Aromatic sulfone polymer and polymerization method and application thereof

By adding polyhydroxyphenyl crosslinking agent to the aromatic sulfone polymer for microcrosslinking, the problem of insufficient adhesion and hardness of the coating is solved, and the coating performance with high adhesion and high hardness is achieved, and good maintenance is maintained. Appearance performance.

CN118955902APending Publication Date: 2024-11-15ZHUHAI WANTONG SPECIAL ENG PLASTICS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411166793.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In high-performance coating applications, aromatic sulfone polymers are prone to peeling due to insufficient adhesion and hardness, and the existing improvement methods are limited in effect.

Method used

By adding trace amounts of polyhydroxyphenyl crosslinking agent during the polymerization of aromatic sulfone polymers, micro-crosslinking of the molecular structure is achieved, and the hardness and adhesion of the coating are improved.

Benefits of technology

Effectively improve the coating hardness and adhesion of aromatic sulfone polymer, maintain excellent appearance performance, achieve ISO grade 0 adhesion and hardness above 3H, and the coating hardness when the crosslinked polymer content is 1.5-1.9 wt%. Balancing with appearance performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a cross-linked aromatic sulfone polymer, the aromatic sulfone polymer contains a cross-linked aromatic sulfone polymer, the cross-linking of the aromatic sulfone polymer is realized through a cross-linking agent, the cross-linked aromatic sulfone polymer accounts for 1.0-2.7 wt% based on the total weight of the aromatic sulfone polymer, and the cross-linking agent is a polyhydroxyphenyl cross-linking agent. According to the preparation method, the polyhydroxyphenyl cross-linking agent can be subjected to nucleophilic substitution cross-linking reaction with the chlorobenzene end group of the aromatic sulfone polymer through nucleophilic substitution reaction, different molecular chains are connected under the action of the cross-linking agent to form a multi-element star polymer, and excellent appearance performance can be kept while the hardness performance of the coating is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to an aromatic sulfone polymer and a polymerization method and application thereof. Background Art

[0002] Aromatic sulfone polymers are high temperature resistant transparent thermoplastic engineering plastics with outstanding thermal properties, excellent chemical resistance, outstanding high temperature creep resistance, excellent dimensional stability, extremely low smoke and toxic gas emissions, as well as superior resistance to hot water, superheated steam and good electrical properties. With the increasing perfection of the development of aromatic sulfone polymer materials, its application range is becoming wider and wider, and it is applicable in the fields of aerospace, medical and health, food, household appliances, electronic appliances, energy and chemical industry.

[0003] However, in terms of high-performance coating applications, aromatic sulfone polymers are widely used in non-stick pan coatings, household appliances, plastic machinery and other fields due to their advantages such as high temperature resistance, corrosion resistance and good safety. However, in actual use, the coating is often easy to peel off due to poor adhesion to the underlying metal or insufficient hardness of the coating itself. Researchers usually improve the coating formula to improve the coating performance, but the effect has certain limitations. Starting from the resin structure, this patent adds a trace amount of polyhydroxyphenyl crosslinking agent during the polymerization process of aromatic sulfone polymers to achieve micro-crosslinking of the molecular structure, which can effectively improve the coating performance of aromatic sulfone polymers, especially the hardness. Summary of the invention

[0004] The object of the present invention is to provide an aromatic sulfone polymer having high coating hardness, high coating adhesion and good appearance.

[0005] The present invention is achieved through the following technical solutions: A cross-linked aromatic sulfone polymer contains a cross-linked aromatic sulfone polymer. The cross-linking of the aromatic sulfone polymer is achieved by a cross-linking agent. Based on the total weight of the aromatic sulfone polymer, the cross-linked aromatic sulfone polymer accounts for 1.0-2.7wt%, wherein the cross-linking agent is a polyhydroxyphenyl cross-linking agent.

[0006] Preferably, the crosslinked aromatic sulfone polymer contains 1.5-1.9 wt % of the total weight of the crosslinked polymer.

