High-performance polyurethane sealant and preparation method thereof
By adding Ni-modified ZIF-8 composite material loaded with MoS2 and iron oxide loaded with Ti3C2Tx to the polyurethane sealant, the problems of degraded bonding performance and insufficient flame retardant performance are solved, and high-performance sealant is realized. Preparation, suitable for a variety of industrial applications.
Patent Information
- Application Number
- CN202411191113.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During use, existing polyurethane sealants have problems such as deteriorating bonding performance and poor flame retardant performance, which cannot meet actual production needs.
High-performance polyurethane sealant was prepared by adding Ni-modified ZIF-8 composite material supported by MoS2 and Ti3C2Tx-loaded iron oxide combined with isocyanate, polyether polyol, plasticizer and silane coupling agent to improve its flame retardant Performance and mechanical properties.
It significantly improves the flame retardant and mechanical properties of the sealant, has excellent comprehensive performance, and is suitable for a variety of industrial applications.
Smart Images

Figure BDA0005015128020000081
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sealants, and more specifically, relates to a high-performance polyurethane sealant and a preparation method thereof. Background Art
[0002] Polyurethane sealants have good properties: (1) excellent wear resistance; (2) low temperature flexibility; (3) wide adjustable performance range; (4) high mechanical strength; (5) good adhesion; (6) good elasticity, excellent recovery, suitable for dynamic joints; (7) good weather resistance, service life can be up to 15 to 20 years; (8) excellent oil resistance; (9) resistance to biological aging. Polyurethane sealants are widely used in civil construction, transportation, electronics, medical equipment, aviation, etc. due to the above advantages. However, the operating temperature range of the existing general polyurethane sealants in China is between -40 and 80°C, and the cured products of this type of general polyurethane sealants often have plasticizer exudation around the bonding area as the use time increases, which reduces the physical properties and bonding properties of the sealant, and the flame retardant properties are poor, which cannot meet the needs of actual production.
[0003] CN117431032A discloses a foamed polyurethane sealant composition for batteries and a preparation method thereof, belonging to the technical field of polymer polyurethane materials. The technical scheme is as follows: the composition is composed of a mixture of component A and component B; the preparation method is as follows: (1) Component A: polyether polyol, flame retardant polyether polyol, polyester ether, crosslinking agent polyether, chain extender, flame retardant, foaming agent, foam stabilizer and composite catalyst are put into a reactor, the temperature is controlled, and component A is obtained by stirring; (2) Component B: bio-based polyether polyol is put into a reactor, the temperature is increased for vacuum dehydration, the temperature is decreased, liquefied MDI is added, the temperature is increased for reaction, sampling and detection are performed, the temperature is decreased for discharge, and the material is sealed for storage; (3) Component A and component B are mixed uniformly according to a proportion, injected into a mold, the mold is closed, and the mold is opened to obtain a foamed polyurethane sealant for batteries. The battery sealant product prepared by the composition of the present invention is light in weight, and has excellent mechanical properties, hydrolysis resistance and hydrophobic properties.
[0004] CN117363298A discloses a halogen-free flame-retardant functional polyurethane sealant and its preparation process. The polyurethane sealant is prepared by mixing polyurethane prepolymer, flame-retardant modifier, inorganic filler, chain extender ethylene glycol, ultraviolet absorber and plasticizer as raw materials at high temperature, wherein the polyurethane prepolymer is prepared by using polyethylene glycol derivative containing rigid heterocycle in the structure as soft segment polymer and isocyanate monomer as hard segment, and the flame-retardant modifier is a POSS derivative grafted with phosphorus-containing flame retardant in the structure. By introducing rigid heterocycle and POSS derivative into the polyurethane structure, the prepared polyurethane sealant can have good heat resistance, flame retardant property and bonding property, which is beneficial to its further development and application in the field of construction industry.
