Heat treatment process method for bearing part made of 40Cr15Mo2VN material
By employing vacuum heating, cooling, and multiple cold treatment processes on 40Cr15Mo2VN material, the wear resistance and corrosion resistance issues of thick-walled bearing parts in high humidity and high salt spray environments were resolved. This achieved uniform hardness and structural stability, meeting the requirements for use in harsh environments.
Patent Information
- Application Number
- CN202411360579.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-15
AI Technical Summary
Existing high-carbon chromium stainless bearing steel has limited corrosion resistance in high humidity and high salt spray marine environments, uneven carbide structure, low contact fatigue strength, and cannot meet heat treatment process requirements when the wall thickness of bearing parts is increased.
Using 40Cr15Mo2VN material, the temperature is gradually increased and held in a vacuum furnace, combined with vacuum air quenching and vacuum oil quenching, increasing the number of cold treatment steps and tempering times, and optimizing the cooling and tempering temperatures to ensure the uniformity of hardness and the stability of the microstructure of the bearing parts.
It improves the wear resistance and corrosion resistance of bearing parts in high humidity and high salt spray environments, ensuring a hardness of 58-58.5 HRC, and meeting the process requirements of thick-walled bearing parts.
Smart Images

Figure CN118957241A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of heat treatment processing of bearing parts, and specifically relates to a heat treatment process method for bearing parts made of 40Cr15Mo2VN material. Background Art
[0002] In many industrial environments, especially in high humidity and heat environments and marine high salt spray environments, stainless steel bearings with high wear resistance and corrosion resistance are required. In the past, high carbon chromium stainless bearing steel G95Cr18 or G102Cr18Mo was selected. After heat treatment, the hardness of the material is required to be ≥58HRC. Due to the high carbon content of high carbon chromium stainless bearing steel, there are several disadvantages: 1. The corrosion resistance is limited, especially in salt spray environments; 2. The carbide structure is coarse and unevenly distributed; 3. The contact fatigue strength of the material is low and the material's spalling sensitivity increases after long-term use.
[0003] In order to improve the service life of bearings in special environments, a high nitrogen martensitic stainless steel 40Cr15Mo2VN is now used to process bearing parts, which include: bearing outer ring, bearing inner ring, and rolling element. Since nitrogen is added to the steel to enhance the strength and corrosion resistance of the material, and after a special heat treatment process, the bearing parts have high wear resistance and high corrosion resistance, meeting the harsh working environment.
[0004] In the past, the effective wall thickness of bearing parts made of 40Cr15Mo2VN material was less than 10mm. After special heat treatment process, the hardness can reach 58~58.5HRC, which can meet the use requirements. With the expansion of the use range of this material, the outer dimensions of bearing parts are also increasing. The effective wall thickness of bearing parts is generally between 10 and 20mm. The original heat treatment process cannot meet the process requirements. A new special heat treatment process method is needed to solve the product quality problem. Summary of the invention
[0005] The purpose of the present invention is to solve the above-mentioned technical problems and to provide a heat treatment process for bearing parts made of 40Cr15Mo2VN material.
[0006] A heat treatment process for bearing parts made of 40Cr15Mo2VN material is implemented by the following steps:
[0007] 1. Quenching heating and cooling:
[0008] The bearing parts of the 40Cr15Mo2VN material to be processed are pre-cleaned, then placed in a vacuum heating furnace, evacuated to a vacuum degree of 5-10Pa, heated from room temperature to 650°C at a rate of 2-6°C / min and kept warm for 50-70min, then heated to 850°C at a rate of 5-9°C / min and kept warm for 50-70min, then heated to 1060°C at a rate of 8-12°C / min and kept warm for 60-80min, to obtain the heated bearing parts, and then taken out of the furnace after cooling;
[0009] 2. Cold treatment and tempering:
[0010] The bearing parts taken out of the furnace are placed in a cold treatment device and cold treated at -80 to -120°C for 2 to 4 hours to complete the first cold treatment; after the bearing parts return to room temperature, they are kept at 160 to 180°C for 3 to 4 hours to complete the first tempering treatment; after the bearing parts are cooled to room temperature, they are placed in a cold treatment device and cold treated at -80 to -120°C for 2 to 4 hours to complete the second cold treatment; after the bearing parts return to room temperature, they are kept at 160 to 180°C for 3 to 4 hours to complete the second tempering treatment;
[0011] 3. Hardness and structure inspection:
[0012] After the second tempering treatment is completed, the hardness and metallographic structure of the bearing parts are inspected. If they are qualified, the heat treatment process method of the bearing parts made of 40Cr15Mo2VN material is completed.
