Waterproof anti-static optical polyester film
Through the multi-layer optical polyester film, combined with SiO2@PMMA nanoparticles and specific resin materials, the problem of insufficient thickness of anti-fouling and waterproof and anti-static layers is solved, and efficient waterproof and anti-static effects are achieved, reducing costs and improving Mechanical properties.
Patent Information
- Application Number
- CN202411010669.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The existing anti-fouling and waterproof optical polyester film has disadvantages in terms of slow curing speed and high viscosity of coated resin. The thickness of the anti-static layer coating is low, resulting in too fast anti-static effect failure, increasing cost and processing difficulty.
Waterproof and anti-static optical polyester film with a multi-layer structure, including a surface roughness layer, a waterproof layer, an anti-static layer and a PET layer. Through specific nanoparticles and resin combinations, SiO2@PMMA nanoparticles and polyglycidine methacrylic acid Materials such as ester and aminosiloxane improve waterproof and anti-static properties, and form an anti-static layer with suitable thickness through ultraviolet irradiation and oven drying.
It improves the waterproof effect and anti-static properties of the optical polyester film, reduces the electrostatic marks and dust adsorption, reduces the dependence on the electrostatic device, reduces production costs, and improves mechanical wear resistance and light transmittance.
Smart Images

Figure CN118955983A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of screen polyester films and relates to a waterproof and antistatic optical polyester film. Background Art
[0002] Liquid crystal display devices (LCD) are the mainstream products in the current flat panel display market. They have the advantages of low operating voltage, low power consumption, high resolution, mature large-scale production technology, and low cost. As the price continues to fall, the application field of the product is rapidly expanding. As the light source provider of the entire LCD display device, the performance of the backlight module will directly affect the display quality of the display. As the key component of the backlight module, the optical film has waterproof and anti-static properties, which are also key properties for shaping good display quality. Since the moisture-proof performance of the optical polyester film is moderate, in humid weather, in addition to using protective film to wrap and placing desiccant to make the optical polyester film waterproof and waterproof, it is also important to give the optical polyester film its own waterproof and moisture-proof properties. In addition, in order to prevent static electricity from affecting the optical polyester film during transportation and deep processing, such as adsorbing fine dust and generating static lines, which affect product quality, it is unnecessary to install static rods, static ropes and other devices during the production process, and directly give the optical polyester film itself anti-static effect to achieve the effect of reducing costs.
[0003] In recent years, researchers have developed optical diffusion films with waterproof properties. For example, patent CN201910974777.0 mentions an optical diffusion film with anti-fouling and waterproof properties. This optical diffusion film can retain the original optical properties of the diffusion film after adding modified resin, and has anti-fouling and waterproof effects; in addition, patent CN202221764272.5 also involves an anti-static optical film, which has a good anti-static effect through an anti-static layer made of epoxy resin material.
[0004] The existing optical polyester films with anti-fouling and waterproof properties have disadvantages in slow curing speed and high viscosity of the coated resin. In addition, the antistatic layer is an antistatic agent coated online, and the coating thickness is relatively low. After the subsequent stretching and slitting process, the surface resistance value is high, and the antistatic effect loses its effect too quickly, which affects the downstream processing and molding, and the installation of antistatic devices increases costs. Summary of the invention
[0005] The purpose of the present invention is to solve the defects of the prior art and provide a waterproof and antistatic optical polyester film. The invention can improve the waterproof effect of the optical polyester film while enhancing the antistatic effect, reduce the possible quality impact of the product during transportation and deep processing, such as water stains, adsorption of fine dust, generation of static lines, etc., eliminate the need to install devices such as static rods and static ropes during the production process, and directly give the optical polyester film itself a waterproof and antistatic effect, thereby reducing costs.