[0005] CN115074073A discloses a flame retardant polyurethane sealant and a preparation method thereof, belonging to the technical field of sealants. The sealant comprises a first component and a second component, and the preparation method comprises the following steps: adding the second component to the first component at a temperature of 70°C, stirring for 1-1.5h, then adding a catalyst, sampling and testing the remaining NCO content every 30min, stopping the reaction when the NCO content is less than 2.5%, discharging the material when the temperature drops to 50°C, pouring it into a mold for curing, and obtaining a polyurethane sealant. In the present invention, epoxy soybean oil is used as a raw material to prepare bio-based polyols, improve the flame retardant properties of bio-based polyols, and the flame retardant elements are linked by chemical bonds, which are not easy to migrate out, thereby improving the flame retardant durability; using bio-based raw materials to synthesize bio-based polyols not only saves energy but also improves the environment.
[0006] CN114250055A discloses a single-component halogen-free flame-retardant silane-modified polyurethane sealant and a preparation method thereof, and relates to the technical field of flame-retardant sealants. The sealant is composed of the following raw materials: a flame-retardant silane-modified polyurethane polymer, a flame-retardant plasticizer, a flame-retardant reinforcing powder, a reinforcing powder material, a dehydrating agent, etc. The single-component halogen-free flame-retardant silane-modified polyurethane sealant of the invention adopts a flame-retardant polyether polyol to synthesize a flame-retardant silane-modified polyurethane polymer, and then adds a flame-retardant plasticizer, a flame-retardant powder filler, a reinforcing powder material, a dehydrating agent, an adhesion promoter, an ultraviolet absorber, an antioxidant, a catalyst and other materials for kneading to prepare the single-component halogen-free flame-retardant silane-modified polyurethane sealant; the single-component halogen-free flame-retardant silane-modified polyurethane sealant prepared by the invention has good flame retardancy, safety and environmental protection, and good mechanical properties.
[0007] In summary, the flame retardant properties and mechanical properties of polyurethane sealants can be improved by adding materials with flame retardant properties. The present invention provides a high-performance polyurethane sealant and a preparation method thereof, which have excellent flame retardant properties and mechanical properties. Summary of the invention
[0008] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art and provide a high-performance polyurethane sealant and a preparation method thereof. The present invention comprises the following components by weight: 30 to 50 parts of isocyanate; 40 to 60 parts of polyether polyol; 8 to 16 parts of MoS2-loaded Ni-modified ZIF-8 composite material; Ti3C2T x 6 to 10 parts of loaded iron oxide; 20 to 40 parts of plasticizer; 1 to 3 parts of dibutyltin dilaurate; and 3 to 7 parts of silane coupling agent. xThe loaded iron oxide utilizes the interaction between the two to improve the flame retardant and mechanical properties of the polyurethane sealant, and the comprehensive performance is excellent.
[0009] The purpose of the present invention is to provide a high-performance polyurethane sealant.
[0010] Another object of the present invention is to provide a method for preparing a high-performance polyurethane sealant.
[0011] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0012] A high-performance polyurethane sealant, comprising the following components in parts by weight:
[0013] 30-50 parts of isocyanate;
[0014] 40-60 parts of polyether polyol;
[0015] 8 to 16 parts of MoS2-supported Ni-modified ZIF-8 composite material;
[0016] Ti3C2T x 6 to 10 parts of loaded iron oxide;
[0017] 20-40 parts of plasticizer;
[0018] 1-3 parts of dibutyltin dilaurate;
[0019] Silane coupling agent 3 to 7 parts.
[0020] In a preferred embodiment, the isocyanate is hexamethylene diisocyanate, isophorone diisocyanate or cyclohexyl diisocyanate; the polyether polyol is polyether polyol 635, polyether polyol 450 or polyether polyol 4110; the plasticizer is phthalate; and the silane coupling agent is aminopropyltrimethoxysilane, aminopropyltriethoxysilane or aminoethylaminopropyltrimethoxysilane.
