Recycled concrete micropowder-slag-based geopolymer cementing material and preparation method thereof

By combining components such as regenerated concrete powder, slag and Bacillus bacterial solution, a geopolymer gelling material with suitable settling time and fluidity was prepared, which solved the problems of low reaction efficiency and poor construction convenience of regenerated concrete powder, and achieved The effect of efficient curing and low-carbon construction is achieved.

CN118955026APending Publication Date: 2024-11-15HAINAN UNIV +2
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411028083.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the recycled concrete powder has low reaction efficiency when it is not activated, resulting in a decrease in the mechanical properties of the consolidated material. The condensation time and flowability performance during transportation and transmission during construction are not ideal, and lack both strength and high Research on condensation flow characteristics.

Method used

The geopolymer gelling material with suitable settling time and fluidity is prepared by specific stirring and preparation methods, and combined with the combination of the regenerated concrete micro powder, slag, blast furnace granulated slag, modified water glass and Bacillus bacterial solution. Alkaline excitants to improve the reaction efficiency and performance of the material.

Benefits of technology

It achieves a curing effect comparable to cement-based cementitious materials, saves energy consumption, reduces carbon emissions, improves the ductility and construction convenience of geopolymer cementitious materials, and meets the transportation and transmission needs during construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955026A_ABST
    Figure CN118955026A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of solid waste resource recycling and green low-carbon cementing materials, in particular to a recycled concrete micro powder-slag based geopolymer cementing material and a preparation method thereof. The material comprises 50-80 parts of recycled concrete micro powder, 20-50 parts of blast furnace granulated slag, 11-26 parts of an exciting agent, 38-44 parts of a solvent and 12-19 parts of bacillus. The preparation method comprises the following steps: preferentially preparing the exciting agent, then mixing the exciting agent with the recycled concrete micro powder and the blast furnace granulated slag, finally inoculating bacillus, and fully stirring and mixing to form the recycled concrete micro powder-slag based geopolymer cementing material. The method has the advantages that cement is partially replaced; the economical problems of solid waste resource storage and resource application can be effectively solved; a high-performance material with condensation flow characteristics and mechanical strength characteristics is simple and economical in material taking, rapid and convenient to construct and reliable and stable in curing effect; microorganisms are introduced, so that the impermeability is better improved; the curing effect is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste resource recycling and green low-carbon cementitious materials, and in particular to a recycled concrete micropowder-slag-based polymer cementitious material and a preparation method thereof. Background Art

[0002] In recent years, the use of construction and demolition waste to prepare geopolymers has attracted more attention. Waste concrete and waste bricks account for up to 80% of the waste. The recycling and crushing of these resources will inevitably produce dust powder with a particle size of less than 75μm, which is called recycled powder, mainly composed of recycled concrete powder and recycled brick powder. The main component of recycled powder is SiO 2 、Al 2 O 3 , CaO and other oxides, which meet the compound element composition required for the geopolymer reaction, and the recycled micropowder is still a solid waste that has not been "productized" and has great market value.

[0003] At present, the application of recycled micropowder is mainly concentrated in cement-based concrete or mortar as a supplementary material to replace part of the cement. However, recycled micropowder contains more inert mineral components, and the efficiency of the volcanic ash reaction without activation treatment is low. Adding large amounts will seriously reduce the mechanical properties of the consolidating material.

[0004] Therefore, in recent years, some experts and scholars have begun to apply it to the field of alkali-activated cementitious materials. The current research mainly focuses on the preparation of geopolymers by mixing sintered brick powder and different recycled micropowders, and lacks research on the performance of multi-component composite geopolymer systems composed of recycled concrete micropowders in conjunction with other solid wastes and consolidation technologies. In addition, the research and development of geopolymer cementitious materials containing recycled micropowders usually pursues high indicators such as strength and durability, but ignores whether they can meet the transportation and transmission requirements in construction in actual use, and does not pay enough attention to their setting time and fluidity performance indicators. The research and development of recycled micropowder geopolymers with both strength and high setting and flow characteristics is an important direction for future research. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a recycled concrete micropowder-slag-based polymer cementitious material and a preparation method thereof.