[0006] The present invention provides a waterproof and antistatic optical polyester film, comprising a rough surface layer, a waterproof layer, an antistatic layer, and a PET layer; the PET layer is coated with antistatic layers on the top and bottom. The waterproof and antistatic optical polyester film is a layered structure, and the order of stacking from top to bottom is the rough surface layer, the waterproof layer, the first antistatic layer, the PET layer, and the second antistatic layer. The waterproof layer is placed between the rough surface layer and the antistatic layer, and the antistatic layer is placed between the waterproof layer and the PET layer and at the lower end of the PET layer.
[0007] In some specific embodiments, the waterproof and antistatic optical polyester film is a layered structure, which includes a surface roughness layer, a waterproof layer, a first antistatic layer, a PET layer, and a second antistatic layer from top to bottom;
[0008] The surface rough layer is composed of SiO2@PMMA nanoparticles and water-based polyacrylate latex;
[0009] The waterproof layer is composed of polyglycidyl methacrylate and aminosiloxane;
[0010] The first antistatic layer and the second antistatic layer are composed of hydrolyzed 3-glycidyloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane and ITO nanoparticles.
[0011] In some preferred embodiments, the weight ratio of the SiO2@PMMA nanoparticles to the aqueous polyacrylate latex is 0.5:1.
[0012] In some preferred embodiments, the weight ratio of polyglycidyl methacrylate to aminosilicone is 2:1.
[0013] In some preferred embodiments, the weight ratio of the hydrolyzed 3-glycidyloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and ITO nanoparticles is 2:3:2.5.
[0014] Another aspect of the present invention further provides a method for preparing any of the above-mentioned waterproof and antistatic optical polyester films, comprising the following steps:
[0015] 1) Coat the antistatic coating on both sides of the PET layer with a coating thickness of 2-3μm, and then place it at 700mW / cm 2 The layers are cured under ultraviolet light of 1000 W for 10 seconds to form a first antistatic layer and a second antistatic layer;
[0016] 2) coating a waterproof layer coating on the first antistatic layer with a coating thickness of 1-2 μm, and then placing in an oven and drying at 100° C. for 20 seconds to form the waterproof layer;
[0017] 3) coating a surface rough layer coating on the waterproof layer with a coating thickness of 2-3 μm, and baking in an oven at 60° C. for 20 minutes to form the surface rough layer; and then performing corona or primer treatment on the surface rough layer to finally obtain the waterproof and antistatic optical polyester film.
[0018] Wherein, the preparation method of the antistatic layer coating is:
[0019] A total of 5 parts by weight of hydrolyzed 3-glycidyloxypropyltrimethoxysilane (GPTS) and 3-methacryloxypropyltrimethoxysilane (MPTS) were added to 10 parts by weight of a 25 wt.% ITO nanoparticle ethanol solution, and ultrasonically mixed for 30 minutes at a power of 100 W.
[0020] More preferably, 2 parts by weight of hydrolyzed 3-glycidoxypropyltrimethoxysilane and 3 parts by weight of 3-methacryloxypropyltrimethoxysilane.
[0021] Wherein, the preparation method of the waterproof layer coating is:
[0022] 1-2 parts of aminosiloxane (amino-POSS) and 1-2 parts of polyglycidyl methacrylate (PGMA) powder are added into 10 parts by weight of DMF solvent, and the mixture is vigorously stirred for 2 hours at room temperature to obtain the waterproof layer coating.
[0023] More preferably, the weight ratio of aminosilicone to polyglycidyl methacrylate powder is 1:2.
[0024] Further preferably, the preparation method of the PGMA powder is:
[0025] 1 wt% azobisisobutyronitrile (AIBN) and 1 part by weight of glycidyl methacrylate (GMA) were dissolved in 2 parts by weight of anhydrous dibutyl ketone and stirred at 70° C. for 5 hours; after removing excess solvent by rotary evaporation, the solution was immersed in 10 parts by weight of methanol and dried in a vacuum oven overnight to obtain the PGMA powder.