[0021] In the present invention, a preferred embodiment, the method for preparing the MoS2-supported Ni-modified ZIF-8 composite material comprises the following steps:
[0022] (1) weighing a molybdenum source and a sulfur source, ultrasonically dispersing them in deionized water, and then transferring them to a hydrothermal reactor, reacting them at 160-200° C. for 16-24 hours; cooling them to room temperature, washing them, and vacuum drying them at 60-80° C. for 10-14 hours to obtain MoS2;
[0023] (2) Ultrasonic dispersion of the MoS2 obtained in step (1) in ethanol, and then adding nickel salt, zinc salt and dimethylimidazole, stirring for 20 to 40 minutes; then hydrothermally reacting at 130 to 150° C. for 4 to 8 hours, filtering, washing, and drying at 80 to 120° C. for 10 to 20 hours to obtain a MoS2-loaded Ni-modified ZIF-8 composite material.
[0024] Preferably, in step (1), the sulfur source is thioacetamide; the molybdenum source is ammonium molybdate; and the molar ratio of the molybdenum source to the sulfur source is 1:3-5.
[0025] Further preferably, in step (2), the nickel salt is at least one of nickel nitrate, nickel chloride, and nickel acetate; the zinc salt is at least one of zinc nitrate, zinc chloride, and zinc acetate; the ratio of MoS2 to zinc salt is 100g:10-30mmol; and the molar ratio of the nickel salt, zinc salt, and dimethylimidazole is 0.01-0.03:1:2-4.
[0026] In the present invention, the preferred solution is that the Ti3C2T x The preparation method of the supported iron oxide is as follows:
[0027] (I) Etching the Ti3AlC2 precursor with a concentrated HF solution to obtain Ti3C2T x Dispersion, separation, washing, drying to Ti3C2T x
[0028] (II) ultrasonically dispersing a certain amount of iron salt into deionized water, and then x Add to the above mixed solution, stir evenly, adjust pH to 9-11, perform hydrothermal reaction, filter, wash and dry to obtain Ti3C2T x Loaded iron oxide.
[0029] Preferably, in step (I), the drying is performed at 90-110° C. for 12-16 hours.
[0030] Further preferably, in step (II), the hydrothermal reaction temperature is 160-240° C., and the reaction time is 14-20 h; and the drying is performed at 90-110° C. for 12-16 h.
[0031] More preferably, in step (II), the iron salt is at least one of ferric nitrate, ferric chloride and ferric acetate, and the Ti3C2T x The ratio to iron salt is 100g:10~30mmol.
[0032] Based on the above-mentioned method for preparing a high-performance polyurethane sealant, the preparation method comprises the following steps:
[0033] Add polyether polyol, plasticizer and isocyanate into the reactor, stir evenly, add half of the catalyst under nitrogen protection, continue stirring, control the reaction temperature at 70-90°C, react for 1-3 hours to obtain a polyurethane prepolymer; then add MoS2-loaded Ni-modified ZIF-8 composite material, Ti3C2T x The loaded iron oxide and silane coupling agent are stirred at a speed of 400 to 600 rpm for 20 to 40 minutes, and then the remaining catalyst is added and stirred for another 20 to 40 minutes to obtain a high-performance polyurethane sealant.