[0013] In step 1, the bearing parts of 40Cr15Mo2VN material to be processed are pre-cleaned: the bearing parts to be processed are placed on the tooling according to the process requirements and enter the pre-cleaning station, which is divided into cleaning agent cleaning and clean water cleaning; the cleaning agent cleaning temperature is 50-80°C, and the cleaning time for each step is 6-10min; the clean water cleaning temperature is 50-80°C, and the cleaning time is 6-8min; after cleaning, drying is carried out, the drying temperature is 110-130°C, and the drying time is 6-10min.
[0014] Furthermore, the cooling in step 1 is vacuum air quenching or vacuum oil quenching.
[0015] Furthermore, the vacuum quenching: after heating, the bearing parts are cooled by high-pressure nitrogen at 7 to 10 bar, and the cooling time is 15 to 25 minutes.
[0016] Furthermore, the vacuum oil quenching: after heating, the bearing parts are immersed in vacuum quenching oil for sufficient cooling, the oil temperature is 60-100° C., and the cooling time is 10-15 minutes.
[0017] Furthermore, after the vacuum oil quenching is completed, it is transported to the cleaning machine for immersion cleaning, with a total of three stations:
[0018] 1. Ultrasonic cleaning, frequency 28-30KHZ, water temperature 45-55℃;
[0019] 2. Foaming cleaning, water temperature 45 ~ 55 ℃;
[0020] 3. Alkaline water cleaning, water temperature 48 ~ 52 ℃, the alkaline water station uses 0.5 ~ 0.8% concentration of sodium nitrite aqueous solution for rust prevention; after cleaning, dry at 120 ~ 160 ℃ for 5 ~ 10 minutes.
[0021] Compared with the existing technology, the present invention has the following advantages:
[0022] ① The present invention changes the temperature rise curve of the vacuum heating furnace, increases the heat preservation in the 650°C interval, and reduces the heating rates in the three heating intervals, thereby ensuring that the bearing parts with a wall thickness of 10 to 20 mm are fully heated under vacuum and that the internal structure is completely austenitized.
[0023] ② The present invention uses vacuum air cooling equipment for processing. During cooling, the pressure of high-pressure nitrogen is increased, which accelerates the cooling speed of bearing parts with a wall thickness of 10 to 20 mm during air cooling, ensuring that the hardness of the bearing during air quenching meets the process requirements and has good hardness uniformity.
[0024] ③ The present invention adds a vacuum oil cooling equipment processing technology. During cooling, a special quenching oil for bearings is used to control the oil temperature, so that the oil cooling of bearing parts with a wall thickness of 10 to 20 mm is more uniform, ensuring that the bearing hardness during oil cooling meets the process requirements and has good hardness uniformity.
[0025] ④ The present invention reduces the cold treatment temperature and prolongs the cold treatment time, so that the residual austenite in the structure of the bearing parts with a wall thickness of 10 to 20 mm after quenching can be fully transformed.
[0026] ⑤ The present invention adopts a double cold treatment process, adding a secondary cold treatment after the first tempering, so as to obtain a more stable martensitic structure and make the residual austenite further transformed and stabilized.
[0027] The invention is applicable to the heat treatment process of bearing parts made of 40Cr15Mo2VN material. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a 500-fold microstructure diagram of the metallographic structure of the bearing part made of 40Cr15Mo2VN material after quenching and tempering in Example 1. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.
[0030] Specific implementation method 1: This implementation method is a heat treatment process for bearing parts made of 40Cr15Mo2VN material, which is implemented by the following steps:
[0031] 1. Quenching heating and cooling:
[0032] The bearing parts of the 40Cr15Mo2VN material to be processed are pre-cleaned, then placed in a vacuum heating furnace, evacuated to a vacuum degree of 5-10Pa, heated from room temperature to 650°C at a rate of 2-6°C / min and kept warm for 50-70min, then heated to 850°C at a rate of 5-9°C / min and kept warm for 50-70min, then heated to 1060°C at a rate of 8-12°C / min and kept warm for 60-80min, to obtain the heated bearing parts, and then taken out of the furnace after cooling;
[0033] 2. Cold treatment and tempering:
[0034] The bearing parts taken out of the furnace are placed in a cold treatment device and cold treated at -80 to -120°C for 2 to 4 hours to complete the first cold treatment; after the bearing parts return to room temperature, they are kept at 160 to 180°C for 3 to 4 hours to complete the first tempering treatment; after the bearing parts are cooled to room temperature, they are placed in a cold treatment device and cold treated at -80 to -120°C for 2 to 4 hours to complete the second cold treatment; after the bearing parts return to room temperature, they are kept at 160 to 180°C for 3 to 4 hours to complete the second tempering treatment;
[0035] 3. Hardness and structure inspection:
[0036] After the second tempering treatment is completed, the hardness and metallographic structure of the bearing parts are inspected. If they are qualified, the heat treatment process method of the bearing parts made of 40Cr15Mo2VN material is completed.
