High-precision and high-efficiency polishing method for hard and brittle ceramic material

By using nano-materials on hard and brittle ceramic materials, the photocatalytic nanopolishing liquid prepared by using nano-materials is polished under ultraviolet light, the problem of difficult balance between processing efficiency and accuracy of hard and brittle ceramic materials is solved, and high-efficiency and environmentally friendly high-precision polishing is achieved Effect, suitable for a variety of processing scenarios.

CN118905731AActive Publication Date: 2024-11-08TIANJIN UNIV

Patent Information

Application Number
CN202411248728.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-08
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

High-precision processing of existing hard and brittle ceramic materials is difficult to achieve a balance between efficiency and precision, resulting in a long production cycle and affecting the development of optoelectronic technology.

Method used

Photocatalytic nanopolishing liquid is prepared by mixing nano-abrasive particles, nanophotocatalytic particles, oxidants, nanographene oxide and deionized water. Polish hard and brittle ceramic materials under ultraviolet light, and combine photocatalytic chemical softening and nanomaterial lubrication. , achieve high-quality material removal.

Benefits of technology

It significantly improves the material removal rate and surface quality of the polishing process, reduces equipment requirements and material costs, has good sustainability and universal application, and can be used in a variety of processing scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905731A_ABST
    Figure CN118905731A_ABST
Patent Text Reader

Abstract

The invention discloses a high-precision and high-efficiency polishing method for a hard and brittle ceramic material, and belongs to the technical field of precision / ultra-precision machining. The invention aims to solve the problems that the balance between efficiency and precision is difficult to realize and the production period is long in the high-precision processing of the existing hard and brittle ceramic material. The method comprises the following steps: firstly, preparing the photocatalytic nano polishing solution, and then polishing the hard and brittle ceramic material by utilizing the photocatalytic nano polishing solution under the irradiation of ultraviolet light. The method is used for high-precision and high-efficiency polishing of the hard and brittle ceramic material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of precision / ultra-precision machining. Background Art

[0002] In recent years, with the continuous development of advanced optoelectronic technology, the requirements for precision optical components have been continuously improved, mainly reflected in the requirements of large aperture, lightweight, asphericity and excellent physical properties. A series of typical hard and brittle ceramic materials represented by silicon carbide, fused quartz and spinel are widely used in large astronomical telescopes, infrared optical systems, laser nuclear fusion devices, semiconductor industry and other defense and civilian cutting-edge technology fields due to their excellent properties such as high hardness, low thermal expansion coefficient, high temperature resistance and corrosion resistance.

[0003] Although the material properties of such hard and brittle ceramics make them popular among relevant practitioners, they have super-high hardness and strong chemical inertness, and their compression strength is much greater than their bending strength. They have significant brittleness, which makes it extremely difficult to process hard and brittle ceramics with high precision and high efficiency. Existing process technologies make it difficult to achieve a balance between efficiency and precision, that is, it is difficult to achieve excellent production efficiency while meeting the target precision requirements. This results in a production cycle of such high-precision components lasting several weeks or even months, which seriously affects the time and economic cost of the research and development of related components. At present, the manufacturing and processing technology of hard and brittle ceramic components has become one of the key factors restricting the development of optoelectronic technology. Therefore, achieving high-precision and efficient processing of hard and brittle ceramics is of great significance to the development of optoelectronic technology in my country. Summary of the invention

[0004] The present invention aims to solve the problem that the existing high-precision processing of hard and brittle ceramic materials is difficult to achieve a balance between efficiency and precision and has a long production cycle, and further provides a high-precision and high-efficiency polishing method for hard and brittle ceramic materials.

[0005] A high-precision and high-efficiency polishing method for hard and brittle ceramic materials is carried out according to the following steps:

[0006] Nano-abrasive particles, nano-photocatalytic particles, oxidants, nano-graphene oxide, dispersants and deionized water are mixed and the pH value is adjusted to obtain a photocatalytic nano-polishing liquid; under ultraviolet light, the photocatalytic nano-polishing liquid is used to polish hard and brittle ceramic materials, thereby completing a high-precision and high-efficiency polishing method for hard and brittle ceramic materials.