[0034] The present invention has the following beneficial effects:
[0035] In the preparation process of the present invention, adding MoS2-loaded Ni-modified ZIF-8 composite material is beneficial to promoting the carbonization ability of the collective material, which can improve the suppression of smoke release, and the above-mentioned material itself can also improve the mechanical properties of the sealant. At the same time, with Ti3C2T x The loaded iron oxide further improves the flame retardant and mechanical properties of the sealant, with excellent comprehensive performance and good application prospects. DETAILED DESCRIPTION
[0036] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0037] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0038] Example 1
[0039] A high-performance polyurethane sealant, comprising the following components in parts by weight:
[0040] 40 parts of isocyanate; the isocyanate is isophorone diisocyanate;
[0041] 50 parts of polyether polyol; the polyether polyol is polyether polyol 450;
[0042] MoS2-loaded Ni-modified ZIF-8 composite material 12 parts;
[0043] Ti3C2T x 8 parts of loaded iron oxide;
[0044] 30 parts of plasticizer; the plasticizer is phthalate;
[0045] 2 parts of dibutyltin dilaurate;
[0046] 5 parts of silane coupling agent; the silane coupling agent is aminopropyltriethoxysilane;
[0047] The preparation method of the MoS2-loaded Ni-modified ZIF-8 composite material comprises the following steps:
[0048] (1) Weigh 1 mol of ammonium molybdate and 4 mol of thioacetamide and ultrasonically disperse them in 200 mL of deionized water, then transfer them to a hydrothermal reactor and react at 180° C. for 20 h; cool to room temperature, wash, and vacuum dry at 70° C. for 12 h to obtain MoS2;
[0049] (2) 100 g of MoS2 obtained in step (1) was ultrasonically dispersed in 300 mL of ethanol, and then 0.4 mmol of nickel nitrate, 20 mmol of zinc chloride and 60 mmol of dimethylimidazole were added and stirred for 30 min; then hydrothermally reacted at 140 °C for 6 h, filtered, washed, and dried at 100 °C for 16 h to obtain a MoS2-loaded Ni-modified ZIF-8 composite material.
[0050] The Ti3C2T x The preparation method of the supported iron oxide is as follows:
[0051] (I) Weigh 10 g Ti3AlC2 and add it to 100 mL 40 wt% HF solution, stir for 20 h, filter, wash, and dry at 100 °C for 14 h to obtain Ti3C2T x ;
[0052] (II) 20 mmol of ferric nitrate was ultrasonically dispersed in 300 mL of deionized water, and then 100 g of the Ti3C2T x Add to the above mixed solution, stir evenly, adjust pH to 10 with 2 mol / L sodium hydroxide solution, hydrothermally react at 200 °C for 18 h, filter, wash, and dry at 100 °C for 14 h to obtain Ti3C2T x Loaded iron oxide.
[0053] A method for preparing a high-performance polyurethane sealant comprises the following steps:
[0054] Add polyether polyol, plasticizer and isocyanate into the reactor and stir evenly. Under nitrogen protection, add half of the catalyst and continue stirring. Control the reaction temperature at 80°C and react for 2 hours to obtain a polyurethane prepolymer. Then add MoS2-loaded Ni-modified ZIF-8 composite material, Ti3C2T x The loaded iron oxide and silane coupling agent were stirred at 500 rpm for 30 min, and then the remaining catalyst was added and stirred for another 30 min to obtain a high-performance polyurethane sealant.
[0055] Example 2
[0056] A high-performance polyurethane sealant, comprising the following components in parts by weight:
[0057] 50 parts of isocyanate; the isocyanate is cyclohexyl diisocyanate;
[0058] 40 parts of polyether polyol; the polyether polyol is polyether polyol 635;
[0059] 16 parts of MoS2-supported Ni-modified ZIF-8 composites;
[0060] Ti3C2T x 6 parts of loaded iron oxide;
[0061] 40 parts of plasticizer; the plasticizer is phthalate;
[0062] 3 parts of dibutyltin dilaurate;
[0063] 7 parts of silane coupling agent; the silane coupling agent is aminoethylaminopropyltrimethoxysilane;
[0064] The preparation method of the MoS2-loaded Ni-modified ZIF-8 composite material comprises the following steps:
[0065] (1) Weigh 1 mol of ammonium molybdate and 5 mol of thioacetamide and ultrasonically disperse them in 200 mL of deionized water, then transfer them to a hydrothermal reactor, react at 200 ° C for 16 h, cool to room temperature, wash, and vacuum dry at 80 ° C for 10 h to obtain MoS2;
[0066] (2) 100 g of MoS2 obtained in step (1) was ultrasonically dispersed in 300 mL of ethanol, and then 0.9 mmol of nickel chloride, 30 mmol of zinc acetate and 120 mmol of dimethylimidazole were added and stirred for 40 min; then hydrothermally reacted at 150 ° C for 4 h, filtered, washed, and dried at 120 ° C for 10 h to obtain a MoS2-loaded Ni-modified ZIF-8 composite material.
