present invention provides a Eu-doped 2+ Element LaAl 10.8 Mg0.10 Si 0.10 O 18 Phosphor (chemical formula is La 1-x Al 10.8-x-y Mg 0.10 Si 0.10+x O 18 :xEu 2+ ) has the following luminescent properties: the pure phase phosphor synthesized at a temperature of 1400-1600°C has an excitation peak less than 400nm and is suitable as a good blue light emitting material.
[0115] Taking the phosphors of Examples 1 and 2 as an example, the synthesized pure phase phosphors exhibit unique luminescence characteristics: the emission peak is located in the blue region, and can accurately absorb ultraviolet light and emit blue, which is not only beneficial to the growth of green crops, thereby converting ultraviolet light in the sunlight spectrum that is less absorbed by green crops into blue that is beneficial to the growth of crops, but can also be used in solar photovoltaic cell encapsulation films to improve photoelectric conversion efficiency.
[0116] like Figure 4 As shown, the phosphors provided in Examples 1 and 2 are blue phosphors, which emit broadband blue light with a peak value at 440 nm under the excitation of ultraviolet light with a wavelength of 308 nm (UVB).
[0117] (2) The present invention provides a Cr-doped 3+ Element LaAl 10.8 Mg 0.10 Si 0.10 O 18 Phosphor (chemical formula: LaAl 10.8-y Mg 0.10 Si 0.10 O 18 :yCr 3+ ) has the following luminescent properties: the pure phase phosphor synthesized at a temperature of 1400-1600°C has excitation peaks at 399nm and 519nm.
[0118] Taking the phosphors of Examples 3 and 4 as an example, the synthesized pure phase phosphors exhibit unique luminescence characteristics: the emission peak is located in the far-red region, can accurately absorb ultraviolet light and green light, and emit far-red light, matching far-red light absorbing crops (P fr , 730nm). 730nm far-infrared light not only plays an indispensable role in the crop growth spectrum, but also works together with other wavelengths of light to provide the necessary light environment for crops. One of the most important effects of 730nm far-infrared light illumination on crops is the shade-avoiding effect, which promotes their normal growth and development. It can also be used in the encapsulation film for solar photovoltaic cells to improve the photoelectric conversion efficiency.
[0119] like Figure 5 As shown, the phosphors provided in Examples 3 and 4 are far-infrared phosphors, which emit far-red light under the excitation of ultraviolet light of 399 nm (UVA) and green light of 519 nm, with a peak at 730 nm.
[0120] (3) The present invention provides a Eu-doped 2+ With Cr 3+ Elemental LaAl 10.8 Mg 0.10 Si 0.10 O 18 Phosphor (chemical formula: La 1-x Al 10.8-x-y Mg 0.10 Si 0.10+x O 18 :xEu 2+ ,yCr 3+ ) has the following luminescent properties: the pure phase phosphor synthesized at a temperature of 1400-1600°C has excitation peaks at 308nm, 399nm and 519nm.
[0121] Taking the phosphors of Examples 5 and 6 as an example, the synthesized pure phase phosphors exhibit unique luminescent characteristics: emitting blue and red light at the same time, accurately absorbing ultraviolet and green light, and emitting far-red light. Red and blue light are the most important wavelength ranges in crop photosynthesis and have a vital impact on crop growth and development. Lights of 730nm and 440nm have different effects and influences on crop growth, flowering, and photosynthesis. When used in horticultural lighting, different effects can be achieved by adjusting the proportion of light of different wavelengths to meet the needs of different crops or different growth stages.
[0122] like Figure 6-7 As shown, the phosphors provided in Examples 5 and 6 are red and blue dual-emission phosphors, which emit blue light and far-red light under the excitation of ultraviolet light wavelengths of 308nm (UVB), 399nm (UVA) and green light wavelength of 519nm, with peak values at 440nm and 713nm.
[0123] 3. Absorption spectrum matching analysis
[0124] like Figure 8 As shown, the blue light emission spectrum generated by the phosphor provided in Example 1 under 308nm ultraviolet light excitation matches the absorption spectrum of chlorophyll b and β-carotene of crops. It can be seen that the phosphor provided by the present invention can improve the light capture ability of crops, help the growth and development of crops, and thus enhance the photosynthesis efficiency. On the other hand, it can protect crops from light damage and promote crop growth and the synthesis of nutrients.
[0125] like Fig. 9 As shown, the far-red light emission spectrum of the phosphor provided in Example 3 under 519nm green light excitation is similar to that of the crop phytochrome P fr It can be seen that when it is applied to plastic film or glass for agricultural use, it can specifically convert ultraviolet light and green light, which are less absorbed by green crops, into photosensitive pigment P fr Absorbing wavelengths is beneficial to the growth of crops and can improve the economic benefits of planting. It can control the flowering cycle of crops and the entire process from germination to nutritional growth and then to flowering.
[0126] like Fig.10 As shown, the red and blue dual emission spectrum of the phosphor provided in Example 5 under 308nm ultraviolet light excitation is similar to that of the crop phytochrome P fr The absorption spectrum matches the absorption spectrum of β-carotene. When blue light is used in combination with red light, the efficiency of photosynthesis can be improved. They affect the growth and development of crops in different ways and can provide the necessary growth conditions for crops. In the regulation of crop lighting and growth environment, full use of the characteristics of blue light and far-red light can help achieve healthy growth, high yield and high quality of crops. When the fluorescent powder provided in Example 5 of the present invention is applied to plastic film or glass for agricultural use, ultraviolet light and green light that are less absorbed by green crops can be specifically converted into red light and blue light, which are the most important in crop photosynthesis. In the regulation of crop lighting and growth environment, full use of the characteristics of blue light and far-red light can be made, thereby achieving healthy growth, high yield and high quality of crops.