[0026] Wherein, the preparation method of the surface rough layer coating is:
[0027] Disperse 4 parts by weight of modified SiO2 nanoparticles in xylene, then add 0.4 parts by weight of dibenzoyl peroxide, heat to 40°C, and mechanically stir for at least 30 minutes under a nitrogen atmosphere; heat the above mixture to 80°C and continue stirring, and drop 40 parts by weight of methyl acrylate; quench in an ice bath after 1 hour to stop polymerization; the product is purified by centrifugal precipitation at 8000r / min, and vacuum dried at 60°C for 12 hours to obtain SiO2@PMMA nanoparticles; reflux the SiO2@PMMA nanoparticles with acetone for 72 hours, and then dry under vacuum for 6 hours to obtain SiO2@PMMA nanoparticles; stir and mix the obtained SiO2@PMMA nanoparticles with water-based polyacrylate latex at a mass ratio of 0.5 to obtain the surface roughening layer coating.
[0028] More preferably, the amount of xylene used is 30-40 ml per gram of SiO2 nanoparticles.
[0029] The present invention has the following beneficial effects:
[0030] The waterproof and antistatic optical polyester film of the present invention has a multilayer structure. Among them, the surface rough layer has the characteristics of a large adjustable range of haze, high light transmittance, and good appearance quality, and with good mechanical wear resistance and high toughness, it effectively avoids relative friction of the optical film during stacking and transportation; the waterproof layer has excellent curing speed and low viscosity, and has excellent surface properties in terms of hydrophobicity, antifouling and transparency; the double electrostatic coating effectively solves the problems of low thickness of the online antistatic coating and increased surface resistance after the biaxial stretching process, and has good bonding performance, and has no effect on the downstream preparation of the prism structure-containing light-enhancing film, and effectively reduces product quality problems caused by the adsorption of tiny particles and the generation of electrostatic lines, and can also avoid the cost problem caused by installing electrostatic rods, electrostatic ropes and other electrostatic removal devices during the production process, thereby achieving the effect of reducing costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram showing the layered structure of the waterproof and antistatic optical polyester film of the present invention. DETAILED DESCRIPTION
[0032] In order to further understand the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0033] The waterproof and antistatic optical polyester film of the present invention comprises a surface roughness layer, a waterproof layer, an antistatic layer, and a PET layer. Figure 1As shown, the waterproof and antistatic optical polyester film includes a surface roughness layer 1, a waterproof layer 2, a PET layer 3, and an antistatic layer 4; wherein the antistatic layer 4 includes a first antistatic layer and a second antistatic layer, which are respectively coated on both sides of the PET layer 3.
[0034] The rough surface layer 1 is located on the waterproof layer 2. The rough surface layer 1 is a resin containing particles such as PMMA, and its surface is treated with corona or primer to increase surface adhesion.
[0035] The waterproof layer 2 is placed between the rough surface layer 1 and the first antistatic layer 3 and is a transparent waterproof coating composed of a mixture of aminosilicone and polyglycidyl methacrylate powder and DMF solution.
[0036] The PET layer 3 is a transparent optical material made of polyethylene terephthalate.
[0037] The antistatic layer 4 is placed between the waterproof layer and the PET layer and at the lower end of the PET layer; the antistatic layer 4 is a mixture of transparent conductive inorganic matter and resin; wherein the transparent conductive inorganic matter can be selected from ITO nanoparticles made from tin powder, silver powder, etc.
[0038] Example 1
[0039] 1) Preparation of antistatic coating:
[0040] In 10 parts by weight of an ITO nanoparticle ethanol solution with a concentration of 25 wt.%, 2 parts by weight of hydrolyzed 3-glycidyloxypropyltrimethoxysilane (GPTS) and 3 parts by weight of 3-methacryloxypropyltrimethoxysilane (MPTS) were added, and the mixture was mixed uniformly by ultrasonication at a power of 100 W for 30 min.