[0067] The Ti3C2T x The preparation method of the supported iron oxide is as follows:
[0068] (I) Weigh 10 g Ti3AlC2 and add it to 100 mL 40 wt% HF solution, stir for 20 h, filter, wash, and dry at 100 °C for 14 h to obtain Ti3C2T x ;
[0069] (II) 30 mmol of ferric chloride was ultrasonically dispersed in 300 mL of deionized water, and then 100 g of the Ti3C2Tx Add to the above mixed solution, stir evenly, adjust pH to 11 with 2 mol / L sodium hydroxide solution, hydrothermally react at 240 °C for 14 h, filter, wash, and dry at 110 °C for 12 h to obtain Ti3C2T x Loaded iron oxide.
[0070] A method for preparing a high-performance polyurethane sealant comprises the following steps:
[0071] Add polyether polyol, plasticizer and isocyanate into the reactor and stir evenly. Under nitrogen protection, add half of the catalyst and continue stirring. Control the reaction temperature at 90°C and react for 1 hour to obtain a polyurethane prepolymer. Then add MoS2-loaded Ni-modified ZIF-8 composite material, Ti3C2T x The loaded iron oxide and silane coupling agent were stirred at 600 rpm for 20 min, and then the remaining catalyst was added and stirred for another 20 min to obtain a high-performance polyurethane sealant.
[0072] Example 3
[0073] A high-performance polyurethane sealant, comprising the following components in parts by weight:
[0074] 30 parts of isocyanate; the isocyanate is hexamethylene diisocyanate;
[0075] 60 parts of polyether polyol; the polyether polyol is polyether polyol 4110;
[0076] 8 parts of MoS2-supported Ni-modified ZIF-8 composites;
[0077] Ti3C2T x 10 parts of loaded iron oxide;
[0078] 20 parts of plasticizer; the plasticizer is phthalate;
[0079] 1 part of dibutyltin dilaurate;
[0080] 3 parts of silane coupling agent; the silane coupling agent is aminopropyltrimethoxysilane;
[0081] The preparation method of the MoS2-loaded Ni-modified ZIF-8 composite material comprises the following steps:
[0082] (1) Weigh 1 mol of ammonium molybdate and 3 mol of thioacetamide and ultrasonically disperse them in 200 mL of deionized water, then transfer them to a hydrothermal reactor and react at 160° C. for 24 h; cool to room temperature, wash, and vacuum dry at 60° C. for 14 h to obtain MoS2;
[0083] (2) 100 g of MoS2 obtained in step (1) was ultrasonically dispersed in 300 mL of ethanol, and then 0.1 mmol of nickel acetate, 10 mmol of zinc nitrate and 20 mmol of dimethylimidazole were added and stirred for 20 min; then hydrothermally reacted at 130 °C for 8 h, filtered, washed, and dried at 80 °C for 20 h to obtain a MoS2-loaded Ni-modified ZIF-8 composite material.
[0084] The Ti3C2T x The preparation method of the supported iron oxide is as follows:
[0085] (I) Weigh 10 g Ti3AlC2 and add it to 100 mL 40 wt% HF solution, stir for 20 h, filter, wash, and dry at 100 °C for 14 h to obtain Ti3C2T x ;
[0086] (II) 10 mmol of ferric acetate was ultrasonically dispersed in 300 mL of deionized water, and then 100 g of the Ti3C2T x Add to the above mixed solution, stir evenly, adjust pH to 9 with 2 mol / L sodium hydroxide solution, hydrothermally react at 160 °C for 20 h, filter, wash, and dry at 90 °C for 16 h to obtain Ti3C2T x Loaded iron oxide.
