Recovery method of nickel cobalt lithium manganate positive plate

Through the immersion and electrochemical adsorption technology of organic acids and hydrogen peroxide under acidic conditions, the problem of binding agent dissolution and extraction agent difficult to recycle in the positive electrode active material recovery of lithium-ion batteries is solved, and efficient separation of nickel, cobalt and manganese is achieved. Lossless recycling of the cathode current collector improves recycling efficiency and cost-effectiveness.

CN118943545APending Publication Date: 2024-11-12DONGGUAN CHAM BATTERY TECH CO LTD

Patent Information

Application Number
CN202410927493.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing technology for recycling positive electrode active materials of lithium-ion batteries, the liquid formed after the binder is dissolved is viscous and the particle size of the positive electrode active material is small, which leads to slow filtration speed and difficult to completely separate, and common extractants are difficult to recycle, which increases costs.

Method used

Immerse the positive electrode sheet under acidic conditions by using organic acid solution and hydrogen peroxide to destroy the structure of the binder and promote the separation of the electrode material and current collector. Combined with electrochemical adsorption technology, no need for crushing and extraction agents, achieving efficient separation of nickel, cobalt and manganese .

Benefits of technology

Lossless recovery of the positive electrode current collector is achieved, pulverizing and using extracting agents is avoided, the recovery efficiency and purification effect of nickel-cobalt-manganese are improved, and the treatment cost is reduced.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a recovery method of a nickel cobalt lithium manganate positive plate. The recovery method comprises the following steps: drying the nickel cobalt lithium manganate positive plate disassembled from a battery to remove electrolyte on the surface of the nickel cobalt lithium manganate positive plate; soaking in an organic acid solution for a certain time, adding hydrogen peroxide, and continuously soaking until the positive electrode powder is separated from the current collector; recycling the collected fluid to obtain a leaching solution containing the positive electrode powder; and performing electrochemical adsorption on the leachate to separate nickel ions, cobalt ions and manganese ions. According to the recovery method, the addition of an extracting agent is avoided, the recovery of nickel-cobalt-manganese valuable metals can be effectively realized, the positive electrode current collector does not need to be crushed in the whole process, scraps are not generated, and the lossless recovery of the whole positive electrode current collector can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of recycling and utilization of lithium-ion batteries, in particular to the recycling of positive electrode materials, and more particularly to a method for recycling positive electrode sheets of nickel-cobalt-manganese-lithium series. Background Art

[0002] With the rapid industrialization of new energy vehicles, their sales will soar, and the number of lithium-ion power batteries will also increase exponentially. At the same time, the environmental pollution problem and the reasonable resource recycling of waste lithium-ion power batteries have become a common concern in the industry and a problem that needs to be solved urgently. Solving this problem is not only conducive to environmental protection, but also conducive to the recycling of resources, and has great practical significance.

[0003] At present, the main materials recovered from waste lithium-ion batteries are negative electrode current collectors (commonly copper foil), positive electrode current collectors (commonly aluminum foil), positive electrode active materials and negative electrode active materials. There are usually three main steps in the recycling of pole pieces: first, discharging the waste batteries and disassembling the pole pieces; second, separating the materials in the pole pieces from the current collectors; and third, recovering and utilizing the valuable metals. Among them, the positive electrode active material, the positive electrode conductive agent, and the positive electrode binder are made into a positive electrode slurry, and then the positive electrode slurry is coated on the aluminum foil, and the positive electrode sheet is obtained after drying. Since the positive electrode active material and the conductive agent are tightly bonded and adhered to the positive electrode current collector by the binder, the prior art often uses a solvent to disperse the positive electrode active material, the conductive agent and the binder in the solvent (where the binder can be dissolved in the solvent, while the positive electrode active material and the conductive carbon black are insoluble), and then further separate the positive electrode active material and the binder, and then extract and separate the valuable metals. However, since the liquid formed after the binder is dissolved by the solvent is very viscous, and the positive electrode active material is a fine powder with a small particle size, when using the existing conventional filtration method to separate them, not only is the filtration speed slow, but the filtrate obtained after filtration still contains a large amount of positive electrode active material, thus limiting the application of the method of solvent separation of positive electrode current collector and positive electrode active material.

