Carbon nanotube composite material for in-situ growth of transition metal fluoride as well as preparation method and application of carbon nanotube composite material

By growing carbon nanotube composites with transition metal fluoride in situ in the positive electrode material of lithium-ion battery, the problems of low conductivity and poor contact effect of existing materials are solved, and the electrochemical performance and energy density of lithium-ion batteries are significantly improved. .

CN118954487APending Publication Date: 2024-11-15DEEPAL AUTOMOBILE TECH CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411042250.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The specific capacity and energy density of the existing lithium-ion battery positive electrode materials are limited, the electronic conductivity of transition metal fluoride is low, which affects the electrochemical performance, and the contact effect with carbon materials is poor, resulting in unsatisfactory improvement effect.

Method used

Carbon nanotube composite materials that grow transition metal fluorides in situ are used to form transition metal fluorides on the surface of carbon nanotubes through acidification and heat treatment to ensure good interface contact between materials and improve electrochemical performance.

Benefits of technology

It significantly improves the electron transfer rate during the electrochemical reaction, and improves the discharge specific capacity and energy density of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954487A_ABST
    Figure CN118954487A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, in particular to a carbon nanotube composite material for in-situ growth of transition metal fluoride as well as a preparation method and application of the carbon nanotube composite material. The method comprises the following steps: S1, acidizing original carbon nanotubes, and dispersing the acidized carbon nanotubes in a transition metal salt solution to obtain a mixed solution; s2, adding alkali into the mixed solution, stirring and reacting for a preset time, and attaching and connecting the precipitate obtained by the reaction of the transition metal salt and the alkali to the surface of the acidified carbon nanotube; after the reaction is completed, taking solids in the mixed solution and drying to obtain a precursor; and S3, mixing the precursor with a fluorine source, and then carrying out heat treatment under a protective atmosphere condition to obtain the carbon nanotube composite material for in-situ growth of the transition metal fluoride. A good interface contact effect between the transition metal fluoride and the carbon nano tube can be ensured, and the carbon nano tube provides an electron rapid transmission channel for the transition metal fluoride, so that the electrochemical performance of the transition metal fluoride is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a carbon nanotube composite material of in-situ grown transition metal fluorides, a preparation method and an application thereof. Background Art

[0002] In the past few decades, lithium-ion batteries have been gradually applied from small electronic devices such as communication equipment to large power supply equipment such as electric vehicles. However, the continuous upgrading of terminal products is accompanied by the gradual increase in the demand for battery energy density. For current commercial lithium-ion battery positive electrode materials such as LiCoO2, LiNi 1-x-y Co x Mn y For O2 and LiFePO4, the lithium storage process of this type of material is based on embedded intercalation reaction. The number of lithium ions stored and electrons transferred per unit of transition metal does not exceed 1, which limits the specific capacity and energy density of the material. Therefore, in order to achieve a wider application of lithium-ion batteries, it is necessary to find a new type of lithium-ion battery positive electrode material with high specific capacity and high energy density.

[0003] Since the redox reaction of the conversion material in the electrochemical process involves multiple electron transfer, it can provide a much higher specific capacity than traditional embedded materials. x (M=Fe, Co, Ni, Cu, etc.) As a kind of conversion material, due to the fact that fluorine (F) element has the strongest electronegativity, the formed MF ionic bond is strong, which makes transition metal fluoride have a higher theoretical potential than similar materials, making it more suitable as anode material for lithium-ion batteries. However, the strong ionic bonding of MF causes x Too large a bandgap width results in low electronic conductivity, which in turn affects the actual electrochemical reaction process. Therefore, improving the electronic conductivity of transition metal fluorides becomes the key to improving their electrochemical performance.