[0127] like Fig.11, as shown in 12, the blue light emission spectrum generated by the phosphor provided in Example 1 under the excitation of 308nm ultraviolet light matches the corresponding curves of perovskite solar cells and amorphous silicon solar cells, so it can specifically convert ultraviolet light with low photoelectric conversion efficiency and aging of the film into the required blue, improve the power of the light conversion film component, and obtain gain at the component end. The spectral response of perovskite solar cells and amorphous silicon solar cells is basically mainly concentrated in 400-800nm. In this embodiment, the spectral response curve of amorphous silicon solar cells refers to "Analysis and Research on the Method of Representing the Light Transmittance Performance of Photovoltaic Glass, Lu University, Cao Yang"; the spectral response curve of perovskite solar cells refers to "Perovskite / c-Sitandem solar cells with realistic inverted architecture: Achieving high efficiency by optical optimization, Lixiang Ba et al.". Although different amorphous silicon solar cells and perovskite solar cell products may be different due to different manufacturing processes, their cell spectral response curves will be somewhat different, but the spectral response wavelength range of their cells is basically mainly concentrated in 400-800nm, which will not affect the analysis of the present invention.
[0128] like Fig.13 As shown, by testing the light-converting film laminated glass provided in Example 7, it is possible to adjust the solar spectrum composition to a ratio of 3:1 between red and blue light, thereby promoting the growth of outdoor horticultural greenhouse crops.
[0129] The above descriptions are only some preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A spectrum-adjustable aluminate-based phosphor, characterized in that: The phosphor comprises a compound represented by the following formula (I): La 1-x Al 10.8-x-y Mg 0.10 Si 0.10+x O 18 :xEu 2+ ,yCr 3+ (I) In formula (I), 0≤x<0.08; 0≤y<0.2; x and y are not 0 at the same time.
2. The spectrum-adjustable aluminate-based phosphor according to claim 1, characterized in that: The purple or green light excitation peak of the phosphor is the main excitation peak; its emission peak is in the blue or far-red region, which is consistent with crop chlorophyll b, carotenoids and P fr The absorption spectra of photosensitive pigments or the high-efficiency response spectra of perovskite and amorphous silicon solar photovoltaic cells overlap.
3. The spectrum-adjustable aluminate-based phosphor according to claim 1, characterized in that: When y=0 in formula (I), the excitation wavelength of the phosphor is 250-400 nm, and the emission wavelength is 400-500 nm in the blue light region; When x=0 in formula (I), the main excitation wavelength of the phosphor is 200-300nm in the far ultraviolet region, 300-490nm in the blue-violet region, 490-600nm in the green region, and the emission wavelength is 600-900nm in the far red region; When x≠0 and y≠0 in formula (I), the main excitation wavelength of the phosphor is 200-300nm in the far ultraviolet region, 300-490nm in the blue-violet region, 490-600nm in the green region, and the emission wavelength is 400-500nm in the blue region and 600-900nm in the far red region.
4. A method for preparing a spectrum-adjustable aluminate-based phosphor according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) weighing raw materials of each element according to the atomic stoichiometric ratio of each element, uniformly mixing them, and then ball milling to obtain a solid mixture; (2) The obtained solid mixture is burned in a carbon reducing atmosphere, cooled to room temperature and then ground evenly to obtain the obtained solid mixture; the burning temperature is 1400° C. to 1600° C., and the burning time is 6 to 10 hours.
5. The method for preparing the spectrum-adjustable aluminate-based phosphor according to claim 4, characterized in that: In step (1), The raw material of Al element is aluminum hydroxide; The raw material of La element is lanthanum oxide; the raw material of Mg element is magnesium oxide; the raw material of Eu element is europium oxide; the raw material of Cr element is chromium oxide; and the raw material of Si element is silicic acid.
6. The method for preparing the spectrum-adjustable aluminate-based phosphor according to claim 4, characterized in that: The ball milling conditions in step (1) are: ball-to-material ratio of 1:1, ball milling time of 25 to 35 minutes, and speed of 180 to 200 rpm.
7. The method for preparing the spectrum-adjustable aluminate-based phosphor according to claim 4, characterized in that: The carbon reducing atmosphere in step (2) is CO or H2 atmosphere.
8. Use of the spectrum-adjustable aluminate-based phosphor according to any one of claims 1 to 3 or the spectrum-adjustable aluminate-based phosphor prepared by the preparation method according to any one of claims 4 to 7, characterized in that: The application is to use the phosphor in solar greenhouse covering materials to provide an optimal action spectrum close to crop growth to promote crop growth; or to use the phosphor in solar photovoltaic power generation to improve the photoelectric conversion efficiency of solar cells.
9. The use according to claim 8, characterized in that: The application is specifically to add the phosphor as a raw material to the preparation process of agricultural plastic greenhouse film or laminated glass or encapsulation film for solar photovoltaic power generation, so that the prepared light-converting agricultural film or light-converting film laminated glass or light-converting film for solar photovoltaic power generation has photoluminescence properties.
10. The use according to claim 9, characterized in that: The raw materials for preparing the light-converting film laminated glass include glass glue and the fluorescent powder, and the mass of the fluorescent powder is 0.1% to 1.0% of the mass of the glass glue.
Citation Information
Patent Citations
Near ultraviolet light and green light excited far-red light fluorescent powder and application method thereof
CN115353885A
Cited By
Method for rapidly detecting light conversion agent in real time
CN120161002A
A method for rapid real-time detection of light conversion agent
CN120161002B