[0004] Although the industry also uses physical methods, that is, mechanical crushing and ultrasonic-assisted separation to assist in the separation of positive electrode active materials. However, this auxiliary method will cause the positive electrode collector (copper foil) to be crushed and destroyed while recovering the positive electrode active materials, resulting in debris, making subsequent separation and material purification and recovery difficult. In addition, extraction is also used instead of filtration, and valuable metal ions such as nickel, cobalt, and manganese in the positive electrode sheet are extracted with an extractant to achieve enrichment and separation. However, the extractant is difficult to recycle, which increases the cost of use.

[0005] Therefore, there is an urgent need for a recyclable and efficient separation method to solve the above problems. Summary of the invention

[0006] Based on the above problems, the object of the present invention is to provide a method for recycling lithium nickel cobalt manganese oxide cathode sheets. This recycling method avoids the addition of extractants, can not only effectively realize the recycling of valuable metals such as nickel, cobalt, and manganese, but also does not require crushing the cathode current collector throughout the process, does not generate debris, and can realize the lossless recycling of the entire cathode current collector sheet.

[0007] To achieve the above object, the present invention provides a method for recycling lithium nickel cobalt manganese oxide cathode sheets. The cathode active material in the lithium nickel cobalt manganese oxide cathode sheet at least includes LiNi x Co y Mn z M (1-x-y-z) O 2 , where M is at least one of Mg, Cu, Zn, Al, Sn, B, Ga, Cr, Sr, V, and Ti, 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z ≤ 1. The method for recycling lithium nickel cobalt manganese oxide cathode sheets includes:

[0008] (1) Drying the lithium nickel cobalt manganese oxide cathode sheet disassembled from the battery to remove the electrolyte on the surface;

[0009] (2) Soaking in an organic acid solution for a certain time and then adding hydrogen peroxide and continuously soaking until the cathode powder detaches from the current collector;

[0010] (3) Recycling the current collector to obtain a leaching solution containing the cathode powder;

[0011] (4) Electrochemically adsorbing the leaching solution to separate nickel ions, cobalt ions, and manganese ions.

[0012] In the technical solution adopted by the present invention, the cathode sheet is first soaked in an organic acid solution. The H + of the organic acid solution reacts with the oxide layer on the surface of the cathode current collector, which can destroy the contact interface between the diaphragm (formed by coating a slurry of cathode active material, conductive agent, and binder and drying) and the cathode current collector in the cathode sheet, causing the diaphragm to detach from the surface of the cathode current collector and realizing the separation of the electrode material and the current collector. On this basis, adding hydrogen peroxide and continuously soaking, under acidic conditions, hydrogen peroxide will undergo a self-dissociation reaction to generate hydrogen ions (H + ), peroxy radicals (·O 2-) and hydroxyl radicals (·OH), the strong oxidizing properties of such active oxidizing groups can achieve oxidative degradation of some organic matter, such as the binder PVDF, or destroy its structure, reducing its bonding properties, thereby further promoting the separation of the membrane and the positive electrode collector. In the above process, no crushing process is used, and an organic weak acid is used, which has no effect on the surface of the positive electrode collector, and the whole positive electrode collector can be recovered without loss. The lossless recovery of the whole positive electrode collector is conducive to the testing and analysis of the composition, surface density, and various indicators of the battery electrode powder, and is of great significance to the industry's competitive product analysis and the analysis of the components of the positive and negative electrode materials of buckle batteries. In addition, compared with strong inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, organic acids tend to be mild in acidity, and their subsequent treatment is simpler and the treatment cost is lower.

[0013] In addition, after the positive electrode current collector is recovered, the membrane is dissolved in the solution to obtain a leachate containing positive electrode powder, and the leachate is treated by electrochemical adsorption to separate nickel ions, cobalt ions and manganese ions. The electrochemical adsorption method is simple and avoids the addition of an extractant. Through the alternating operation of electrochemical positive and negative charges, the adsorption and regeneration of the electrode plate can be achieved, which has the advantage of being recyclable and usable multiple times.

[0014] As a technical solution of the present invention, the nickel cobalt manganese oxide lithium positive electrode sheet includes a positive electrode active material, a binder and a conductive agent.

[0015] As a technical solution of the present invention, the binder includes PVDF.