[0006] The first object of the present invention is to provide a recycled concrete powder-slag-based polymer cementitious material, comprising the following components in parts by mass:

[0007] 50-80 parts of recycled concrete powder;

[0008] 20-50 parts of blast furnace granulated slag;

[0009] 11 to 26 parts of stimulant;

[0010] 38-44 parts of solvent;

[0011] Bacillus 12-19 parts;

[0012] The activator is modified water glass obtained by mixing water glass solution and sodium hydroxide particles, and the modulus of the modified water glass is 1.0-1.6.

[0013] Preferably, the Bacillus is Bacillus pasteurianus;

[0014] The water glass solution comprises the following components in mass fractions: 29.5-30.0% silicon dioxide, 13.5-14.0% sodium hydroxide and 56.0-56.5% water.

[0015] Preferably, the particle size of the recycled concrete powder is 0.01 to 120 μm, and the specific surface area is 350 to 450 m 2 / Kg, or density is 2.16~2.77g / cm 3 .

[0016] Preferably, the particle size of the blast furnace granulated slag is 0.01 to 120 μm, and the specific surface area is 400 to 500 m 2 / Kg, or density is 2.67~3.33g / cm 3 .

[0017] Preferably, the solvent is water, with a pH value of ≥4.5; the sodium hydroxide particles in the activator are of analytical grade, with a solid content of 95-99%.

[0018] Preferably, the modulus of the modified water glass is 1.4.

[0019] Preferably, the recycled concrete powder is 60 parts, the blast furnace granulated slag is 40 parts, the activator is 21 parts, the solvent is 42 parts, and the Bacillus is 15 parts.

[0020] The second object of the present invention is to provide a method for preparing a recycled concrete powder-slag-based polymer cementitious material, which specifically comprises the following steps:

[0021] S1. Weigh recycled concrete powder, blast furnace granulated slag, water glass solution, sodium hydroxide particles, solvent and Bacillus according to each weight portion;

[0022] S2. The sodium hydroxide particles are slowly added to the water glass solution, and the addition process is continuously stirred and exothermic until completely dissolved. After the solution is stabilized, the film is cooled to room temperature to prepare an activator;

[0023] S3. Stir the recycled concrete powder and blast furnace granulated slag for 3 to 5 minutes until they are evenly mixed;

[0024] S4. The activator and solvent are added to the mixed powder of step S3 and stirred until the slurry is uniformly stirred;

[0025] S5. Prepare a spore-forming bacteria liquid, inoculate it into the mixed slurry of step S4, and stir it again for 3 to 5 minutes until it is completely stirred and uniform, so as to obtain a recycled concrete powder-slag-based polymer cementitious material.

[0026] Preferably, the stirring in steps S3, S4 and S5 has a rotation speed of 110 to 130 r / min.

[0027] Preferably, the Bacillus bacterial solution is Bacillus pasteurian bacterial solution, and the urease activity of the Bacillus pasteurian bacterial solution is 1.6 mM urea hydrolysed / min.

[0028] Compared with the prior art, the present invention can achieve the following beneficial effects:

[0029] In the prior art, cement-based cementitious materials are often used to reinforce soft soil layers, which will face the problems of high energy consumption and increased carbon emissions, causing multiple negative impacts on the ecological environment. The present invention uses recycled concrete micropowder, which is powder produced when concrete is crushed, to promote the utilization of waste concrete, and to achieve waste recycling, which is conducive to saving energy consumption. The geopolymer cementitious materials made by combining blast furnace slag and alkali excitation for soft soil reinforcement can also achieve a curing effect equivalent to that of cement-based cementitious materials, and the addition of Bacillus liquid to the cementitious materials combined with the biological consolidation method can greatly make up for the lack of ductility of the geopolymer cementitious materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The present invention is a flowchart of a method for preparing a recycled concrete micropowder-slag-based polymer cementitious material according to an embodiment of the present invention. DETAILED DESCRIPTION

[0031] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. In the following description, the same modules are represented by the same reference numerals. In the case of the same reference numerals, their names and functions are also the same. Therefore, the detailed description thereof will not be repeated.

[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and do not constitute a limitation of the present invention.