[0007] The beneficial effects of the present invention are:

[0008] (1) Based on abrasive removal, this method introduces photocatalytic chemical softening and nanomaterial lubrication. The synergistic effect of the three achieves high-quality removal of hard and brittle ceramic materials and achieves a balance between efficiency and precision. Compared with traditional free abrasive polishing, this method can significantly improve the material removal rate and surface quality of the polishing process.

[0009] (2) The materials used in this method are non-toxic and harmless, and are significantly sustainable and environmentally friendly.

[0010] (3) This method has low equipment requirements and only requires the introduction of an ultraviolet light source. The materials used are low in cost, so the overall cost of the method is low and the economic controllability is strong.

[0011] (4) This method can be applied to a variety of processing scenarios. It can be used for sub-aperture shaping processing as well as full-aperture flattening processing, and has significant application universality.

[0012] Instruction Manual

[0013] Figure 1 Schematic diagram of high-precision and high-efficiency polishing of hard and brittle ceramic materials of the present invention, 1 is a sub-aperture polishing disc, 2 is a polishing pad, 3 is a hard and brittle ceramic material, 4 is a clamping workbench, 5 is an ultraviolet light source, and 6 is a photocatalytic nano-polishing liquid;

[0014] Figure 2 It is a schematic diagram comparing the surface roughness and material removal rate of silicon carbide ceramic materials after high-precision polishing of Example and Comparative Examples 1 to 3;

[0015] Figure 3 Schematic diagrams of the surface morphology of silicon carbide ceramic materials after high-precision polishing of the embodiment and comparative examples 1 to 3, (a) is comparative example 1, (b) is comparative example 2, (c) is comparative example 3, and (d) is the embodiment;

[0016] Figure 4 This is a schematic diagram of the grid trajectory in step 2 of the embodiment. DETAILED DESCRIPTION

[0017] Specific implementation method 1, combined with Figure 1 Specific description: This embodiment is a high-precision and high-efficiency polishing method for hard and brittle ceramic materials, which is carried out in the following steps:

[0018] Nano-abrasive particles, nano-photocatalytic particles, oxidants, nano-graphene oxide, dispersants and deionized water are mixed and the pH value is adjusted to obtain a photocatalytic nano-polishing liquid; under ultraviolet light, the photocatalytic nano-polishing liquid is used to polish hard and brittle ceramic materials, thereby completing a high-precision and high-efficiency polishing method for hard and brittle ceramic materials.

[0019] The beneficial effects of this embodiment are:

[0020] (1) Based on abrasive removal, this method introduces photocatalytic chemical softening and nanomaterial lubrication. The synergistic effect of the three achieves high-quality removal of hard and brittle ceramic materials and achieves a balance between efficiency and precision. Compared with traditional free abrasive polishing, this method can significantly improve the material removal rate and surface quality of the polishing process.

[0021] (2) The materials used in this method are non-toxic and harmless, and are significantly sustainable and environmentally friendly.

[0022] (3) This method has low equipment requirements and only requires the introduction of an ultraviolet light source. The materials used are low in cost, so the overall cost of the method is low and the economic controllability is strong.

[0023] (4) This method can be applied to a variety of processing scenarios. It can be used for sub-aperture shaping processing as well as full-aperture flattening processing, and has significant application universality.

[0024] Specific embodiment 2: This embodiment is different from the specific embodiment 1 in that: 1% to 5% of nano-abrasive particles, 0.1% to 2% of nano-photocatalytic particles, 2% to 10% of oxidant, 0.1% to 0.5% of nano-graphene oxide, 0.1% to 0.8% of dispersant and the balance of deionized water are weighed and mixed by mass percentage, and then a pH regulator is added to a pH of 3 to 11, and finally the mixture is uniformly mixed by mechanical stirring and ultrasonic dispersion in sequence to obtain a photocatalytic nano-polishing liquid. The rest is the same as the specific embodiment 1.