[0016] As a technical solution of the present invention, the conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.

[0017] As a technical solution of the present invention, the drying temperature is 50° C. to 60° C., and the drying time is 8 h to 12 h.

[0018] As a technical solution of the present invention, the organic acid solution is an aqueous solution of organic acid with a mass concentration of 8% to 10%, and the organic acid includes at least one of tartaric acid, oxalic acid, malic acid, citric acid, acetic acid, ascorbic acid and benzoic acid.

[0019] As a technical solution of the present invention, soaking for 5 to 10 hours and then continuing to soak for 5 to 10 hours.

[0020] As a technical solution of the present invention, a device including a cathode plate is used to electrically adsorb the nickel ions, the cobalt ions and the manganese ions on the cathode plate under the action of an external electric field. The cathode plate is made of graphite or activated carbon.

[0021] As a technical solution of the present invention, cathode plates with different pore sizes are used, and different voltages are applied to electro-adsorb the nickel ions, cobalt ions, and manganese ions onto different cathode plates in sequence and separately.

[0022] As a technical solution of the present invention, a negative charge is applied to detach the nickel ions, cobalt ions, and manganese ions adsorbed on the cathode plate from the cathode plate and enter a fresh solution to obtain a mixed solution. An aluminum plate is placed in the mixed solution as an anode plate, and electrocoagulation is carried out under the action of an external electric field to obtain an aluminum-containing nickel-cobalt-manganese ternary precursor. Detailed implementation manners

[0023] The present invention provides a method for recycling a lithium nickel cobalt manganese oxide-based positive electrode sheet, which can realize the separation and purification of single metals in multivalent metals and can also prepare a nickel-cobalt-manganese ternary precursor.

[0024] The lithium nickel cobalt manganese oxide-based positive electrode sheet of the present invention refers to a positive electrode sheet containing a lithium nickel cobalt manganese oxide-based positive electrode active material. The lithium nickel cobalt manganese oxide-based positive electrode sheet includes a positive electrode active material, a binder, and a conductive agent. The positive electrode active material includes a lithium nickel cobalt manganese oxide-based positive electrode active material, and its chemical formula is LiNi x Co y Mn z M (1-x-y-z) O 2 , where M is at least one of Mg, Cu, Zn, Al, Sn, B, Ga, Cr, Sr, V, and Ti, 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z ≤ 1. The binder includes PVDF. The conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotube, and graphene. The mass ratio of the positive electrode active material, the binder, and the conductive agent can be, but is not limited to, 85-98:0.5-3.0:0.5-3.0. The positive electrode active material, the binder, and the conductive agent are made into a slurry with a solvent and coated on a positive electrode current collector, and then dried, roll-pressed, etc. to obtain a positive electrode sheet.

[0025] The method for recycling the lithium nickel cobalt manganese oxide-based positive electrode sheet of the present invention includes the following steps.

[0026] (1) The lithium nickel cobalt manganese oxide-based positive electrode sheet disassembled from the battery is dried to remove the electrolyte on the surface.

[0027] (2) After soaking in an organic acid solution for a certain time, hydrogen peroxide is added and soaking is continued until the positive electrode powder detaches from the positive electrode current collector.

[0028] (3) The positive electrode current collector is recycled to obtain a leaching solution containing the positive electrode powder.

[0029] (4) Electrochemical adsorption is carried out on the leaching solution to separate nickel ions, cobalt ions, and manganese ions.

[0030] Wherein, in step (1), the waste lithium-ion battery is discharged and disassembled by conventional technology, and then the positive electrode sheet and the negative electrode sheet are collected respectively. The drying temperature is 50°C to 60°C, which can be but not limited to 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C. The time is 8h to 12h, which can be but not limited to 8h, 9h, 10h, 11h, 12h. After drying, the electrolyte on the surface of the positive electrode sheet can be removed to avoid reaction with organic acid.