[0007] The proportion of the cross-linked polymer is determined by gel permeation chromatography (GPC). The test method is: using polystyrene or polymethyl methacrylate as a standard, tetrahydrofuran or N, N-dimethylformamide or chloroform as a mobile phase, the polymer concentration is 0.1~10 mg / mL, and the relative molecular weight of the polymer is determined by gel permeation chromatography. The data correspondence between dwt / d(lgMw) and lgMw in the GPC (gel permeation chromatography) test data results is plotted using Origin software, where the abscissa is lgMw, the ordinate is dwt / d(lgMw), and the starting point of the ordinate is 0. According to the data integration function in the Origin software, the area SM formed by the weight-average molecular weight distribution curve and the abscissa is 1, the single peak that preferentially flows out is the peak of the cross-linked polymer, the peak area T is calculated by integration, the total area is T0, and T / T0 is the proportion of the cross-linked polymer in the total polymer chain.

[0008] The molecular weight range of the aromatic sulfone polymer is Mw=35,000-100,000.

[0009] The aromatic sulfone polymer is obtained by polymerizing a phenolic monomer and a sulfone monomer, wherein the phenolic monomer is selected from at least one of 4,4'-dihydroxydiphenyl sulfone, 4,4'-biphenol, and 2,2'-bis(4-hydroxyphenyl)propane; and the sulfone monomer is selected from at least one of 4,4'-dichlorodiphenyl sulfone, 4,4'-difluorodiphenyl sulfone, and bis-(4-chlorophenylsulfone)biphenyl.

[0010] The polyhydroxyphenyl crosslinking agent is selected from at least one of tri(4-hydroxyphenyl)methane and tetra(4-hydroxyphenyl)methane.

[0011] The polymerization method of an aromatic sulfone polymer of the present invention comprises the following steps: quantitatively adding a solvent, a phenol monomer, a sulfone monomer, a salt-forming agent and an entrainer into a reaction kettle protected by an inert gas, maintaining the temperature between 180 and 210° C. for 4 to 6 hours by a solution polycondensation method, wherein the entrainer continuously discharges reaction water by azeotropy during the reaction until no water is discharged, the salt-forming reaction is finished, and the entrainer is evaporated; after the entrainer is evaporated, the reaction system is heated to 230 to 240° C., maintained for 2 to 3 hours, a polyhydroxyphenyl crosslinking agent is added, the reaction is continued for 0.5 to 1 hour, and the polymerization reaction is finished; and stirring and heating are stopped, the polymer material is precipitated into strips in water, crushed by a crusher to obtain a powdery material, and the aromatic sulfone polymer is obtained by post-treatment.

[0012] The solvent is selected from sulfolane, the salt-forming agent is selected from at least one of sodium carbonate and potassium carbonate, the entrainer is selected from at least one of toluene and xylene, and the inert gas is selected from at least one of nitrogen and helium.

[0013] The polyhydroxyphenyl crosslinking agent is selected from at least one of tri(4-hydroxyphenyl)methane and tetra(4-hydroxyphenyl)methane.

[0014] The molar amount of the polyhydroxyphenyl crosslinking agent is 0.06-0.13 times the total molar amount of the sulfone monomers; the added amount of the solvent is 1.5-3 times the total weight of the reaction monomers; the molar amount of the salt-forming agent is 1.02-1.5 times the total molar amount of the bisphenol monomers; and the added amount of the azeotropic agent is 0.1-0.3 times the total weight of the reaction monomers.

[0015] The aromatic sulfone polymer of the present invention is used for preparing non-stick pan coating, household appliances and plastic machinery.