[0004] Current research has mostly used carbon materials, metal oxides and other materials with better conductivity to compound with transition metal fluorides to improve the overall conductivity of the material. However, due to the poor contact between the transition metal fluorides and the introduced materials, the improvement effect is still not ideal. Summary of the invention

[0005] The purpose of the present invention is to provide a carbon nanotube composite material with in-situ grown transition metal fluorides, a preparation method and an application thereof, which can ensure a good interface contact effect between the transition metal fluorides and the carbon nanotubes. The carbon nanotubes provide a rapid electron transmission channel for the transition metal fluorides located on the surface of the tube wall, thereby improving their electrochemical performance.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] In a first aspect, the present invention provides a method for preparing a carbon nanotube composite material of in-situ grown transition metal fluoride, comprising the following steps:

[0008] S1, acidifying the original carbon nanotubes, and then dispersing the acidified carbon nanotubes in a transition metal salt solution to obtain a mixed solution;

[0009] S2, adding a base to the mixed solution, stirring the reaction for a preset time, and the precipitate obtained by the reaction of the transition metal salt and the base is attached to the surface of the acidified carbon nanotubes; after the reaction is completed, the solid matter in the mixed solution is taken and dried to obtain a precursor;

[0010] S3, mixing the precursor with a fluorine source, and then performing a heat treatment under protective atmosphere conditions to obtain a carbon nanotube composite material with in-situ growth of transition metal fluoride.

[0011] Furthermore, the acidification treatment of the original carbon nanotubes in S1 includes: adding the original carbon nanotubes to a prepared mixed acid solution of concentrated sulfuric acid and concentrated nitric acid, the concentration ratio of concentrated sulfuric acid to concentrated nitric acid is 6:1 to 2:1, heating the reaction for a preset time, the heating temperature is 50 to 100°C, and the heating reaction time is 120 to 360 minutes; washing the reaction product with deionized water until it is neutral, and obtaining the acidified carbon nanotubes after filtering and drying.

[0012] Further, the transition metal salt in S1 is a sulfate, oxalate, acetate or nitrate of a transition metal; the transition metal includes at least one of iron Fe, cobalt Co, nickel Ni, copper Cu, zinc Zn and manganese Mn;

[0013] and / or, the concentration of the transition metal salt solution in S1 is 0.05 to 2 mol / L;

[0014] And / or, the mass ratio of the acidified carbon nanotubes to the transition metal salt in S1 is 1:2 to 1:10.

[0015] Furthermore, the transition metal salt solution in S1 further comprises a dispersant, wherein the dispersant is at least one of polyvinyl pyrrolidone, carboxymethyl cellulose, methyl cellulose and polyacrylamide;

[0016] The mass ratio of the dispersant to the transition metal salt is 1:2 to 1:10.

[0017] Further, the alkali in S2 is a sodium hydroxide solution with a concentration of 0.05 to 2 mol / L;

[0018] and / or, the volume ratio of the mixed solution to the sodium hydroxide solution in S2 is 1:1 to 1:5;

[0019] And / or, the stirring reaction time of the mixed solution and the alkali in S2 is 30 to 180 minutes.

[0020] Further, the fluorine source in S3 includes at least one of ammonium fluoride, ammonium bifluoride and polyvinylidene fluoride;

[0021] and / or, the mass ratio of the precursor to the fluorine source in S3 is 1:1 to 1:5;

[0022] And / or, the heat treatment temperature in S3 is 230-280° C., and the insulation time is 90-720 min.

[0023] Furthermore, the obtained carbon nanotube composite material with in-situ grown transition metal fluoride comprises carbon nanotubes and transition metal fluoride in-situ grown on the wall surface of the carbon nanotubes.

[0024] In a second aspect, the present invention provides an in-situ grown transition metal fluoride carbon nanotube composite material prepared by the above-mentioned method for preparing the in-situ grown transition metal fluoride carbon nanotube composite material.

[0025] Furthermore, the material includes carbon nanotubes and transition metal fluorides that are in-situ grown on the wall surfaces of the carbon nanotubes.

[0026] In a third aspect, the present invention provides an application of an in-situ grown transition metal fluoride carbon nanotube composite material prepared by the above-mentioned preparation method of an in-situ grown transition metal fluoride carbon nanotube composite material in a lithium ion battery.

[0027] Beneficial effects of the present invention: By adopting the preparation method of the present invention, transition metal fluorides can be grown in situ on the surface of the tube wall of the carbon nanotube, so that there is a good contact effect between the carbon nanotube and the transition metal fluoride. The carbon nanotube provides a fast electron transmission channel for the transition metal fluoride located on the surface of the tube wall, fully utilizing the high conductivity of the carbon nanotube, effectively improving the transmission rate between electrons and active substances in the electrochemical reaction process, and significantly improving its discharge specific capacity and energy density. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention.

[0029] Figure 1 The flowchart of the preparation method of the carbon nanotube composite material with in-situ growth of transition metal fluoride according to the embodiment of the present invention is shown.