[0037] In step 1 of this embodiment, the bearing parts to be processed are pre-cleaned to remove impurities such as cutting fluid, dust, oil and the like remaining on the bearing surface, so as to ensure that the appearance color of the bearing parts after quenching and tempering is consistent.
[0038] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the bearing parts of the 40Cr15Mo2VN material to be processed in step 1 are pre-cleaned: the bearing parts to be processed are placed on the tooling according to the process requirements and enter the pre-cleaning station, which is divided into cleaning agent cleaning and water cleaning; the cleaning agent cleaning temperature is 50-80°C, and the cleaning time for each step is 6-10 minutes; the water cleaning temperature is 50-80°C, and the cleaning time is 6-8 minutes; after cleaning, drying is performed, the drying temperature is 110-130°C, and the drying time is 6-10 minutes. Other steps and parameters are the same as those of specific implementation method 1.
[0039] Specific implementation method three: This implementation method is different from specific implementation method one in that, in step one, the vacuum is evacuated to a vacuum degree of 8 Pa, the temperature is raised from room temperature to 650°C at a rate of 3°C / min and kept at that temperature for 60 min, then the temperature is raised to 850°C at a rate of 5°C / min and kept at that temperature for 60 min, and then the temperature is raised to 1060°C at a rate of 10°C / min and kept at that temperature for 70 min. The other steps and parameters are the same as those in specific implementation method one.
[0040] Specific implementation method 4: This implementation method is different from specific implementation method 1 in that the cooling in step 1 is vacuum air quenching or vacuum oil quenching. The other steps and parameters are the same as those in specific implementation method 1.
[0041] Specific implementation method 5: This implementation method is different from specific implementation method 4 in that the vacuum gas quenching: the heated bearing parts are cooled by high-pressure nitrogen gas of 7 to 10 bar, and the cooling time is 15 to 25 minutes. The other steps and parameters are the same as those of specific implementation method 4.
[0042] Specific implementation method 6: This implementation method is different from specific implementation method 4 in that the vacuum oil quenching: after heating, the bearing parts are immersed in vacuum quenching oil for sufficient cooling, the oil temperature is 60-100°C, and the cooling time is 10-15 minutes. Other steps and parameters are the same as those of specific implementation method 4.
[0043] Specific implementation method 7: This implementation method is different from specific implementation method 6 in that after the vacuum oil quenching is completed, it is transported to a cleaning machine for immersion cleaning, with a total of three stations:
[0044] 1. Ultrasonic cleaning, frequency 28-30KHZ, water temperature 45-55℃;
[0045] 2. Foaming cleaning, water temperature 45 ~ 55 ℃;
[0046] 3. Alkaline water cleaning, water temperature 48 ~ 52 ℃, 0.5 ~ 0.8% sodium nitrite aqueous solution is used for rust prevention in the alkaline water station; after cleaning, drying at 120 ~ 160 ℃ for 5 ~ 10 minutes. Other steps and parameters are the same as the sixth embodiment.
[0047] Specific implementation eight: This implementation is different from specific implementation one in that in step two, the first cold treatment is completed by cold treatment at -90°C for 3 hours; after the bearing parts are restored to room temperature, they are kept at 170°C for 4 hours to complete the first tempering treatment; after the bearing parts are cooled to room temperature, they are placed in a cold treatment device and cold treated at -90°C for 3 hours to complete the second cold treatment; after the bearing parts are restored to room temperature, they are kept at 170°C for 4 hours to complete the second tempering treatment. Other steps and parameters are the same as those in specific implementation one.