[0025] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that: the average particle size of the nano-abrasive particles is 50nm to 500nm; the average particle size of the nano-photocatalytic particles is 10nm to 100nm. Other aspects are the same as specific implementation method 1 or 2.

[0026] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the nano-abrasive particles are one or a combination of diamond, silicon oxide, silicon carbide, aluminum oxide and cerium oxide. Other aspects are the same as specific embodiments 1 to 3.

[0027] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the nano photocatalytic particles are one or a combination of titanium dioxide, cerium oxide, zinc oxide and chromium oxide. The rest is the same as specific embodiments 1 to 4.

[0028] Specific embodiment 6: This embodiment is different from specific embodiments 1 to 5 in that the oxidant is one or a combination of hydrogen peroxide, potassium permanganate and potassium persulfate. Other aspects are the same as specific embodiments 1 to 5.

[0029] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the nanographene oxide sheet has a diameter of 0.2 μm to 50 μm, 1 to 2 layers, and a single layer thickness of 0.3 nm to 3 nm. Other aspects are the same as specific embodiments 1 to 6.

[0030] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that the dispersant is one or a combination of sodium polyacrylate, sodium hexametaphosphate, sodium dodecyl sulfate and sodium dodecylbenzene sulfonate. Other aspects are the same as specific embodiments 1 to 7.

[0031] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 8 in that the pH regulator is one or a combination of potassium hydroxide, phosphoric acid, ammonia water, triethanolamine and aminomethyl propanol. Others are the same as specific embodiments 1 to 8.

[0032] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: when the ultraviolet light wavelength is 300nm to 400nm and the ultraviolet light intensity is 1000mW / cm 2 ~2000mW / cm 2 Under the conditions of a sub-aperture polishing disc speed of 200rpm to 1200rpm, a pressure of 35kPa to 65kPa and a feed speed of 0.5mm / s to 1.5mm / s, the hard and brittle ceramic material is polished once or twice using a polishing pad and a photocatalytic nano-polishing liquid; under the conditions of an ultraviolet light wavelength of 300nm to 400nm and an ultraviolet light intensity of 1000mW / cm 2 ~2000mW / cm 2 , under the conditions of full-diameter polishing disc speed of 60rpm to 120rpm and pressure of 35kPa to 65kPa, polish the hard and brittle ceramic material with the polishing pad and the photocatalytic nano-polishing liquid for 10min to 20min; the supply flow rate of the photocatalytic nano-polishing liquid is 0.2L / min to 0.5L / min. The rest is the same as the specific embodiments 1 to 9.

[0033] The following examples are used to verify the beneficial effects of the present invention:

[0034] Example:

[0035] A high-precision and high-efficiency polishing method for hard and brittle ceramic materials is carried out according to the following steps:

[0036] 1. Preparation of photocatalytic nano-polishing liquid:

[0037] 1% of nano-diamond abrasive particles, 0.2% of nano-photocatalytic particles, 5% of an oxidant, 0.2% of nano-graphene oxide, 0.2% of a dispersant and the balance of deionized water are weighed and mixed according to mass percentage, and then a pH regulator is added to a pH of 3.5, and finally the mixture is uniformly mixed by mechanical stirring and ultrasonic dispersion in sequence to obtain a photocatalytic nano-polishing liquid;

[0038] 2. Silicon carbide precision polishing:

[0039] When the UV wavelength is 365nm and the UV intensity is 1000mW / cm 2 Under the conditions of sub-aperture polishing disk speed of 600rpm, pressure of 65kPa and feed speed of 1mm / s, silicon carbide was polished once with a polishing pad and photocatalytic nano-polishing liquid (polishing time was 12min), then immersed in deionized water for ultrasonic cleaning for 20min, and then gently wiped the surface of the workpiece with a dust-free cloth, and finally dried with a nitrogen flow to obtain a high-precision polished silicon carbide ceramic material.