[0030] Figure 2The XRD diagram of the in-situ grown transition metal fluoride carbon nanotube composite material prepared in Example 1 of the present invention is shown.

[0031] Figure 3 The TEM image of the in-situ grown transition metal fluoride carbon nanotube composite material prepared in Example 1 of the present invention is shown. DETAILED DESCRIPTION

[0032] The following will describe the embodiments of the present invention with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.

[0033] In one embodiment, see Figure 1 As shown, the present invention provides a method for preparing a carbon nanotube composite material of in-situ grown transition metal fluoride, which comprises the following steps:

[0034] S1, acidifying the original carbon nanotubes, and then dispersing the acidified carbon nanotubes in a transition metal salt solution to obtain a mixed solution;

[0035] S2, adding a base to the mixed solution, stirring the reaction for a preset time, and the precipitate obtained by the reaction of the transition metal salt and the base is attached to the surface of the acidified carbon nanotubes; after the reaction is completed, the solid matter in the mixed solution is taken and dried to obtain a precursor;

[0036] S3, mixing the precursor with a fluorine source, and then performing a heat treatment under protective atmosphere conditions to obtain a carbon nanotube composite material with in-situ growth of transition metal fluoride.

[0037] By adopting the preparation method of the present invention, transition metal fluorides can be grown in situ on the tube wall surface of the carbon nanotube, so that there is a good contact effect between the carbon nanotube and the transition metal fluoride. The carbon nanotube provides a fast electron transmission channel for the transition metal fluoride located on the tube wall surface, fully utilizing the high conductivity of the carbon nanotube, effectively improving the transmission rate between electrons and active substances in the electrochemical reaction process, and significantly improving its discharge specific capacity and energy density.

[0038] In a preferred embodiment, the acidification treatment of the original carbon nanotubes in S1 includes: adding the original carbon nanotubes to a prepared mixed acid solution of concentrated sulfuric acid and concentrated nitric acid, heating the reaction for a preset time, washing the reaction product with deionized water until it is neutral, and obtaining the acidified carbon nanotubes after filtering and drying.

[0039] The mixed acid solution of concentrated sulfuric acid and concentrated nitric acid is extremely oxidizing and corrosive, which can effectively remove impurities on the surface of carbon nanotubes and introduce active functional groups on their surface. When preparing the mixed acid solution of concentrated sulfuric acid and concentrated nitric acid, the concentrated nitric acid should be added to the concentrated sulfuric acid slowly and stirred continuously to avoid splashing caused by intense heat release. At the same time, the operation should be carried out in a fume hood and appropriate protective equipment should be worn.

[0040] The concentration ratio of concentrated sulfuric acid to concentrated nitric acid is 6:1 to 2:1. When using a mixed solution of concentrated sulfuric acid and concentrated nitric acid to acidify the original carbon nanotubes, the concentration ratio of concentrated sulfuric acid to concentrated nitric acid is an important parameter, which will affect the rate and effect of the acidification reaction and the chemical properties of the surface of the carbon nanotubes. The mentioned concentration ratio range of 6:1 to 2:1 is a relatively reasonable range, but the specific ratio needs to be determined according to the specific requirements and goals of the experiment.

[0041] Function of concentrated sulfuric acid: concentrated sulfuric acid is a strong acid with dehydrating and oxidizing properties. During the acidification process, it mainly removes impurities (such as catalyst residues, amorphous carbon, etc.) on the surface of carbon nanotubes, and may introduce some oxygen-containing functional groups (such as carboxyl, hydroxyl, etc.) on the surface of carbon nanotubes through dehydration reaction.

[0042] The role of concentrated nitric acid: concentrated nitric acid is also a strong acid, but it has stronger oxidizing properties than concentrated sulfuric acid. In mixed acids, the strong oxidizing property of concentrated nitric acid helps to further oxidize the surface of carbon nanotubes and promote the formation of active functional groups. In addition, concentrated nitric acid can also work synergistically with concentrated sulfuric acid to improve the efficiency of the acidification reaction.