[0087] A method for preparing a high-performance polyurethane sealant comprises the following steps:
[0088] Add polyether polyol, plasticizer and isocyanate into the reactor and stir evenly. Under nitrogen protection, add half of the catalyst and continue stirring. Control the reaction temperature at 70 °C and react for 3 hours to obtain a polyurethane prepolymer. Then add MoS2-loaded Ni-modified ZIF-8 composite material, Ti3C2T x The loaded iron oxide and silane coupling agent were stirred at 400 rpm for 40 min, and then the remaining catalyst was added and stirred for another 40 min to obtain a high-performance polyurethane sealant.
[0089] Comparative Example 1
[0090] The difference between Control Example 1 and Example 1 is that an equal amount of MoS2-loaded ZIF-8 composite material is used to replace the MoS2-loaded Ni-modified ZIF-8 composite material. The preparation method of the MoS2-loaded ZIF-8 composite material is as follows:
[0091] (1) Weigh 1 mol of ammonium molybdate and 4 mol of thioacetamide and ultrasonically disperse them in 200 mL of deionized water, then transfer them to a hydrothermal reactor and react at 180° C. for 20 h; cool to room temperature, wash, and vacuum dry at 70° C. for 12 h to obtain MoS2;
[0092] (2) 100 g of MoS2 obtained in step (1) was ultrasonically dispersed in 300 mL of ethanol, and then 20.4 mmol of zinc chloride and 60 mmol of dimethylimidazole were added and stirred for 30 min; then hydrothermally reacted at 140 °C for 6 h, filtered, washed, and dried at 100 °C for 16 h to obtain a MoS2-loaded ZIF-8 composite material.
[0093] Comparative Example 2
[0094] The difference between Control Example 2 and Example 1 is that an equal amount of MoS2 is used to replace the Ni-modified ZIF-8 composite material loaded with MoS2, wherein the preparation method of MoS2 is as follows:
[0095] Weigh 1 mol of ammonium molybdate and 4 mol of thioacetamide, ultrasonically disperse them in 200 mL of deionized water, and then transfer them to a hydrothermal reactor and react at 180°C for 20 h; cool to room temperature, wash, and vacuum dry at 70°C for 12 h to obtain MoS2.
[0096] Comparative Example 3
[0097] The difference between Comparative Example 3 and Example 1 is that: Ti3C2T x Unloaded iron oxide.
[0098] Comparative Example 4
[0099] The difference between the comparative example 4 and the example 1 is that it does not contain Ti3C2T x The loaded iron oxide, wherein the MoS2 loaded Ni modified ZIF-8 composite material is 20 parts.
[0100] The performance of Examples 1-3 and Comparative Examples 1-4 was tested, and the specific test results are shown in Table 1. Among them,
[0101] Peel strength: GB / T 532-2008;
[0102] Limiting oxygen index: GB / T 2406.2-2009.
[0103] Table 1:
[0104]
[0105] It can be seen from Table 1 that the high-performance polyurethane sealant prepared by the present invention has excellent mechanical properties and flame retardant properties, wherein the peel strength can reach up to 8.2 kN / m; the limiting oxygen index can reach up to 39.1, with excellent performance, broad application prospects and good market prospects.
[0106] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A high performance polyurethane sealant, characterized in that: By weight, it includes the following components: 30-50 parts of isocyanate; 40-60 parts of polyether polyol; 8 to 16 parts of MoS2-supported Ni-modified ZIF-8 composite material; Ti3C2T x 6-10 parts of loaded iron oxide; 20-40 parts of plasticizer; 1-3 parts of dibutyltin dilaurate; Silane coupling agent 3 to 7 parts.
2. A high performance polyurethane sealant according to claim 1, characterized in that: The isocyanate is hexamethylene diisocyanate, isophorone diisocyanate or cyclohexyl diisocyanate; the polyether polyol is polyether polyol 635, polyether polyol 450 or polyether polyol 4110; the plasticizer is phthalate; and the silane coupling agent is aminopropyl trimethoxy silane, aminopropyl triethoxy silane or aminoethylaminopropyl trimethoxy silane.