[0016] The present invention has the following beneficial effects: The present invention uses a polyhydroxyphenyl crosslinking agent to perform a nucleophilic substitution crosslinking reaction with the chlorophenyl end group of the aromatic sulfone polymer through a nucleophilic substitution reaction. Different molecular chains are connected under the action of the crosslinking agent to form a multi-element star polymer, which can improve the hardness performance of the coating while maintaining excellent appearance performance. DETAILED DESCRIPTION

[0017] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0018] The raw materials used in the embodiments and comparative examples of the present invention are described as follows, but are not limited to these materials: Raw materials such as 4,4'-dichlorodiphenyl sulfone, 4,4'-biphenol, 4,4'-dihydroxydiphenyl sulfone, sulfolane, toluene, potassium carbonate, tris(4-hydroxyphenyl)methane, tetrakis(4-hydroxyphenyl)methane, and trimesic acid were obtained from commercial sources.

[0019] Embodiments and Comparative Examples A polymerization method for an aromatic sulfone polymer: cyclopentane (2.0 times the total weight of the reaction monomers), phenol monomers, sulfone monomers, potassium carbonate (molar amount is 1.30 times the total molar amount of bisphenol monomers), and toluene (0.22 times the total weight of the reaction monomers) are quantitatively added into a reaction kettle protected by inert gas, and a solution polycondensation method is adopted, and the temperature is maintained at 180-210° C. for 4-6 hours. During the reaction, toluene continuously discharges reaction water through azeotropy until no water is discharged, and the salt-forming reaction is completed, and toluene is evaporated; after toluene is evaporated, the reaction system is heated to 230-240° C. ℃, keep for 2-3h, add a cross-linking agent (tris(4-hydroxyphenyl)methane, tetrakis(4-hydroxyphenyl)methane or trimesic acid, the amount is shown in the table) according to the feeding table of the examples and comparative examples, and continue the reaction for 0.5-1h (if no cross-linking agent is added, continue the reaction for 0.5-1h), and the polymerization reaction is completed; stop stirring and heating, precipitate the above polymer material into strips in water, crush it with a crusher to obtain a powdery material, and post-treat to obtain an aromatic sulfone polymer.

[0020] Various test methods: (1) Coating preparation: The aromatic sulfone polymer was dissolved in N-methylpyrrolidone (NMP) to prepare a 25 wt% polymer solution. A coating with a thickness of 10 ± 5 μm was prepared on a dry and smooth aluminum plate using a scraper. The coating was then baked in an oven at 150 °C for 1 h. The solution was then baked in a muffle furnace at 380 °C for 20 min to obtain an aromatic sulfone polymer coating.

[0021] (2) Coating adhesion test: Place the coated aluminum plate test piece on a flat plate with sufficient hardness, hold the handle of the grid cutter, and make the multi-blade cutter perpendicular to the plane of the test piece to form a grid pattern. Use 25mm wide 3M tape to stick on the entire grid, then tear it off at the minimum angle and observe the peeling of the paint film. Rating according to the following standards.

[0022] ISO grade: 0, the edges of the cut are completely smooth, and there is no peeling on the edges of the lattice.

[0023] ISO grade: 1, small flakes are peeled off at the intersection of the cuts, and the actual damage in the cross-cut area does not exceed 5%.

[0024] ISO Grade: 2, the edges and / or intersections of the cut are peeled off, with an area greater than 5% but less than 15%.

[0025] (3) Coating hardness test: Tested with a pencil hardness tester. According to standard ASTM D3363, pencils of different hardness are used to scratch the surface of the above coating multiple times at the same angle and force. The pencil hardness value that just scratches the coating is defined as the scratch resistance of the above coating.

[0026] (4) Appearance performance test: The aromatic sulfone compositions of the embodiments of the present invention and the comparative examples were injection molded at 360° C. in an injection molding machine to obtain a standard color plate with a thickness of 2 mm. The YI value of the color plate was measured according to standard ASTM E1164, and the YI value was used to compare the color depth. The smaller the YI value, the lighter the color and the higher the color grade.