[0043] Selection of concentration ratio: When the concentration of concentrated sulfuric acid is much higher than that of concentrated nitric acid, the acidification reaction may rely more on the dehydration and acidity of concentrated sulfuric acid, while the strong oxidizing effect of concentrated nitric acid is relatively weak. This ratio may be suitable for scenarios where milder acidification conditions are required or there is a concern that concentrated nitric acid may damage the structure of carbon nanotubes due to its strong oxidizing property. As the proportion of concentrated nitric acid increases, the oxidizing property of the mixed acid increases. This ratio may be more suitable for scenarios where impurities on the surface of carbon nanotubes need to be removed quickly and thoroughly, and a large number of active functional groups are introduced on their surface. However, an excessively high proportion of concentrated nitric acid may also increase the potential risk of damage to the structure of carbon nanotubes. In actual operation, the appropriate concentration ratio should be selected according to the specific requirements and objectives of the experiment. The effect of different concentration ratios on the acidification effect can be evaluated through preliminary experiments.

[0044] The specific operation of the acidification treatment is: gradually add a certain amount of original carbon nanotubes to the prepared mixed acid solution, stirring while adding to ensure that the carbon nanotubes are fully in contact with the mixed acid solution. It should be noted that too much carbon nanotubes should not be added at one time to avoid excessive local concentration leading to uneven reaction.

[0045] Heating can accelerate the rate of chemical reactions and make the acidification process more thorough. The preset time for the heating reaction needs to be determined based on specific experimental conditions (such as acid concentration, temperature, type and purity of carbon nanotubes, etc.). Generally speaking, sufficient time is required to ensure that the acidification reaction is fully carried out, but it is also necessary to avoid damaging the carbon nanotube structure due to too long a time. It should be noted that the temperature should be controlled during heating to avoid excessively high temperatures that cause the solution to boil or the carbon nanotubes to burn. At the same time, samples should be taken regularly to observe the progress of the reaction. Preferably, the heating temperature is set to 50-100°C, and the heating reaction time is set to 120-360min.

[0046] Purpose of washing to neutrality: to remove the acid remaining on the surface of the carbon nanotubes and the by-products generated by the reaction, so that the surface of the carbon nanotubes is restored to neutrality, which is beneficial to the subsequent steps.

[0047] Deionized water: Deionized water is used to avoid the introduction of new ionic impurities.

[0048] Washing method: Multiple washing and centrifugal separation can be used until the washing liquid becomes neutral.

[0049] Filtration: Use a filtration device to separate the washed carbon nanotubes from water. During filtration, it is necessary to control the pressure to avoid excessive pressure that may damage the carbon nanotube structure.

[0050] Drying: Place the filtered carbon nanotubes in an oven to dry to remove residual moisture. The drying temperature should be moderate to avoid high temperature causing oxidation or structural changes in the carbon nanotubes.

[0051] Through the above steps, the surface of the original carbon nanotubes was successfully acidified and active functional groups were introduced, providing favorable conditions for the subsequent combination with transition metal salts.

[0052] In a preferred embodiment, the transition metal salt in S1 is a sulfate, oxalate, acetate or nitrate of a transition metal; the transition metal includes at least one of iron Fe, cobalt Co, nickel Ni, copper Cu, zinc Zn and manganese Mn; these salts have good solubility in water and are easy to react with alkali to form corresponding hydroxides or basic salt precipitations. These precipitates will serve as precursors for subsequent fluorination reactions and adhere to the surface of the acidified carbon nanotubes.

[0053] And / or, the concentration of the transition metal salt solution in S1 is 0.05-2 mol / L. If the concentration is too low, the amount of transition metal compound attached to the surface of the carbon nanotubes may be insufficient, affecting the performance of the final composite material. If the concentration is too high, it may cause excessive precipitation and form agglomerates, which is not conducive to uniform distribution. Therefore, it is necessary to select the most appropriate concentration according to the specific experimental conditions and objectives.

[0054] And / or, the mass ratio of the acidified carbon nanotubes to the transition metal salt in S1 is 1:2 to 1:10. During the preparation process, the mass of the transition metal salt can be relatively large relative to the mass of the acidified carbon nanotubes. This helps to ensure that the surface of the carbon nanotubes can be fully covered with the transition metal compound. However, too high a mass ratio may also cause the transition metal compound layer on the surface of the carbon nanotubes to be too thick, affecting the conductivity and other properties of the composite material. Therefore, it is also necessary to determine the optimal mass ratio based on the specific requirements and objectives of the experiment.