[0031] The organic acid solution in step (2) is an aqueous solution of organic acid with a mass concentration of 8% to 10%, and the mass concentration can be but not limited to 8%, 9%, and 10%. The organic acid includes at least one of tartaric acid, oxalic acid, malic acid, citric acid, acetic acid, ascorbic acid, and benzoic acid. One or more organic acids can be selected and used in combination according to actual conditions to improve the treatment effect. During the acid leaching process, H + By reacting with the oxide layer on the surface of the positive electrode current collector, the contact interface between the membrane in the electrode (formed by coating the positive electrode active material, conductive agent and binder into a slurry and then drying) and the positive electrode current collector can be destroyed, thereby separating the electrode material from the current collector. At the same time, compared with strong inorganic acids such as sulfuric acid, hydrochloric acid and nitric acid, organic acids tend to be milder, and the post-processing of related waste materials is simpler and the processing cost is lower. In addition, the organic acid remaining in the positive electrode material layer after acid leaching can be converted into carbon material through high-temperature solid phase repair for recycling.

[0032] After adding the organic acid, hydrogen peroxide (H 2 O 2 ) The electrode is further immersed. The concentration of hydrogen peroxide can be appropriately adjusted and limited according to the actual situation, and can be but not limited to 0.1mol / L to 3mol / L. This concentration can ensure the oxidation effect while avoiding the impact on the positive electrode current collector. After adding hydrogen peroxide, it exhibits oxidizing properties under acidic conditions. Hydrogen peroxide undergoes a self-dissociation reaction to generate hydrogen ions (H + ), peroxide free radical (·O 2- ) and hydroxyl radicals (·OH) and other active oxidizing groups. The strong oxidizing properties of these active oxidizing groups can achieve oxidative degradation of some organic substances, such as the binder PVDF, or destroy its structure, reducing its bonding properties, thereby further promoting the separation of the membrane and the positive electrode current collector. In this process, hydrogen peroxide is equivalent to a free radical generator.

[0033] The immersion time of the positive electrode sheet of the nickel-cobalt-manganese oxide series in the organic acid solution is 5 to 10 hours, which can be but not limited to 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, and 10 hours. After adding hydrogen peroxide, it is immersed for another 5 to 10 hours, which can be but not limited to 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, and 10 hours.

[0034] Since step (1) and step (2) do not use a pulverization process and use an organic weak acid, which has no effect on the surface of the positive electrode current collector, the positive electrode current collector can be recovered in step (3) without loss, and a leachate containing positive electrode powder can be obtained after the positive electrode current collector is recovered. The binder in the positive electrode sheet will be dissolved or swelled in the above-mentioned acid leaching process and enter the leachate, and the conductive agent will be separated from the leachate in the form of a poorly soluble substance and can be removed by filtration.

[0035] The nickel ions, cobalt ions and manganese ions in the leachate can be electrically adsorbed onto the electrode plates under the action of an external electric field by using an electric adsorption device. The electric adsorption device can mainly include an anode plate, a cathode plate, an external wire and an external power source. The anode plate and the cathode plate can be composed of materials such as graphite and activated carbon, and the specific components are not limited. The anode plate and the cathode plate are both placed in the leachate, and the external power source is turned on to charge the anode plate and the cathode plate. The nickel, cobalt and manganese ions in the leachate are adsorbed onto the graphite and activated carbon electrode plates with a huge specific surface area under the action of the electric field, thereby realizing recovery. The dissolved or swollen binder continues to remain in the leachate during the electric adsorption process and will not be adsorbed onto the electrode plates together with the metal ions.

[0036] Furthermore, cathode plates with different pore sizes can be used, and different voltages can be applied to sequentially and separately adsorb nickel ions, cobalt ions, and manganese ions on different cathode plates, so that the three different ions of nickel, cobalt, and manganese can be separated in sequence to achieve the separation and purification of single metals. For example, the pore size of the cathode plate can be, but not limited to, 1 nm to 10 nm, and the specific surface area can be, but not limited to, 1500.0 m 2 / g to 1800.0m 2 The voltage may be, but is not limited to, 0.8V to 1.0V.