[0040] The average particle size of the nano-diamond abrasive particles described in step 1 is 200 nm; the average particle size of the nano-photocatalytic particles described in step 1 is 60 nm.

[0041] The nano-photocatalytic particles described in step 1 are titanium dioxide.

[0042] The oxidant described in step 1 is 5% by mass of hydrogen peroxide.

[0043] The nano graphene oxide described in step 1 is industrial-grade graphene oxide, with a sheet diameter of 10 μm to 50 μm, 1 to 2 layers, and a single thickness of 1 nm to 3 nm.

[0044] The dispersant described in step one is sodium polyacrylate.

[0045] The pH regulator described in step 1 is phosphoric acid with a mass percentage of 0.35 mol / L.

[0046] The silicon carbide described in step 2 is a 60mm×60mm×2mm pressure-sintered silicon carbide ceramic sheet, and the surface roughness after rough polishing is about 100nm.

[0047] The polishing pad described in step 2 is an IC1000 composite polyurethane polishing pad; the sub-aperture polishing disk described in step 2, that is, the polishing disk size is smaller than the size of the workpiece to be polished, and the central liquid supply polishing disk specifically selected in this embodiment has a diameter of 20 mm; the photocatalytic nano-polishing liquid described in step 2 is evenly supplied to the processing area from the central liquid supply polishing disk through a peristaltic pump, and the supply flow rate is 0.3L / min.

[0048] Step 2: During the polishing process, the machine moves along a grid track and processes on an area of ​​26×26mm with a grid spacing of 1mm. Figure 4 As shown, Figure 4 This is a schematic diagram of the grid trajectory in step 2 of the embodiment;

[0049] In step 2, a 6-DOF industrial robot in the application number 201510506108.2, the invention name of which is “An over-constrained high-strength robot with tri-symmetric kinematic performance”, is used in combination with a polishing device in the application number 201710708784.7, the invention name of which is “Eccentric planetary polishing device for large-caliber non-spherical robot” to conduct a polishing experiment;

[0050] The workpiece mass before and after processing was measured using a ZA805AS precision electronic balance to calculate the material removal rate of the polishing process; the surface morphology and surface roughness after processing were measured using a white light interferometer (Bruker, ContourGT, USA). The surface roughness Sa measured in Example 1 was 10.2792 nm, and the material removal rate was 0.03564 mm 3 / min.

[0051] Comparative Example 1, polishing silicon carbide ceramics with conventional free diamond abrasives: The difference between this comparative example and the embodiment is that in step 1, 1% of nano-diamond abrasive particles, 0.2% of dispersant and the balance of deionized water are weighed and mixed by mass percentage, and then a pH regulator is added to a pH of 3.5, and finally the mixture is uniformly mixed by mechanical stirring and ultrasonic dispersion in sequence to obtain a photocatalytic nano-polishing liquid; ultraviolet light irradiation is omitted in step 2. The rest is the same as the embodiment.

[0052] The workpiece mass before and after processing was measured using a ZA805AS precision electronic balance to calculate the material removal rate of the polishing process; the surface morphology and surface roughness after processing were measured using a white light interferometer (Bruker, ContourGT, USA). The surface roughness Sa measured in Comparative Example 1 was 30.8084nm, and the material removal rate was 0.02347mm 3 / min.

[0053] Comparative Example 2, photocatalysis assisted free diamond abrasive polishing silicon carbide ceramics: The difference between this comparative example and the embodiment is that in step 1, 1% of nano diamond abrasives, 0.2% of nano photocatalytic particles, 5% of oxidant, 0.2% of dispersant and the balance of deionized water are weighed and mixed by mass percentage, and then a pH regulator is added to a pH of 3.5, and finally the mixture is uniformly mixed by mechanical stirring and ultrasonic dispersion in turn to obtain a photocatalytic nano polishing liquid. The rest is the same as the embodiment.