[0041] 2) Preparation of waterproof coating:
[0042] 1 wt% azobisisobutyronitrile (AIBN) and 1 part by weight of glycidyl methacrylate (GMA) were dissolved in 2 parts by weight of anhydrous dibutyl ketone and stirred at 70° C. for 5 hours; after removing excess solvent by rotary evaporation, the solution was immersed in 10 parts by weight of methanol and dried in a vacuum oven overnight to obtain the polyglycidyl methacrylate (PGMA) powder.
[0043] 1 part of aminosiloxane (amino-POSS) and 2 parts of PGMA powder were added into 10 parts by weight of DMF solvent, and stirred vigorously at room temperature for 2 hours to obtain the waterproof layer coating.
[0044] 3) Preparation of surface rough layer coating:
[0045] About 4 parts by weight of modified SiO2 nanoparticles are dispersed in xylene (40 ml per gram of SiO2 nanoparticles) using ultrasound, and then 0.4 parts by weight of dibenzoyl peroxide is added, heated to 40°C, and mechanically stirred for at least 30 minutes in a nitrogen atmosphere; the above mixture is heated to 80°C and stirred continuously, and 40 parts by weight of methyl acrylate is dropped; after 1 hour, the polymerization is stopped by quenching in an ice bath; the product is purified by repeated centrifugal precipitation at 8000 r / min, and after vacuum drying at 60°C for 12 hours, a crude SiO2@PMMA nanoparticle is obtained; the crude SiO2@PMMA nanoparticle is refluxed with acetone for 72 hours to ensure that the homopolymer is completely removed, and then dried under vacuum for 6 hours to obtain SiO2@PMMA nanoparticles; the obtained SiO2@PMMA nanoparticles are stirred and mixed with water-based polyacrylate latex at a mass ratio of 0.5 to obtain the waterproof layer coating.
[0046] 5) Coat the antistatic coating on both sides of the PET layer with a coating thickness of 2-3μm, and then place it at 700mW / cm 2 The layers are cured under ultraviolet light of 1000 W for 10 seconds to form a first antistatic layer and a second antistatic layer;
[0047] 6) coating a waterproof layer coating on the first antistatic layer with a coating thickness of 1-2 μm, and then placing in an oven and drying at 100° C. for 20 seconds to form the waterproof layer;
[0048] 7) coating a surface rough layer coating on the waterproof layer with a coating thickness of 2-3 μm, and baking in an oven at 60° C. for 20 minutes to form the surface rough layer; and then performing corona treatment on the surface rough layer to finally obtain the waterproof and antistatic optical polyester film.
[0049] Example 2
[0050] Referring to the preparation method of the waterproof coating in Example 1, the feeding amount of amino-POSS and PGMA powder was adjusted, and the viscosity and the shortest curing time required in an oven at 100° C. were tested. When the feeding weight ratio of amino-POSS to PGMA powder was 1:2, the viscosity was higher and the curing time was the shortest.
[0051] Table 1
[0052]
[0053] Example 3
[0054] Referring to the preparation method of the antistatic layer coating in Example 1, the concentration of ITO nanoparticles, the amount of GPTS and MPTS were adjusted, and the surface resistance of the prepared waterproof and antistatic optical polyester film was tested. When the weight ratio of GPTS to MPTS was 2:3, the resistance of the prepared waterproof and antistatic optical polyester film was the lowest.
[0055] Table 2
[0056]
[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For the technical personnel in this field, the present invention can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made to the present invention should be included in the protection scope of the present invention.
Claims
1. A waterproof and antistatic optical polyester film, characterized in that: The waterproof and antistatic optical polyester film is a layered structure, which includes a surface roughness layer, a waterproof layer, a first antistatic layer, a PET layer, and a second antistatic layer from top to bottom; The surface rough layer is composed of SiO2@PMMA nanoparticles and water-based polyacrylate latex; The waterproof layer is composed of polyglycidyl methacrylate and aminosiloxane; The first antistatic layer and the second antistatic layer are composed of hydrolyzed 3-glycidyloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane and ITO nanoparticles.