[0033] Example 1

[0034] This embodiment provides a recycled concrete fine powder-slag-based polymer cementitious material, comprising the following components in parts by weight:

[0035] Recycled concrete powder: 60 parts;

[0036] Blast furnace granulated slag: 40 parts;

[0037] Stimulant: 21 parts;

[0038] Solvent: 42 parts;

[0039] Bacillus: 15 parts;

[0040] Modified water glass modulus: 1.4.

[0041] The activator is a modified water glass prepared by mixing water glass solution and sodium hydroxide particles. The water glass solution includes the following components by mass fraction: 29.9% silicon dioxide (SiO 2 ), 13.75% sodium hydroxide (NaOH) and 56.35% water (H 2 O);

[0042] The specific surface area of ​​recycled concrete powder is 443.2m 2 / Kg, or a density of 2.36g / cm 3 , chemical composition is 39.66% SiO 2 、11.64%Al 2 O 3 , 32.36% CaO, 5.44% MgO, 4.90% Fe 2 O 3 、1.44% SO 3 、1.14%Na 2 O, 1.79% K 2 O, 0.86% TiO 2 , 0.23%P 2 O 5 , 0.52% others, the balance is loss on ignition, the particle size of the recycled concrete powder is less than 120μm;

[0043] The specific surface area of ​​blast furnace granulated slag is 467.40m 2 / Kg, density is 3.01g / cm 3 ; Chemical composition is 30.41% SiO 2 、15.26%Al 2 O 3 , 41.07% CaO, 8.33% MgO, 0.34% Fe 2 O 3 、2.07%SO 3 , 0.46%Na 2 O, 0.46% K 2 O, 0.72% TiO 2 , 0.12%P2 O 5 , 0.83% others, and the balance is loss on ignition. The particle size of the blast furnace granulated slag particles is less than 120μm.

[0044] The solvent is water, pH value ≥ 4.5, insoluble matter ≤ 10000 mg / L, soluble matter ≤ 10000 mg / L, chloride (as Cl - ≤3500mg / L, sulfate (in terms of SO 4 2- Calculation) ≤2700mg / L;

[0045] Urease activity of Bacillus pasteurianus culture 1.3mM urea hydrolysed / min, OD 600 The value is 2.4;

[0046] The sodium hydroxide particles are of analytical grade, with a solid content of 99%;

[0047] The preparation method specifically comprises the following steps:

[0048] S1. Weigh recycled concrete powder, blast furnace granulated slag, water glass, sodium hydroxide, solvent and Bacillus according to their weight parts:

[0049] S2. Slowly add the sodium hydroxide particles to the water glass, stirring and releasing heat during the addition process until the solution is completely dissolved, and after the solution is stabilized, the film is cooled to room temperature to prepare an activator;

[0050] S3. Stir the recycled concrete powder and slag powder for 3 to 5 minutes until they are evenly mixed. The speed during stirring is 120 ± 10 r / min;

[0051] S4. The activator and solvent are added to the mixed powder of recycled concrete powder and slag powder obtained in step S3 and stirred for at least 10 minutes until the slurry is uniformly stirred, and the speed during stirring is 120 ± 10r / min;

[0052] S5. Prepare a spore-forming bacteria liquid, inoculate it into the mixed slurry of step S4, and stir it again for 3 to 5 minutes until it is completely stirred and uniform, so as to obtain a recycled concrete micropowder-slag-based polymer cementitious material. The rotation speed during stirring is 120±10r / min.

[0053] The prepared recycled concrete micropowder-slag-based polymer slurry will be tested for its slurry fluidity, initial setting and final setting time, and its 28d unconfined compressive strength and 28d flexural strength under standard curing conditions (20±1℃, humidity 85%).

[0054] Various testing methods and processes:

[0055] The fluidity of geopolymer slurry is measured according to the standard "Test Method for Homogeneity of Concrete Admixtures" (GB / T8077-2012). The stirred geopolymer slurry is quickly injected into a truncated cone mold (upper inner diameter 36mm×lower inner diameter 60mm×height 60mm). The mold is lifted vertically for 30 seconds. The maximum diameters in two perpendicular directions are measured with a ruler, and the average value is taken as the fluidity of the geopolymer slurry.