3. A high performance polyurethane sealant according to claim 1, characterized in that: The preparation method of the MoS2-loaded Ni-modified ZIF-8 composite material comprises the following steps: (1) weighing a molybdenum source and a sulfur source, ultrasonically dispersing them in deionized water, and then transferring them to a hydrothermal reactor, reacting them at 160-200° C. for 16-24 hours; cooling them to room temperature, washing them, and vacuum drying them at 60-80° C. for 10-14 hours to obtain MoS2; (2) Ultrasonic dispersion of the MoS2 obtained in step (1) in ethanol, and then adding nickel salt, zinc salt and dimethylimidazole, stirring for 20 to 40 minutes; then hydrothermally reacting at 130 to 150° C. for 4 to 8 hours, filtering, washing, and drying at 80 to 120° C. for 10 to 20 hours to obtain a MoS2-loaded Ni-modified ZIF-8 composite material.
4. A high performance polyurethane sealant according to claim 3, characterized in that: In step (1), the sulfur source is thioacetamide; the molybdenum source is ammonium molybdate; and the molar ratio of the molybdenum source to the sulfur source is 1:3-5.
5. A high performance polyurethane sealant according to claim 3, characterized in that: In step (2), the nickel salt is at least one of nickel nitrate, nickel chloride, and nickel acetate; the zinc salt is at least one of zinc nitrate, zinc chloride, and zinc acetate; the ratio of MoS2 to zinc salt is 100g:10-30mmol; the molar ratio of the nickel salt, zinc salt, and dimethylimidazole is 0.01-0.03:1:2-4.
6. A high performance polyurethane sealant according to claim 1, characterized in that: The Ti3C2T x The preparation method of the supported iron oxide is as follows: (I) Etching the Ti3AlC2 precursor with a concentrated HF solution to obtain Ti3C2T x Dispersion, separation, washing, drying to Ti3C2T x (II) ultrasonically dispersing a certain amount of iron salt into deionized water, and then x Add to the above mixed solution, stir evenly, adjust pH to 9-11, perform hydrothermal reaction, filter, wash and dry to obtain Ti3C2T x Loaded iron oxide.
7. A high performance polyurethane sealant according to claim 6, characterized in that: In step (I), the drying is performed at 90-110° C. for 12-16 hours.
8. A high performance polyurethane sealant according to claim 6, characterized in that: In step (II), the hydrothermal reaction temperature is 160-240° C., and the reaction time is 14-20 h; and the drying is performed at 90-110° C. for 12-16 h.
9. A high performance polyurethane sealant according to claim 6, characterized in that: In step (II), the iron salt is at least one of ferric nitrate, ferric chloride and ferric acetate, and the Ti3C2T x The ratio to iron salt is 100g:10~30mmol.
10. A method for preparing a high-performance polyurethane sealant according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: Add polyether polyol, plasticizer and isocyanate into the reactor, stir evenly, add half of the catalyst under nitrogen protection, continue stirring, control the reaction temperature at 70-90°C, react for 1-3 hours to obtain a polyurethane prepolymer; then add MoS2-loaded Ni-modified ZIF-8 composite material, Ti3C2T x The loaded iron oxide and silane coupling agent are stirred at a speed of 400 to 600 rpm for 20 to 40 minutes, and then the remaining catalyst is added and stirred for another 20 to 40 minutes to obtain a high-performance polyurethane sealant.
Citation Information
Patent Citations
Expandable graphite modified flame retardant polyurethane sealant and preparation method thereof
CN108359403A
Fast-cure polyurethane waterproof sealant and method for preparing same
CN108410412A
Environment-friendly efficient flame-retardant cable material and preparation method thereof
CN115558282A
Flame-retardant sealant as well as preparation method and application thereof
CN115975590A
Cited By
Waterborne polyurethane emulsion as well as preparation method and application thereof
CN121537603A
A waterborne polyurethane emulsion, a preparation method and application thereof
CN121537603B