2. The waterproof and antistatic optical polyester film according to claim 1, characterized in that: The weight ratio of the SiO2@PMMA nanoparticles to the aqueous polyacrylate latex is 0.5:
1.
3. The waterproof and antistatic optical polyester film according to claim 1, characterized in that: The weight ratio of polyglycidyl methacrylate to aminosiloxane is 2:
1.
4. The waterproof and antistatic optical polyester film according to claim 1, characterized in that: The weight ratio of the hydrolyzed 3-glycidyloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane and ITO nanoparticles is 2:3:2.
5.
5. A method for preparing the waterproof and antistatic optical polyester film according to any one of claims 1 to 4, characterized in that: The following steps are involved: 1) Coat the antistatic coating on both sides of the PET layer with a coating thickness of 2-3μm, and then place it at 700mW / cm 2 The layers are cured under ultraviolet light of 1000 W for 10 seconds to form a first antistatic layer and a second antistatic layer; 2) coating a waterproof layer coating on the first antistatic layer with a coating thickness of 1-2 μm, and then placing in an oven and drying at 100° C. for 20 seconds to form the waterproof layer; 3) coating a surface rough layer coating on the waterproof layer with a coating thickness of 2-3 μm, and baking in an oven at 60° C. for 20 minutes to form the surface rough layer; and then performing corona or primer treatment on the surface rough layer to finally obtain the waterproof and antistatic optical polyester film.
6. The preparation method according to claim 5, characterized in that: The preparation method of the antistatic layer coating is: In 10 parts by weight of a 25wt.% ITO nanoparticle ethanol solution, a total of 5 parts by weight of hydrolyzed 3-glycidyloxypropyltrimethoxysilane and 3-methacryloxypropyltrimethoxysilane are added, and ultrasonic mixing is performed at a power of 100 W for 30 minutes; more preferably, 2 parts by weight of hydrolyzed 3-glycidyloxypropyltrimethoxysilane and 3 parts by weight of 3-methacryloxypropyltrimethoxysilane are added.
7. The preparation method according to claim 5, characterized in that: The preparation method of the waterproof layer coating is: 1-2 parts of aminosilicone and 1-2 parts of polyglycidyl methacrylate powder are added to 10 parts by weight of DMF solvent, and vigorously stirred for 2 hours at room temperature to obtain the waterproof layer coating; more preferably, the weight ratio of aminosilicone to polyglycidyl methacrylate powder is 1:
2.
8. The preparation method according to claim 7, characterized in that: The preparation method of the polyglycidyl methacrylate powder is: 1 wt% of azobisisobutyronitrile and 1 part by weight of glycidyl methacrylate are dissolved in 2 parts by weight of anhydrous dibutyl ketone and stirred at 70° C. for 5 hours; after removing excess solvent by rotary evaporation, the solution is immersed in 10 parts by weight of methanol and dried in a vacuum oven overnight to obtain the polyglycidyl methacrylate powder.
9. The preparation method according to claim 5, characterized in that: The preparation method of the surface rough layer coating is: Disperse 4 parts by weight of modified SiO2 nanoparticles in xylene, then add 0.4 parts by weight of dibenzoyl peroxide, heat to 40°C, and mechanically stir for at least 30 minutes under a nitrogen atmosphere; heat the above mixture to 80°C and continue stirring, and drop 40 parts by weight of methyl acrylate; quench in an ice bath after 1 hour to stop polymerization; the product is purified by centrifugal precipitation at 8000r / min, and vacuum dried at 60°C for 12 hours to obtain SiO2@PMMA nanoparticles; reflux the SiO2@PMMA nanoparticles with acetone for 72 hours, and then dry under vacuum for 6 hours to obtain SiO2@PMMA nanoparticles; stir and mix the obtained SiO2@PMMA nanoparticles with water-based polyacrylate latex at a mass ratio of 0.5 to obtain the surface roughening layer coating.
10. The preparation method according to claim 9, characterized in that: The amount of xylene used is 30-40 ml per gram of SiO2 nanoparticles.