[0056] The setting time of geopolymer slurry is measured with reference to the standard "Test Method for Water Consumption, Setting Time and Soundness of Cement Standard Consistency" (GBT1346-2011). During the test, the specimen is taken out of the moisture curing box and placed under the initial setting test needle of the standard Favica instrument. When the test needle sinks to 4mm±1mm from the bottom plate, it is the initial setting time of the slurry. Then replace it with the final setting needle of the annular attachment. When the annular attachment begins to leave no trace on the specimen, it is the final setting time of the clean slurry.

[0057] The unconfined compressive strength and flexural strength tests are tested in accordance with the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T17671-2021). The evenly stirred geopolymer slurry is divided into two layers and loaded into a 40mm×40mm×160mm prism triple mold and vibrated for 30 seconds. It is quickly placed in a curing room for curing for 2 hours (temperature 20±1℃, relative humidity not less than 85%), demolded, and cured for 28 days. The flexural strength and unconfined compressive strength of the test block are tested successively. The cement mortar test hydraulic press is used to load at a rate of 10mm / min. The flexural strength is taken as the average strength of three prisms, and the unconfined compressive strength is taken as the average strength of six broken half prisms. If a test block deviates from the mean by more than 10%, this group of test blocks shall be redone.

[0058] Test results: The initial setting and final setting times of the recycled concrete powder-slag-based polymer obtained according to the proportion of the components in this group are 47 minutes and 55 minutes respectively. According to the "General Portland Cement" (GB175-2007) specification, it can meet the requirements of cement paste for initial setting time ≥45 minutes and final setting time ≤6 hours. The fluidity is 203mm, with good slurry fluidity. The unconfined compressive strength of the test block under 28-day standard curing conditions is 45.81MPa, and the flexural strength is 6.50MPa. The recycled concrete powder can be effectively dissolved in the water glass solution under the flocculation and synergistic effect of slag, providing the [SiO4] and [AlO4] tetrahedral units required for the polymerization reaction and additional Ca 2 + nucleation sites, combined with the free SiO 3 2- and Na +, promoting the geopolymer system to form a hybrid bonding cement composed of gels such as C-(N)-ASH and C-(A)-SH, thereby forming a dense and compact microstructure and providing the required strength for the sample.

[0059] Example 2

[0060] This embodiment provides a recycled concrete fine powder-slag-based polymer cementitious material, comprising the following components in parts by weight:

[0061] Recycled concrete powder: 80 parts;

[0062] Blast furnace granulated slag: 20 parts;

[0063] Stimulant: 21 parts;

[0064] Solvent: 42 parts;

[0065] Bacillus: 15 parts;

[0066] Modified water glass modulus: 1.4;

[0067] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the recycled concrete fine powder-slag-based polymer cementitious material is the same as that in Example 1.

[0068] Measurement results: The initial and final setting times of the recycled concrete micropowder-slag-based polymer obtained according to the proportion of components in this group are 101min and 197min respectively, the fluidity is 175mm, and the unconfined compressive strength of the test block under 28d standard curing conditions is 14.22MPa, and the flexural strength is 3.41MPa.

[0069] Example 3

[0070] This embodiment provides a recycled concrete fine powder-slag-based polymer cementitious material, comprising the following components in parts by weight:

[0071] Recycled concrete powder: 60 parts;

[0072] Blast furnace granulated slag: 40 parts;

[0073] Stimulant: 11 parts;

[0074] Solvent: 38 parts;

[0075] Bacillus: 12 parts

[0076] Modified water glass modulus: 1.4;

[0077] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the recycled concrete fine powder-slag-based polymer cementitious material is the same as that in Example 1.

[0078] Measurement results: The initial and final setting times of the recycled concrete powder-slag-based polymer obtained according to the proportion of components in this group are 71min and 89min respectively, the fluidity is 181mm, and the unconfined compressive strength of the test block under 28d standard curing conditions is 20.21MPa, and the flexural strength is 3.97MPa.

[0079] Example 4

[0080] This embodiment provides a recycled concrete fine powder-slag-based polymer cementitious material, comprising the following components in parts by weight:

[0081] Recycled concrete powder: 50 parts;

[0082] Blast furnace granulated slag: 50 parts;

[0083] Stimulant: 16 parts;

[0084] Solvent: 40 parts;

[0085] Bacillus: 19 parts

[0086] Modified water glass modulus: 1.4;

[0087] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the recycled concrete fine powder-slag-based polymer cementitious material is the same as that in Example 1.