[0037] As another technical solution, the nickel, cobalt, and manganese ions adsorbed on the cathode plate can be negatively charged to separate the nickel ions, cobalt ions, and manganese ions from the cathode plate and enter the fresh solution to obtain a mixed solution. The fresh solution is different from the leachate and can form a stable solution with the nickel ions, cobalt ions, and manganese ions, including but not limited to dilute sulfuric acid, dilute hydrochloric acid, etc., so as to realize the transfer of nickel, cobalt, and manganese ions from the leachate to the ordinary solution. An aluminum plate is placed in the mixed solution as an anode plate and electro-flocculation is performed under the action of an external electric field to obtain an aluminum-containing nickel-cobalt-manganese ternary precursor. The device used for electro-flocculation may include an anode plate, a cathode plate, an external wire, and an external power source. The anode plate of the device used for electro-flocculation may be an aluminum plate, and the material of the cathode plate is graphite or activated carbon. During the electro-flocculation process, it can react with nickel, cobalt, and manganese ions to finally form an aluminum-containing nickel-cobalt-manganese ternary precursor.

[0038] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.

[0039] Example 1

[0040] This embodiment is a method for recovering nickel, cobalt and manganese metals in a nickel-cobalt-manganese-lithium oxide positive electrode sheet, and the steps are as follows.

[0041] (1) In a glove box, the waste lithium-ion batteries were completely discharged and disassembled to obtain positive electrode sheets. The positive electrode sheet contained NCM523 as the positive electrode active material, PVDF as the binder, and SP as the conductive agent, with a mass ratio of 95:3:2. The positive electrode sheet was dried at 55°C for 10 h to remove the electrolyte on the surface of the sheet.

[0042] (2) The dried electrode was immersed in a 10 wt.% aqueous solution of citric acid for 7 h, and then 2 mol / L hydrogen peroxide was added and immersed for 8 h until the positive electrode powder was separated from the aluminum foil.

[0043] (3) Recycling the aluminum foil to obtain a leachate containing positive electrode powder.

[0044] (4) An electric adsorption device is used, which includes a graphite anode plate, a graphite cathode plate, an external wire and an external power source. The anode plate and the cathode plate are both placed in the leaching solution, and the external power source is turned on to charge the anode plate and the cathode plate. Three cathode plates with different pore sizes are used, and different voltages are applied to sequentially and separately adsorb nickel ions, cobalt ions and manganese ions on different cathode plates, thereby separating the three different ions of nickel, cobalt and manganese into nickel, cobalt and manganese metals.

[0045] In this embodiment, the aluminum foil recovered in step (3) is a whole sheet with no damage on the surface. Then, the nickel, cobalt and manganese metals on the cathode sheet are recovered respectively, and the recovery rates are calculated. The nickel, cobalt and manganese are 88.5%, 87.9% and 89.2% respectively, indicating that the recovery rates of nickel, cobalt and manganese obtained by the recovery method of the present invention are relatively high.

[0046] Example 2

[0047] This embodiment is a method for recovering nickel, cobalt and manganese metals in a nickel-cobalt-manganese-lithium oxide positive electrode sheet, and the steps are as follows.

[0048] (1) In a glove box, the waste lithium-ion batteries were completely discharged and then disassembled to obtain positive electrode sheets. The positive electrode sheet contained NCM523 as the positive electrode active material, PVDF as the binder, and CNT as the conductive agent, with a mass ratio of 96:2:2. The positive electrode sheet was dried at 60°C for 11 hours to remove the electrolyte on the surface of the sheet.

[0049] (2) The dried electrode was immersed in an aqueous solution of tartaric acid with a concentration of 8 wt.% for 5 h, and then hydrogen peroxide with a concentration of 1 mol / L was added and immersed for 10 h until the positive electrode powder was separated from the aluminum foil.

[0050] (3) Recycling the aluminum foil to obtain a leachate containing positive electrode powder.

[0051] (4) An electric adsorption device is used, which includes a graphite anode plate, a graphite cathode plate, an external wire and an external power source. The anode plate and the cathode plate are both placed in the leaching solution, and the external power source is turned on to charge the anode plate and the cathode plate. Three cathode plates with different pore sizes are used, and different voltages are applied to sequentially and separately adsorb nickel ions, cobalt ions and manganese ions on different cathode plates, thereby separating the three different ions of nickel, cobalt and manganese into nickel, cobalt and manganese metals.

[0052] In this embodiment, the aluminum foil recovered in step (3) is a whole sheet with no damage on the surface. Then, the nickel, cobalt and manganese metals on the cathode sheet are recovered respectively, and the recovery rates are calculated. The nickel, cobalt and manganese are 89.4%, 88.9% and 89.5% respectively, indicating that the recovery rates of nickel, cobalt and manganese obtained by the recovery method of the present invention are relatively high.