[0054] The workpiece mass before and after processing was measured using a ZA805AS precision electronic balance to calculate the material removal rate of the polishing process; the surface morphology and surface roughness after processing were measured using a white light interferometer (Bruker, ContourGT, USA). The surface roughness Sa measured in Comparative Example 2 was 24.8189 nm, and the material removal rate was 0.02497 mm 3 / min.

[0055] Comparative Example 3, Nano-graphene oxide assisted free diamond abrasive polishing silicon carbide ceramics: The difference between this comparative example and the embodiment is that in step 1, 1% of nano-diamond abrasives, 0.2% of nano-graphene oxide, 0.2% of dispersant and the balance of deionized water are weighed and mixed by mass percentage, and then a pH adjuster is added to a pH of 3.5, and finally the mixture is uniformly mixed by mechanical stirring and ultrasonic dispersion in turn to obtain a photocatalytic nano-polishing liquid; ultraviolet light irradiation is omitted in step 2. The rest is the same as the embodiment.

[0056] The workpiece mass before and after processing was measured using a ZA805AS precision electronic balance to calculate the material removal rate of the polishing process; the surface morphology and surface roughness after processing were measured using a white light interferometer (Bruker, ContourGT, USA). The surface roughness Sa measured in Comparative Example 3 was 22.524 nm, and the material removal rate was 0.0313 mm 3 / min.

[0057] Figure 2 It is a schematic diagram comparing the surface roughness and material removal rate of silicon carbide ceramic materials after high-precision polishing in Example and Comparative Examples 1 to 3; from the comparative analysis of the figures, it is found that the surface roughness and material removal rate obtained by using the traditional free diamond abrasive polishing method, photocatalysis-assisted free diamond abrasive polishing and nano-graphene oxide-assisted free diamond abrasive polishing are inferior to the process and polishing liquid proposed in the embodiment.

[0058] Figure 3 The figure is a schematic diagram of the surface morphology of silicon carbide ceramic materials after high-precision polishing of the embodiments and comparative examples 1 to 3, (a) is comparative example 1, (b) is comparative example 2, (c) is comparative example 3, and (d) is the embodiment. As can be seen from the figure, after polishing silicon carbide ceramics using traditional free diamond abrasives, the surface high-frequency error is large and there are a large number of surface defects, such as deep pits and grooves; the surface finish is improved by using photocatalytic assisted free diamond abrasive polishing and nano-graphene oxide assisted free diamond abrasive polishing, but there are still deep scratches and the surface quality is not ideal; and after polishing silicon carbide ceramics using the method of the embodiment, the surface is relatively smooth and finish, and the surface quality is excellent.

Claims

1. A high-precision and high-efficiency polishing method for hard and brittle ceramic materials. Features It is carried out in the following steps: Nano-abrasive particles, nano-photocatalytic particles, oxidants, nano-graphene oxide, dispersants and deionized water are mixed and the pH value is adjusted to obtain a photocatalytic nano-polishing liquid; under ultraviolet light, the photocatalytic nano-polishing liquid is used to polish hard and brittle ceramic materials, thereby completing a high-precision and high-efficiency polishing method for hard and brittle ceramic materials.

2. A high-precision and high-efficiency polishing method for hard and brittle ceramic materials according to claim 1, Features 1% to 5% of nano-abrasive particles, 0.1% to 2% of nano-photocatalytic particles, 2% to 10% of oxidant, 0.1% to 0.5% of nano-graphene oxide, 0.1% to 0.8% of dispersant and the balance of deionized water are weighed and mixed according to mass percentage, and then a pH adjuster is added to a pH value of 3 to 11, and finally the mixture is uniformly mixed by mechanical stirring and ultrasonic dispersion in sequence to obtain a photocatalytic nano-polishing liquid.