[0088] Measurement results: The initial and final setting times of the recycled concrete powder-slag-based polymer obtained according to the proportion of components in this group are 31min and 34min respectively, the fluidity is 192mm, and the unconfined compressive strength of the test block under 28d standard curing conditions is 49.81MPa, and the flexural strength is 5.55MPa.

[0089] Example 5

[0090] This embodiment provides a recycled concrete fine powder-slag-based polymer cementitious material, comprising the following components in parts by weight:

[0091] Recycled concrete powder: 60 parts;

[0092] Blast furnace granulated slag: 40 parts;

[0093] Exciter: 26 parts;

[0094] Solvent: 40 parts;

[0095] Bacillus: 19 parts

[0096] Modified water glass modulus: 1.4;

[0097] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the recycled concrete fine powder-slag-based polymer cementitious material is the same as that in Example 1.

[0098] Measurement results: The initial and final setting times of the recycled concrete micropowder-slag-based polymer obtained according to the proportion of components in this group are 32min and 34min respectively, the fluidity is 218mm, and the unconfined compressive strength of the test block under 28d standard curing conditions is 55.78MPa, and the flexural strength is 6.14MPa.

[0099] Example 6

[0100] This embodiment provides a recycled concrete fine powder-slag-based polymer cementitious material, comprising the following components in parts by weight:

[0101] Recycled concrete powder: 70 parts;

[0102] Blast furnace granulated slag: 30 parts;

[0103] Stimulant: 21 parts;

[0104] Solvent: 44 parts;

[0105] Bacillus: 15 parts

[0106] Modified water glass modulus: 1.0;

[0107] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the recycled concrete fine powder-slag-based polymer cementitious material is the same as that in Example 1.

[0108] Measurement results: The initial and final setting times of the recycled concrete micropowder-slag-based polymer obtained according to the proportion of components in this group are 88min and 134min respectively, the fluidity is 219mm, and the unconfined compressive strength of the test block under 28d standard curing conditions is 35.27MPa, and the flexural strength is 2.64MPa.

[0109] Example 7

[0110] This embodiment provides a recycled concrete fine powder-slag-based polymer cementitious material, comprising the following components in parts by weight:

[0111] Recycled concrete powder: 60 parts;

[0112] Blast furnace granulated slag: 40 parts;

[0113] Exciter: 26 parts;

[0114] Solvent: 38 parts;

[0115] Bacillus: 19;

[0116] Modified water glass modulus: 1.6;

[0117] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the recycled concrete fine powder-slag-based polymer cementitious material is the same as that in Example 1.

[0118] Measurement results: The initial and final setting times of the recycled concrete powder-slag-based polymer obtained according to the proportion of components in this group are 40min and 47min respectively, the fluidity is 201mm, and the unconfined compressive strength of the test block under 28d standard curing conditions is 35.11MPa, and the flexural strength is 2.90MPa.

[0119] Example 8

[0120] This embodiment provides a recycled concrete fine powder-slag-based polymer cementitious material, comprising the following components in parts by weight:

[0121] Recycled concrete powder: 60 parts;

[0122] Blast furnace granulated slag: 40 parts;

[0123] Stimulant: 11 parts;

[0124] Solvent: 38 parts;

[0125] Bacillus: 19 parts

[0126] Modified water glass modulus: 1.0;

[0127] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the recycled concrete fine powder-slag-based polymer cementitious material is the same as that in Example 1.

[0128] Measurement results: The initial and final setting times of the recycled concrete powder-slag-based polymer obtained according to the proportion of components in this group are 66min and 75min respectively, the fluidity is 188mm, and the unconfined compressive strength of the test block under 28d standard curing conditions is 28.52MPa, and the flexural strength is 2.17MPa.

[0129] In summary, the weight percentage of blast furnace granulated slag should be at least higher than 30 parts, because too high a weight percentage of recycled concrete micropowder will make the geopolymer slurry lose its fluidity and make it difficult to meet the plasticity and ease of handling requirements during construction. Taking into account the economic efficiency, working performance and strength growth benefits, the weight percentage of recycled concrete micropowder is 60 parts, and the weight percentage of blast furnace granulated slag is 40 parts, which is more appropriate. When the weight percentage of the activator is 16 to 21 parts, the recycled concrete micropowder-slag-based geopolymer slurry can obtain a suitable setting time and good geopolymer slurry fluidity. The setting rate of the slurry first slows down and then speeds up with the increase of the modulus. Reducing the modulus can improve the fluidity of the geopolymer slurry, but in general, the modulus does not have a significant effect on the working performance of the slurry system.