[0053] Example 3

[0054] This embodiment is a method for recovering a nickel-cobalt-manganese ternary precursor in a nickel-cobalt-manganese lithium oxide positive electrode sheet, and the steps are as follows.

[0055] (1) In a glove box, the waste lithium-ion batteries were completely discharged and then disassembled to obtain the positive electrode sheet. The positive electrode active material of the positive electrode sheet is LiNi 0.8 Co 0.098 Mn 0.098 Mg 0.004 O2 The binder is PVDF, the conductive agent is SP, and the mass ratio of the three is 95:3:2. The positive electrode sheet is dried at 55°C for 10 hours to remove the electrolyte on the surface of the electrode sheet.

[0056] (2) The dried electrode was immersed in a 10 wt.% aqueous solution of citric acid for 7 h, and then mol / L hydrogen peroxide was added and immersed for 8 h until the positive electrode powder was separated from the aluminum foil.

[0057] (3) Recycling the aluminum foil to obtain a leachate containing positive electrode powder.

[0058] (4) An electric adsorption device is used, which includes an activated carbon anode plate, an activated carbon cathode plate, an external wire and an external power source. The anode plate and the cathode plate are both placed in the leaching solution, and the external power source is turned on to charge the anode plate and the cathode plate, and the nickel ions, cobalt ions and manganese ions are all adsorbed on the cathode plate. Then, negative electricity is applied to separate the nickel ions, cobalt ions and manganese ions from the cathode plate and enter a hydrochloric acid solution with a concentration of 5wt.% to obtain a mixed solution. An electric flocculation device is placed in the mixed solution to perform electric flocculation, and the electric flocculation device includes an anode aluminum plate, a graphite cathode plate, an external wire and an external power source. Under the action of the external electric field, electric flocculation occurs on the aluminum plate to obtain a nickel-cobalt-manganese ternary precursor containing aluminum and magnesium.

[0059] In this embodiment, the aluminum foil recovered in step (3) is a whole sheet with no surface damage, and the nickel-cobalt-manganese ternary precursor is recovered, and the recovery rate is calculated to be 87.5%, indicating that the recovery rate of the nickel-cobalt-manganese ternary precursor prepared by the recovery method of the present invention is relatively high.

[0060] Example 4

[0061] This embodiment is a method for recovering a nickel-cobalt-manganese ternary precursor in a nickel-cobalt-manganese lithium oxide positive electrode sheet, and the steps are as follows.

[0062] (1) In a glove box, the waste lithium-ion batteries were completely discharged and then disassembled to obtain the positive electrode sheet. The positive electrode active material of the positive electrode sheet is LiNi 0.8 Co 0.098 Mn 0.098 Mg 0.004 O 2 The binder is PVDF, the conductive agent is CNT, and the mass ratio of the three is 96:2:2. The positive electrode sheet is dried at 60°C for 11 hours to remove the electrolyte on the surface of the electrode sheet.

[0063] (2) The dried electrode was immersed in an aqueous solution of 8 wt.% citric acid for 5 h, and then 1 mol / L hydrogen peroxide was added and immersed for 10 h until the positive electrode powder was separated from the aluminum foil.

[0064] (3) Recycling the aluminum foil to obtain a leachate containing positive electrode powder.

[0065] (4) An electric adsorption device is used, which includes an activated carbon anode plate, an activated carbon cathode plate, an external wire and an external power source. The anode plate and the cathode plate are both placed in the leaching solution, and the external power source is turned on to charge the anode plate and the cathode plate, and the nickel ions, cobalt ions and manganese ions are all adsorbed on the cathode plate. Then, negative electricity is applied to separate the nickel ions, cobalt ions and manganese ions from the cathode plate and enter a hydrochloric acid solution with a concentration of 5wt.% to obtain a mixed solution. An electric flocculation device is placed in the mixed solution to perform electric flocculation, and the electric flocculation device includes an anode aluminum plate, a graphite cathode plate, an external wire and an external power source. Under the action of the external electric field, electric flocculation occurs on the aluminum plate to obtain a nickel-cobalt-manganese ternary precursor containing aluminum and magnesium.