[0027] The monomers used for polymer A were: 8.79 kg of 4,4'-dichlorodiphenyl sulfone and 5.59 kg (30 mol) of 4,4'-biphenyl diphenol; The monomers used for polymer B were: 8.79 kg of 4,4'-dichlorodiphenyl sulfone and 7.51 kg (30 mol) of 4,4'-dihydroxydiphenyl sulfone; Crosslinker A: tetrakis(4-hydroxyphenyl)methane; Crosslinker B: tris(4-hydroxyphenyl)methane; Cross-linking agent C: trimesic acid.

[0028] Table 1 shows the parameters of aromatic sulfone polymers: Example 1 Example 2 Example 3 Example 4 Example 5 Aromatic sulfone polymers A-1 A-2 A-3 A-4 A-5 Tetrakis(4-hydroxyphenyl)methane, mol 1.8 2.4 3 3.9 Tris(4-hydroxyphenyl)methane, mol 2.5 Trimesic acid, mol Weight average molecular weight, 10,000 6.3 6.0 6.4 6.2 6.2 Cross-linked polymer, wt% 1.03 1.51 1.89 2.66 1.60 ISO Grade 0 0 0 0 0 hardness 3H 3H 4H 4H 4H YI 23.3 23.5 24.0 24.4 23.8 Table 1 continued: Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Aromatic sulfone polymers A-6 A-7 A-8 A-9 Tetrakis(4-hydroxyphenyl)methane, mol 0 1.2 4.5 Tris(4-hydroxyphenyl)methane, mol Trimesic acid, mol 1.5 Weight average molecular weight, 10,000 6.5 6.1 6.4 5.9 Cross-linked polymer, wt% 0 0.57 3.28 2.41 ISO Grade 1 1 0 1 hardness H 2H 4H 4H YI 22.5 23.1 26.6 28.7 Table 1 continued: Example 6 Example 7 Example 8 Example 9 Example 10 Aromatic sulfone polymers B-1 B-2 B-3 B-4 B-5 Tetrakis(4-hydroxyphenyl)methane, mol 1.8 2.4 3 3.9 Tris(4-hydroxyphenyl)methane, mol 2.4 Trimesic acid, mol Weight average molecular weight, 10,000 6.3 6.0 6.4 6.1 6.3 Cross-linked polymer, wt% 1.08 1.55 1.90 2.62 1.57 ISO Grade 0 0 0 0 0 hardness 3H 3H 4H 4H 3H YI 23.1 23.4 23.8 24.2 23.5 It can be seen from Examples 1-4 / 6-9 that the adhesion between the cross-linked aromatic sulfone polymer of the present application and the coating can reach the level of ISO grade 0, the hardness reaches above 3H, and the YI value is less than 24.4. As the content of the cross-linked polymer increases, the hardness of the coating increases and the appearance of the polymer decreases. Preferably, when the cross-linked material in the cross-linked aromatic sulfone polymer accounts for 1.5-1.9wt% of the total weight, the hardness of the coating and the appearance performance of the polymer are balanced.

[0029] Table 1 continued: Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Aromatic sulfone polymers B-5 B-6 B-7 B-8 Tetrakis(4-hydroxyphenyl)methane, mol 0 1.2 4.5 Tris(4-hydroxyphenyl)methane, mol Trimesic acid, mol 1.5 Weight average molecular weight, 10,000 6.5 6.2 6.4 6.1 Cross-linked polymer, wt% 0 0.66 3.46 2.39 ISO Grade 1 1 0 1 hardness H 2H 4H 4H YI 22.9 23.0 27.5 28.5 It can be seen from Comparative Examples 1 / 2 / 5 / 6 that when there is no crosslinking or the crosslinking is low, the hardness of the coating is low, and the adhesion between the crosslinked aromatic sulfone polymer and the coating is poor.

[0030] It can be seen from Comparative Example 3 / 7 that if the content of the cross-linked polymer is too high, the polymer surface appearance is poor.

[0031] It can be seen from Comparative Example 4 / 8 that even if trimesic acid is used to make the cross-linked polymer reach the scope of the present invention, the aromatic sulfone polymer has poor adhesion to the coating and the appearance of the aromatic sulfone polymer is not good, probably because the bonding force between the carboxyl group of trimesic acid and the coating is far weaker than that between the carboxyl group and the coating.