[0055] When the transition metal salt solution is mixed with the acidified carbon nanotubes, sufficient stirring should be ensured so that the transition metal salt can be evenly distributed on the surface of the carbon nanotubes.

[0056] The attachment and growth process of transition metal compounds on the surface of carbon nanotubes can be controlled by adjusting parameters such as the pH value of the solution, reaction temperature and time.

[0057] Before proceeding to the subsequent steps, the mixed solution should be thoroughly washed and centrifuged to remove unattached transition metal salts and other impurities.

[0058] The entire operation process should be carried out in a fume hood and appropriate protective equipment should be worn to ensure the safety of the experimenters.

[0059] In a preferred embodiment, the transition metal salt solution in S1 also includes a dispersant, which is at least one of polyvinyl pyrrolidone, carboxymethyl cellulose, methyl cellulose and polyacrylamide; the mass ratio of the dispersant to the transition metal salt is 1:2 to 1:10. The addition of the dispersant is intended to improve the dispersibility and adhesion uniformity of the transition metal salt on the surface of the acidified carbon nanotubes. Polyvinyl pyrrolidone PVP, as a high molecular polymer, has good water solubility and surface activity, and can be adsorbed on the surface of carbon nanotubes and transition metal particles to prevent agglomeration between them, thereby promoting more uniform dispersion.

[0060] In a preferred embodiment, the alkali in S2 is a sodium hydroxide solution with a concentration of 0.05 to 2 mol / L; the volume ratio of the mixed solution to the sodium hydroxide solution is 1:1 to 1:5; and the stirring reaction time of the mixed solution and the alkali is 30 to 180 min.

[0061] By using sodium hydroxide solution as an alkali source and controlling its concentration, volume ratio with the mixed solution and stirring reaction time, the reaction rate between the transition metal salt and the alkali and the generation of the product can be effectively adjusted.

[0062] The concentration of sodium hydroxide solution is 0.05-2 mol / L, which provides a suitable alkaline environment for reacting with transition metal salts to generate corresponding hydroxide precipitates. If the concentration is too low, the reaction rate may be too slow and the precipitation may not be completely generated; while if the concentration is too high, a violent reaction may be triggered, resulting in the precipitation particles being too large or forming agglomerates.

[0063] The volume ratio of the mixed solution to the sodium hydroxide solution is 1:1 to 1:5, and the amount of alkali added can be adjusted according to actual needs. A smaller volume ratio means that more alkali is added to the mixed solution, which helps to accelerate the reaction rate and promote the formation of precipitation. However, an excessively large volume ratio may cause other components in the mixed solution (such as acidified carbon nanotubes) to be diluted, affecting the adhesion effect of the precipitate on the surface of the carbon nanotubes.

[0064] The stirring reaction time is 30 to 180 minutes, which is determined based on the kinetic characteristics of the reaction between transition metal salts and bases. A shorter reaction time may not be enough for the reaction to proceed completely, resulting in insufficient precipitation; while a too long reaction time may increase unnecessary energy consumption and may induce other side reactions. Therefore, it is necessary to select the most appropriate reaction time based on the specific circumstances and objectives of the experiment.

[0065] In a preferred embodiment, the fluorine source in S3 includes at least one of ammonium fluoride, ammonium bifluoride and polyvinylidene fluoride. These fluorine sources can release fluoride ions or fluoride gases during the heat treatment process, reacting with the transition metal compound to achieve its fluorination. Ammonium fluoride and ammonium bifluoride, as inorganic fluorine sources, have the advantages of high reactivity and easy control; while polyvinylidene fluoride, as an organic fluorine source, may release fluoride gases by pyrolysis and the like, and react with the transition metal compound.

[0066] In a preferred embodiment, the mass ratio of the precursor to the fluorine source in S3 is 1:1 to 1:5, and this ratio range is determined based on experimental experience and the performance of the target product. A larger fluorine source ratio means that more fluoride ions or fluorinated gases will react with the transition metal compound, which may promote a more complete fluorination reaction, but it may also increase the risk of side reactions, such as excessive deposition of fluorides or destruction of the carbon nanotube structure. Therefore, it is necessary to select a suitable ratio based on the specific conditions of the experiment and the performance of the target product.

[0067] In a preferred embodiment, the heat treatment temperature in S3 is 230-280° C., and the holding time is 90-720 min. By reasonably limiting the heat treatment process parameters, the in-situ generation of transition metal fluorides is ensured.