3. A high-precision and high-efficiency polishing method for hard and brittle ceramic materials according to claim 2, Features The average particle size of the nano-abrasive particles is 50nm to 500nm; the average particle size of the nano-photocatalytic particles is 10nm to 100nm.

4. A high-precision and high-efficiency polishing method for hard and brittle ceramic materials according to claim 2, Features The nano-abrasive particles are one of diamond, silicon oxide, silicon carbide, aluminum oxide and cerium oxide, or a combination of several of them.

5. A high-precision and high-efficiency polishing method for hard and brittle ceramic materials according to claim 2, Features The nanometer photocatalytic particles are one of titanium dioxide, cerium oxide, zinc oxide and chromium oxide, or a combination of several of them.

6. A high-precision and high-efficiency polishing method for hard and brittle ceramic materials according to claim 2, Features The oxidant is one of hydrogen peroxide, potassium permanganate and potassium persulfate or a combination of several of them.

7. A high-precision and high-efficiency polishing method for hard and brittle ceramic materials according to claim 2, Features The sheet diameter of the nano graphene oxide is 0.2 μm to 50 μm, the number of layers is 1 to 2, and the thickness of a single layer is 0.3 nm to 3 nm.

8. A high-precision and high-efficiency polishing method for hard and brittle ceramic materials according to claim 2, Features The dispersant is one of sodium polyacrylate, sodium hexametaphosphate, sodium dodecyl sulfate and sodium dodecylbenzene sulfonate or a combination of several of them.

9. A high-precision and high-efficiency polishing method for hard and brittle ceramic materials according to claim 2, Features The pH regulator is one of potassium hydroxide, phosphoric acid, ammonia water, triethanolamine and aminomethyl propanol or a combination of several of them.

10. A high-precision and high-efficiency polishing method for hard and brittle ceramic materials according to claim 1, Features When the wavelength of ultraviolet light is 300nm~400nm and the intensity of ultraviolet light is 1000mW / cm 2 ~2000mW / cm 2 Under the conditions of a sub-aperture polishing disc speed of 200rpm to 1200rpm, a pressure of 35kPa to 65kPa and a feed speed of 0.5mm / s to 1.5mm / s, the hard and brittle ceramic material is polished once or twice using a polishing pad and a photocatalytic nano-polishing liquid; under the conditions of an ultraviolet light wavelength of 300nm to 400nm and an ultraviolet light intensity of 1000mW / cm 2 ~2000mW / cm 2 , under the conditions of a full-aperture polishing disc speed of 60rpm to 120rpm and a pressure of 35kPa to 65kPa, the hard and brittle ceramic material is polished for 10min to 20min using a polishing pad and a photocatalytic nano-polishing liquid; the supply flow rate of the photocatalytic nano-polishing liquid is 0.2L / min to 0.5L / min.

Citation Information

Patent Citations

  • Polishing solution, polishing machine and polishing method

    CN105773399A

  • Polishing solution for semiconductor material and preparation method thereof

    CN115851137A

  • Ultra-thin laser crystal chemical mechanical polishing solution based on light field coupling and preparation and polishing methods of ultra-thin laser crystal chemical mechanical polishing solution

    CN116463061A

  • Preparation and polishing method of ultraviolet light catalysis assisted chemical mechanical polishing solution suitable for gallium nitride

    CN116589927A

  • Silicon carbide polishing device and process

    CN117464549A

Cited By

  • Semiconductor material polishing method based on photo-thermal coupling catalysis and application

    CN119734186A

  • A semiconductor material polishing method based on photothermal coupling catalysis and its application

    CN119734186B

  • Monocrystal diamond polishing solution for polishing high-thermal-conductivity aluminum nitride ceramic substrate

    CN122357006A

  • Gel abrasive tool based on photocatalysis-mechanical synergistic mechanism and polishing method

    CN122807773A