[0048] The beneficial effects of the present invention are verified by the following examples:
[0049] Embodiment 1:
[0050] A heat treatment process for bearing parts made of 40Cr15Mo2VN material is implemented by the following steps:
[0051] 1. Quenching heating and cooling:
[0052] The bearing parts of the 40Cr15Mo2VN material to be treated were pre-cleaned, then placed in a vacuum heating furnace, evacuated to a vacuum degree of 8Pa, heated from room temperature to 650°C at a rate of 3°C / min and kept warm for 60min, then heated to 850°C at a rate of 5°C / min and kept warm for 60min, then heated to 1060°C at a rate of 10°C / min and kept warm for 70min, to obtain the heated bearing parts, which were then taken out of the furnace after cooling;
[0053] 2. Cold treatment and tempering:
[0054] The bearing parts taken out of the furnace are placed in a cold treatment device and cold treated at -90°C for 3 hours to complete the first cold treatment; after the bearing parts return to room temperature, they are kept at 170°C for 4 hours to complete the first tempering treatment; after the bearing parts are cooled to room temperature, they are placed in a cold treatment device and cold treated at -90°C for 3 hours to complete the second cold treatment; after the bearing parts return to room temperature, they are kept at 170°C for 4 hours to complete the second tempering treatment;
[0055] 3. Hardness and structure inspection:
[0056] After the second tempering treatment is completed, the hardness and metallographic structure of the bearing parts are inspected. If they are qualified, the heat treatment process method of the bearing parts made of 40Cr15Mo2VN material is completed.
[0057] In step 1 of this embodiment, the bearing parts to be processed are pre-cleaned: the bearing parts to be processed are placed on the tooling according to the process requirements and enter the pre-cleaning station, which is divided into cleaning agent cleaning and clean water cleaning; the cleaning agent cleaning temperature is 60°C, each cleaning time is 8min, the cleaning agent concentration is 2%, and the cleaning agent is a water-based metal cleaning agent produced by Nanjing Kerun Industrial Media Co., Ltd., model: KR-F400H; the clean water cleaning temperature is 60°C, the cleaning time is 8min; after cleaning, drying is carried out, the drying temperature is 120°C, and the drying time is 8min.
[0058] The cooling described in step 1 of this embodiment is vacuum oil quenching; the vacuum oil quenching: after heating, the bearing parts are immersed in vacuum quenching oil for sufficient cooling, the oil temperature is 80°C, and the cooling time is 12 minutes; in this embodiment, the quenching oil is Nanjing Kerun KR468G bearing special quenching oil.
[0059] After vacuum oil quenching, it is transported to the cleaning machine for immersion cleaning. There are three stations in total:
[0060] 1. Ultrasonic cleaning, frequency 28-30KHZ, water temperature 45-55℃;
[0061] 2. Foaming cleaning, water temperature 45 ~ 55 ℃;
[0062] 3. Alkaline water cleaning, water temperature 48 ~ 52 ℃, the alkaline water station uses 0.5 ~ 0.8% concentration of sodium nitrite aqueous solution for rust prevention; after cleaning, dry at 120 ~ 160 ℃ for 5 ~ 10 minutes.
[0063] The vacuum heating furnace in this embodiment is: Beijing Zhongfu Yueda JVTF966.
[0064] The cold treatment equipment in this embodiment is LC297 cold treatment equipment produced by Shenzhen Dejieli Metal Technology Co., Ltd.; the equipment used for the primary cold treatment and the secondary cold treatment is the same.
[0065] The first tempering treatment and the second tempering treatment in this embodiment use the same equipment, both of which are RHW-100-800 mesh belt low temperature tempering furnaces produced by Hangzhou Jinzhou Technology Co., Ltd.
[0066] The bearing parts made of 40Cr15Mo2VN heat-treated in this embodiment have dimensions of: diameter 310mm×height 53mm×inner diameter 274mm, and effective wall thickness 18mm; the test results are as follows:
[0067] Hardness: 60~60.5HRC;
[0068] Metallographic structure: Figure 1 As shown, it is composed of tempered martensite + a small amount of primary carbides + dispersed secondary carbides + a small amount of retained austenite.
[0069] Embodiment 2:
[0070] The difference between this embodiment and embodiment 1 is that the cooling in step 1 is vacuum air quenching; the vacuum air quenching: the heated bearing parts are cooled by 8 bar high pressure nitrogen, and the cooling time is 20 minutes. The rest is the same as embodiment 1.
[0071] The bearing parts made of 40Cr15Mo2VN heat-treated in this embodiment are tested and the results are as follows:
[0072] Hardness: 59~59.5HRC;
[0073] Metallographic structure: It is composed of tempered martensite + a small amount of primary carbides + dispersed secondary carbides + a small amount of retained austenite.