[0068] The following is an explanation with reference to specific examples.

[0069] Embodiment 1, a method for preparing a carbon nanotube composite material of in-situ grown transition metal fluoride, characterized by comprising the following steps:

[0070] S1, acidifying the original carbon nanotubes, adding 1g of the original carbon nanotubes to 300mL of a mixed acid solution of concentrated sulfuric acid / concentrated nitric acid with a concentration ratio of 6:1, and heating the reaction at a temperature of 50°C for 360min. The reaction product is washed with deionized water until neutral, and then filtered and dried to obtain the acidified carbon nanotubes.

[0071] 1.81 g of cupric acetate, i.e., transition metal salt, and 0.181 g of polyvinyl pyrrolidone, i.e., dispersant, were weighed and dissolved in 200 mL of water to obtain a transition metal salt solution. 0.181 g of acidified carbon nanotubes were then dispersed in the transition metal salt solution and subjected to ultrasonic treatment to obtain a mixed solution.

[0072] S2, add 200mL of 0.05mol / L sodium hydroxide solution, i.e., alkali, to the mixed solution, stir and react for 180min, and the precipitate obtained by the reaction of the transition metal salt and the alkali is attached to the surface of the acidified carbon nanotubes. After the reaction is completed, centrifuge, obtain the solid in the mixed solution and dry it to obtain a precursor.

[0073] S3, mixing the precursor with a fluorine source, and then heat treating it under protective atmosphere conditions. Specifically: 0.5 g of the dried precursor is ground and mixed with 0.5 g of ammonium fluoride, and then heated at 230° C. for 720 min under nitrogen protection to obtain an in-situ grown copper fluoride carbon nanotube composite material.

[0074] The obtained product was subjected to XRD analysis, and the results are shown in Figure 2 The diffraction peaks at 2θ=27.6°, 31.6°, 33.6° and 35.5° correspond to the (011), (-101), (110) and (101) crystal planes of copper fluoride, respectively; while the diffraction peak near 2θ=26° can be attributed to carbon nanotubes, proving that the physical phases of the composite material are composed of pure anhydrous copper fluoride and carbon nanotubes.

[0075] The obtained product was subjected to TEM analysis. Figure 3 , you can see carbon nanotubes and copper fluoride particles growing on the walls of carbon nanotubes.

[0076] Embodiment 2, a method for preparing a carbon nanotube composite material of in-situ grown transition metal fluoride, characterized by comprising the following steps:

[0077] S1, acidifying the original carbon nanotubes, adding 1g of the original carbon nanotubes to 300mL of a mixed acid solution of concentrated sulfuric acid / concentrated nitric acid with a concentration ratio of 2:1, and heating the reaction at a temperature of 100°C for 120min. The reaction product is washed with deionized water until neutral, and then filtered and dried to obtain the acidified carbon nanotubes.

[0078] 1.81 g of cupric acetate, i.e., transition metal salt, and 0.181 g of polyvinyl pyrrolidone, i.e., dispersant, were weighed and dissolved in 50 mL of water to obtain a transition metal salt solution. 0.181 g of acidified carbon nanotubes were then dispersed in the transition metal salt solution and subjected to ultrasonic treatment to obtain a mixed solution.

[0079] S2, add 200mL of 0.05mol / L sodium hydroxide solution, i.e., alkali, to the mixed solution, stir and react for 180min, and the precipitate obtained by the reaction of the transition metal salt and the alkali is attached to the surface of the acidified carbon nanotubes. After the reaction is completed, centrifuge, obtain the solid in the mixed solution and dry it to obtain a precursor.

[0080] S3, mixing the precursor with a fluorine source, and then heat treating it under protective atmosphere conditions. Specifically, 0.5 g of the dried precursor is ground and mixed with 2.5 g of ammonium fluoride, and then heated at 280° C. for 90 minutes under nitrogen protection to obtain an in-situ grown copper fluoride carbon nanotube composite material.

[0081] Embodiment 3, a method for preparing a carbon nanotube composite material with in-situ growth of transition metal fluoride, characterized by comprising the following steps:

[0082] S1, acidifying the original carbon nanotubes, adding 1g of the original carbon nanotubes to 300mL of a mixed acid solution of concentrated sulfuric acid / concentrated nitric acid with a concentration ratio of 2:1, and heating the reaction at a temperature of 100°C for 120min. The reaction product is washed with deionized water until neutral, and then filtered and dried to obtain the acidified carbon nanotubes.