[0066] In this embodiment, the aluminum foil recovered in step (3) is a whole sheet with no surface damage, and the nickel-cobalt-manganese ternary precursor is recovered, and the recovery rate is calculated to be 88.2%, indicating that the recovery rate of the nickel-cobalt-manganese ternary precursor prepared by the recovery method of the present invention is relatively high.

[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for recycling nickel-cobalt-manganese-lithium positive electrode sheets, characterized in that: The cathode active material in the lithium nickel cobalt manganese oxide-based cathode sheet includes at least LiNi x Co y Mn z M (1-x-y-z) O2, where M is at least one of Mg, Cu, Zn, Al, Sn, B, Ga, Cr, Sr, V, and Ti, 0 < x < 1, 0 < y < 1, 0 < z < 1, and x + y + z ≤ 1, including: (1) drying the nickel-cobalt-manganese-lithium oxide positive electrode sheet removed from the battery to remove the electrolyte on the surface; (2) After soaking in the organic acid solution for a certain period of time, hydrogen peroxide is added and continued to soak until the positive electrode powder is separated from the positive electrode current collector; (3) recovering the positive electrode current collector to obtain a leachate containing the positive electrode powder; (4) The leaching solution is subjected to electrochemical adsorption to separate nickel ions, cobalt ions and manganese ions.

2. The method for recycling nickel-cobalt-manganese-lithium oxide positive electrode sheets according to claim 1, characterized in that: The nickel-cobalt-manganese-oxide lithium positive electrode sheet comprises a positive electrode active material, a binder and a conductive agent.

3. The method for recycling nickel-cobalt-manganese-lithium oxide positive electrode sheets according to claim 2, characterized in that: The binder includes PVDF.

4. The method for recycling nickel-cobalt-manganese-lithium oxide positive electrode sheets according to claim 2, characterized in that: The conductive agent includes at least one of conductive carbon black, conductive graphite, carbon fiber, carbon nanotube and graphene.

5. The method for recycling nickel-cobalt-manganese-lithium oxide positive electrode sheets according to claim 1, characterized in that: The drying temperature is 50° C. to 60° C., and the drying time is 8 h to 12 h.

6. The method for recycling nickel-cobalt-manganese-lithium oxide positive electrode sheets according to claim 1, characterized in that: The organic acid solution is an aqueous solution of organic acid with a mass concentration of 8% to 10%, and the organic acid includes at least one of tartaric acid, oxalic acid, malic acid, citric acid, acetic acid, ascorbic acid and benzoic acid.

7. The method for recycling nickel-cobalt-manganese-lithium oxide positive electrode sheets according to claim 1, characterized in that: Soak for 5 to 10 hours and then continue soaking for another 5 to 10 hours.

8. The method for recycling nickel-cobalt-manganese-lithium oxide positive electrode sheets according to claim 1, characterized in that: A device including a cathode plate is used to electrically adsorb the nickel ions, the cobalt ions and the manganese ions on the cathode plate under the action of an external electric field. The cathode plate is made of graphite or activated carbon.

9. The method for recycling nickel-cobalt-manganese-lithium oxide positive electrode sheets according to claim 8, characterized in that: The cathode plates with different pore sizes are used, and different voltages are applied to electrically adsorb the nickel ions, the cobalt ions and the manganese ions on different cathode plates in sequence and respectively.

10. The method for recycling nickel-cobalt-manganese-lithium oxide positive electrode sheets according to claim 1, characterized in that: Negative electricity is applied to separate the nickel ions, cobalt ions and manganese ions adsorbed on the cathode plate from the cathode plate and enter into a fresh solution to obtain a mixed solution. An aluminum plate is placed in the mixed solution as an anode plate and electrocoagulation is performed under the action of an external electric field to obtain an aluminum-containing nickel-cobalt-manganese ternary precursor.

Citation Information

Patent Citations

  • Method for separating and recovering valuable metals from positive electrode materials of waste lithium ion batteries

    CN110620277A

  • Treatment method and treatment device for positive electrode powder of waste lithium ion battery

    CN117936962A

  • Method for separating and enriching manganese

    CN118086699A

  • Eco friendly recycling method for battery

    KR102441685B1

Cited By

  • Recycling method of waste lithium ion battery

    CN119921019A