[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A heat treatment process for bearing parts made of 40Cr15Mo2VN material, characterized in that It is implemented as follows:
1. Quenching heating and cooling: The bearing parts of the 40Cr15Mo2VN material to be processed are pre-cleaned, then placed in a vacuum heating furnace, evacuated to a vacuum degree of 5-10Pa, heated from room temperature to 650°C at a rate of 2-6°C / min and kept warm for 50-70min, then heated to 850°C at a rate of 5-9°C / min and kept warm for 50-70min, then heated to 1060°C at a rate of 8-12°C / min and kept warm for 60-80min, to obtain the heated bearing parts, and then taken out of the furnace after cooling; 2. Cold treatment and tempering: The bearing parts taken out of the furnace are placed in a cold treatment device and cold treated at -80 to -120°C for 2 to 4 hours to complete the first cold treatment; after the bearing parts return to room temperature, they are kept at 160 to 180°C for 3 to 4 hours to complete the first tempering treatment; after the bearing parts are cooled to room temperature, they are placed in a cold treatment device and cold treated at -80 to -120°C for 2 to 4 hours to complete the second cold treatment; after the bearing parts return to room temperature, they are kept at 160 to 180°C for 3 to 4 hours to complete the second tempering treatment; 3. Hardness and structure inspection: After the second tempering treatment is completed, the hardness and metallographic structure of the bearing parts are inspected. If they are qualified, the heat treatment process method of the bearing parts made of 40Cr15Mo2VN material is completed.
2. According to claim 1, a heat treatment process for bearing parts made of 40Cr15Mo2VN material, characterized in that In step 1, the bearing parts of 40Cr15Mo2VN material to be processed are pre-cleaned: the bearing parts to be processed are placed on the tooling according to the process requirements and enter the pre-cleaning station, which is divided into cleaning agent cleaning and clean water cleaning; the cleaning agent cleaning temperature is 50-80°C, and the cleaning time for each step is 6-10min; the clean water cleaning temperature is 50-80°C, and the cleaning time is 6-8min; after cleaning, drying is carried out, the drying temperature is 110-130°C, and the drying time is 6-10min.
3. The heat treatment process for bearing parts made of 40Cr15Mo2VN material according to claim 1 is characterized in that In step 1, evacuate to a vacuum degree of 8 Pa, heat from room temperature to 650°C at a rate of 3°C / min and keep warm for 60 min, then heat to 850°C at a rate of 5°C / min and keep warm for 60 min, then heat to 1060°C at a rate of 10°C / min and keep warm for 70 min.
4. The heat treatment process for bearing parts made of 40Cr15Mo2VN material according to claim 1 is characterized in that The cooling in step 1 is vacuum air quenching or vacuum oil quenching.
5. A heat treatment process for bearing parts made of 40Cr15Mo2VN material according to claim 4, characterized in that The vacuum quenching: after heating, the bearing parts are cooled by high-pressure nitrogen of 7 to 10 bar, and the cooling time is 15 to 25 minutes.
6. A heat treatment process for bearing parts made of 40Cr15Mo2VN material according to claim 4, characterized in that The vacuum oil quenching: after heating, the bearing parts are immersed in vacuum quenching oil for sufficient cooling, the oil temperature is 60-100°C, and the cooling time is 10-15 minutes.
7. A heat treatment process for bearing parts made of 40Cr15Mo2VN material according to claim 6, characterized in that After the vacuum oil quenching is completed, the machine is moved to the cleaning machine for immersion cleaning, with a total of three stations:
1. Ultrasonic cleaning, frequency 28-30KHZ, water temperature 45-55℃; 2. Foaming cleaning, water temperature 45 ~ 55 ℃; 3. Alkaline water cleaning, water temperature 48 ~ 52 ℃, the alkaline water station uses 0.5 ~ 0.8% concentration of sodium nitrite aqueous solution for rust prevention; after cleaning, dry at 120 ~ 160 ℃ for 5 ~ 10 minutes.
8. The heat treatment process for bearing parts made of 40Cr15Mo2VN material according to claim 1, characterized in that In step 2, the first cold treatment is completed by cold treatment at -90°C for 3 hours; after the bearing parts return to room temperature, they are kept at 170°C for 4 hours to complete the first tempering treatment; after the bearing parts are cooled to room temperature, they are placed in a cold treatment device and cold treated at -90°C for 3 hours to complete the second cold treatment; after the bearing parts return to room temperature, they are kept at 170°C for 4 hours to complete the second tempering treatment.
Citation Information
Cited By
Process method for solving denitrification after heat treatment of high-nitrogen stainless steel bearing part
CN119427072A