[0083] 1.81 g of cupric acetate, i.e., transition metal salt, and 0.181 g of polyvinyl pyrrolidone, i.e., dispersant, were weighed and dissolved in 100 mL of water to obtain a transition metal salt solution. 0.543 g of acidified carbon nanotubes were then dispersed in the transition metal salt solution and subjected to ultrasonic treatment to obtain a mixed solution.

[0084] S2, add 50mL of 2mol / L sodium hydroxide solution, i.e., alkali, to the mixed solution, stir and react for 180min, and the precipitate obtained by the reaction of the transition metal salt and the alkali is attached to the surface of the acidified carbon nanotubes. After the reaction is completed, centrifuge, obtain the solid in the mixed solution and dry it to obtain a precursor.

[0085] S3, mixing the precursor with a fluorine source, and then heat treating it under protective atmosphere conditions. Specifically, 0.5 g of the dried precursor is ground and mixed with 1.5 g of ammonium fluoride, and then heated at 250° C. for 300 min under nitrogen protection to obtain a carbon nanotube composite material with in-situ growth of copper fluoride.

[0086] Embodiment 4, a method for preparing a carbon nanotube composite material of in-situ grown transition metal fluoride, characterized by comprising the following steps:

[0087] S1, acidifying the original carbon nanotubes, adding 1g of the original carbon nanotubes to 300mL of a mixed acid solution of concentrated sulfuric acid / concentrated nitric acid with a concentration ratio of 3:1, and heating the reaction at a temperature of 60°C for 180min. The reaction product is washed with deionized water until neutral, and then filtered and dried to obtain the acidified carbon nanotubes.

[0088] 1.81 g of cupric acetate, i.e., transition metal salt, and 0.181 g of polyvinyl pyrrolidone, i.e., dispersant, were weighed and dissolved in 100 mL of water to obtain a transition metal salt solution. 0.905 g of acidified carbon nanotubes were then dispersed in the transition metal salt solution and subjected to ultrasonic treatment to obtain a mixed solution.

[0089] S2, add 100mL of 0.1mol / L sodium hydroxide solution, i.e., alkali, to the mixed solution, stir and react for 180min, and the precipitate obtained by the reaction of the transition metal salt and the alkali is attached to the surface of the acidified carbon nanotubes. After the reaction is completed, centrifuge, obtain the solid in the mixed solution and dry it to obtain a precursor.

[0090] S3, mixing the precursor with a fluorine source, and then heat treating it under protective atmosphere conditions. Specifically, 0.5 g of the dried precursor and 1 g of ammonium fluoride are ground and mixed, and then heated under argon protection at a temperature of 250° C. for 300 min to obtain an in-situ grown copper fluoride carbon nanotube composite material.

[0091] The products obtained in Examples 1 to 4 were respectively used as positive electrode active materials to assemble lithium ion batteries, and copper fluoride that had not been treated in any way was used as a positive electrode active material to assemble a lithium ion battery of a comparative example. The assembled lithium ion batteries were tested at a voltage range of 1.5 V to 4.2 V and a discharge rate of 0.1 C. The test results are shown in Table 1.

[0092] Table 1 Lithium-ion battery performance test results

[0093] Group First discharge specific capacity (mAh / g) First discharge specific energy (Wh / kg) Embodiment 1 545.2 1305.76 Embodiment 2 585.5 1395.43 Embodiment 3 597.8 1433.8 Embodiment 4 626.3 1532.44 Comparative Example 481.8 1072.06

[0094] By comparison, the first discharge specific capacity and first discharge specific energy of the lithium-ion batteries corresponding to Examples 1 to 4 are higher than those of the comparative example, indicating that the carbon nanotube composite improves the electrochemical properties of the material and improves the first discharge specific capacity and first discharge energy density of copper fluoride.

[0095] The above embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitution or change made by a person skilled in the art based on the present invention is within the protection scope of the present invention.