Claims

1. A cross-linked aromatic sulfone polymer, characterized in that The aromatic sulfone polymer contains a cross-linked aromatic sulfone polymer, which is cross-linked by a cross-linking agent. Based on the total weight of the aromatic sulfone polymer, the cross-linked aromatic sulfone polymer accounts for 1.0-2.7wt%, wherein the cross-linking agent is a polyhydroxyphenyl cross-linking agent.

2. The crosslinked aromatic sulfone polymer according to claim 1, characterized in that The crosslinked aromatic sulfone polymer contains 1.5-1.9 wt% of the total weight of the crosslinked polymer.

3. The crosslinked aromatic sulfone polymer according to claim 1, characterized in that The molecular weight range of the aromatic sulfone polymer is Mw=35,000-100,000.

4. The crosslinked aromatic sulfone polymer according to claim 1, characterized in that The aromatic sulfone polymer is obtained by polymerizing a phenolic monomer and a sulfone monomer, wherein the phenolic monomer is selected from at least one of 4,4'-dihydroxydiphenyl sulfone, 4,4'-biphenol, and 2,2'-bis(4-hydroxyphenyl)propane; and the sulfone monomer is selected from at least one of 4,4'-dichlorodiphenyl sulfone, 4,4'-difluorodiphenyl sulfone, and bis-(4-chlorophenylsulfone)biphenyl.

5. The crosslinked aromatic sulfone polymer according to claim 1, characterized in that The polyhydroxyphenyl crosslinking agent is selected from at least one of tri(4-hydroxyphenyl)methane and tetra(4-hydroxyphenyl)methane.

6. The method for polymerizing an aromatic sulfone polymer according to any one of claims 1 to 5, characterized in that: The following steps are involved: A solvent, a phenol monomer, a sulfone monomer, a salt-forming agent and an entrainer are quantitatively added into a reaction kettle protected by an inert gas, and the temperature is maintained at 180-210° C. for 4-6 hours by a solution polycondensation method. During the reaction, the entrainer continuously discharges reaction water by azeotropy until no water is discharged, and the salt-forming reaction is completed, and the entrainer is evaporated; after the entrainer is evaporated, the reaction system is heated to 230-240° C., maintained for 2-3 hours, and a polyhydroxyphenyl crosslinking agent is added, and the reaction is continued for 0.5-1 hour, and the polymerization reaction is completed; stirring and heating are stopped, and the above polymer material is precipitated into strips in water, which are crushed by a crusher to obtain a powdery material, and an aromatic sulfone polymer is obtained by post-treatment.

7. The method for polymerizing an aromatic sulfone polymer according to claim 6, characterized in that: The solvent is selected from sulfolane, the salt-forming agent is selected from at least one of sodium carbonate and potassium carbonate, the entrainer is selected from at least one of toluene and xylene, and the inert gas is selected from at least one of nitrogen and helium.

8. The method for polymerizing an aromatic sulfone polymer according to claim 6, characterized in that: The polyhydroxyphenyl crosslinking agent is selected from at least one of tri(4-hydroxyphenyl)methane and tetra(4-hydroxyphenyl)methane.

9. The method for polymerizing an aromatic sulfone polymer according to claim 6, characterized in that: The molar amount of the polyhydroxyphenyl crosslinking agent is 0.06-0.13 times the total molar amount of the sulfone monomers; the added amount of the solvent is 1.5-3 times the total weight of the reaction monomers; the molar amount of the salt-forming agent is 1.02-1.5 times the total molar amount of the bisphenol monomers; and the added amount of the entrainer is 0.1-0.3 times the total weight of the reaction monomers.

10. Use of the aromatic sulfone polymer according to any one of claims 1 to 5, characterized in that: Used for preparing non-stick coatings for pans, household appliances, and plastic machinery.