[0130] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. For example, the steps described in the disclosure of the present invention can be performed in parallel, sequentially or in different orders, as long as the desired results of the technical solution disclosed in the present invention can be achieved, and this document does not limit this.

[0131] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. Recycled concrete powder-slag-based polymer cementitious material, characterized in that: The composition includes the following components in parts by weight: 50-80 parts of recycled concrete powder; 20-50 parts of blast furnace granulated slag; 11 to 26 parts of stimulant; 38-44 parts of solvent; Bacillus 12-19 parts; The activator is modified water glass obtained by mixing water glass solution and sodium hydroxide particles, and the modulus of the modified water glass is 1.0-1.

6.

2. The recycled concrete powder-slag-based polymer cementitious material according to claim 1, characterized in that: The bacillus is Bacillus pasteurianus; The water glass solution comprises the following components in mass fractions: 29.5-30.0% silicon dioxide, 13.5-14.0% sodium hydroxide and 56.0-56.5% water.

3. The recycled concrete powder-slag-based polymer cementitious material according to claim 2, characterized in that: The particle size of the recycled concrete powder is 0.01-120 μm, and the specific surface area is 350-450 m 2 / Kg, or density is 2.16~2.77g / cm 3 .

4. The recycled concrete powder-slag-based polymer cementitious material according to claim 3, characterized in that: The particle size of the blast furnace granulated slag is 0.01-120 μm, and the specific surface area is 400-500 m 2 / Kg, or density is 2.67~3.33g / cm 3 .

5. The recycled concrete powder-slag-based polymer cementitious material according to claim 4, characterized in that: The solvent is water, with a pH value of ≥4.5; the sodium hydroxide particles in the activator are of analytical grade, with a solid content of 95-99%.

6. The recycled concrete powder-slag-based polymer cementitious material according to claim 5, characterized in that: The modified water glass modulus is 1.

4.

7. The recycled concrete powder-slag-based polymer cementitious material according to claim 6, characterized in that: The recycled concrete powder is 60 parts, the blast furnace granulated slag is 40 parts, the activator is 21 parts, the solvent is 42 parts, and the Bacillus is 15 parts.

8. The method for preparing the recycled concrete fine powder-slag-based polymer cementitious material according to any one of claims 1 to 7, characterized in that: The specific steps include: S1. Weigh recycled concrete powder, blast furnace granulated slag, water glass solution, sodium hydroxide particles, solvent and Bacillus according to each weight portion; S2. The sodium hydroxide particles are slowly added to the water glass solution, and the addition process is continuously stirred and exothermic until completely dissolved. After the solution is stabilized, the film is cooled to room temperature to prepare an activator; S3. Stir the recycled concrete powder and blast furnace granulated slag for 3 to 5 minutes until they are evenly mixed; S4. The activator and solvent are added to the mixed powder of step S3 and stirred until the slurry is uniformly stirred; S5. Prepare a spore-forming bacteria liquid, inoculate it into the mixed slurry of step S4, and stir it again for 3 to 5 minutes until it is completely stirred and uniform, so as to obtain a recycled concrete fine powder-slag-based polymer cementitious material.

9. The method for preparing the recycled concrete fine powder-slag-based polymer cementitious material according to claim 8, characterized in that: The stirring described in steps S3, S4 and S5 has a rotation speed of 110 to 130 r / min.

10. The method for preparing the recycled concrete fine powder-slag-based polymer cementitious material according to claim 9, characterized in that: The Bacillus bacterial liquid is Bacillus pasteurianus bacterial liquid, and the urease activity of the Bacillus pasteurianus bacterial liquid is 1.6 mMurea hydrolysed / min.

Citation Information

Cited By

  • Multi-waste-based pavement patching material and preparation method thereof

    CN120463448A

  • A multi-element waste-based pavement repair material and a method of preparing the same

    CN120463448B