Claims

1. A method for preparing a carbon nanotube composite material of in-situ grown transition metal fluoride, characterized in that: The steps include: S1, acidifying the original carbon nanotubes, and then dispersing the acidified carbon nanotubes in a transition metal salt solution to obtain a mixed solution; S2, adding a base to the mixed solution, stirring the reaction for a preset time, and the precipitate obtained by the reaction of the transition metal salt and the base is attached to the surface of the acidified carbon nanotubes; after the reaction is completed, the solid matter in the mixed solution is taken and dried to obtain a precursor; S3, mixing the precursor with a fluorine source, and then performing a heat treatment under protective atmosphere conditions to obtain a carbon nanotube composite material with in-situ growth of transition metal fluoride.

2. The method for preparing the in-situ grown transition metal fluoride carbon nanotube composite material according to claim 1, characterized in that: The acidification treatment of the original carbon nanotubes in S1 includes: adding the original carbon nanotubes to a prepared mixed acid solution of concentrated sulfuric acid and concentrated nitric acid, wherein the concentration ratio of the concentrated sulfuric acid to the concentrated nitric acid is 6:1-2:1, heating the reaction for a preset time, the heating temperature is 50-100°C, and the heating reaction time is 120-360min; washing the reaction product with deionized water until it is neutral, and obtaining the acidified carbon nanotubes after suction filtration and drying.

3. The method for preparing the in-situ grown transition metal fluoride carbon nanotube composite material according to claim 1, characterized in that: The transition metal salt in S1 is a sulfate, oxalate, acetate or nitrate of a transition metal; the transition metal includes at least one of iron Fe, cobalt Co, nickel Ni, copper Cu, zinc Zn and manganese Mn; and / or, the concentration of the transition metal salt solution in S1 is 0.05-2 mol / L; And / or, the mass ratio of the acidified carbon nanotubes to the transition metal salt in S1 is 1:2 to 1:

10.

4. The method for preparing the in-situ grown transition metal fluoride carbon nanotube composite material according to claim 1, characterized in that: The transition metal salt solution in S1 further includes a dispersant, wherein the dispersant is at least one of polyvinyl pyrrolidone, carboxymethyl cellulose, methyl cellulose and polyacrylamide; The mass ratio of the dispersant to the transition metal salt is 1:2 to 1:

10.

5. The method for preparing the in-situ grown transition metal fluoride carbon nanotube composite material according to claim 1, characterized in that: The alkali in S2 is a sodium hydroxide solution with a concentration of 0.05~2mol / L; and / or, the volume ratio of the mixed solution to the sodium hydroxide solution in S2 is 1:1 to 1:5; And / or, the stirring reaction time of the mixed solution and the alkali in S2 is 30 to 180 minutes.

6. The method for preparing the in-situ grown transition metal fluoride carbon nanotube composite material according to claim 1, characterized in that: The fluorine source in S3 includes at least one of ammonium fluoride, ammonium bifluoride and polyvinylidene fluoride; and / or, the mass ratio of the precursor to the fluorine source in S3 is 1:1 to 1:5; And / or, the heat treatment temperature in S3 is 230-280° C., and the holding time is 90-720 min.

7. The method for preparing the in-situ grown transition metal fluoride carbon nanotube composite material according to claim 1, characterized in that: The obtained carbon nanotube composite material with in-situ grown transition metal fluoride comprises carbon nanotubes and transition metal fluoride in-situ grown on the tube wall surface of the carbon nanotubes.

8. An in-situ grown transition metal fluoride carbon nanotube composite material obtained by the method for preparing an in-situ grown transition metal fluoride carbon nanotube composite material as claimed in any one of claims 1 to 7.

9. The in-situ grown transition metal fluoride carbon nanotube composite material according to claim 8, characterized in that: The material comprises carbon nanotubes and transition metal fluorides in-situ grown on the tube wall surfaces of the carbon nanotubes.

10. Use of the in-situ grown transition metal fluoride carbon nanotube composite material obtained by the method for preparing the in-situ grown transition metal fluoride carbon nanotube composite material according to any one of claims 1 to 7 in a lithium ion battery.

Citation Information

Cited By

  • Nanotube-based adsorbing material and application thereof in resource utilization of waste incineration fly ash

    CN119346088A

  • Carbon nanotube / ZIF-67-derived Co-C / CNT catalytic membrane, preparation method and application

    CN120733788A

  • Carbon nanotube / ZIF-67 derived Co-C / CNT catalytic membranes, preparation methods and applications

    CN120733788B

  • High-performance fluoride composite material for thermal battery and preparation method of high-performance fluoride composite material