TOPCon battery capable of reducing ultraviolet induced degradation and preparation method
By adopting a multi-layer passivation structure in TOPCon batteries, including a stack of silicon dioxide and alumina layers, combined with silicon nitride layers, the problem of ultraviolet induced attenuation is solved, the interface passivation level is maintained and the reduction of solar light absorption efficiency is avoided. , realizes effective blocking of ultraviolet rays.
Patent Information
- Application Number
- CN202411149624.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-15
AI Technical Summary
TOPCon batteries are susceptible to ultraviolet-induced attenuation, and existing methods reduce solar light absorption while reducing ultraviolet attenuation, resulting in a drop in current.
Using a multi-layer passivation structure, including a layer of silicon dioxide and alumina layer on the front and back of the silicon wafer, combined with a silicon nitride layer, the silicon dioxide and alumina layer are grown by thermal oxidation or ALD technology, with thickness and refractive index optimization To improve interface passivation and fixed charge density, preventing hot carriers from passing through the interface.
Effectively reduce ultraviolet-induced attenuation, maintain the interface passivation level, improve the battery's ultraviolet light stability, and do not affect the solar light absorption efficiency.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of solar cells, and in particular relates to a TOPCon cell capable of reducing ultraviolet induced attenuation and a preparation method thereof. Background Art
[0002] The Renewable Energy Testing Center (RETC), an international authoritative testing organization, has released the "2024 Photovoltaic Module Index Report". In the 2024 edition of the Photovoltaic Module Index Report, RETC identified 7 important reliability tests. From the monitoring results, the results of the ultraviolet induced degradation (UVID) test are worrying, and 40% of the module samples show red light warning signals. Regarding the issue of ultraviolet degradation, RETC has already warned the industry in the "2022 Photovoltaic Module Index Report" released in 2023. The report pointed out that some new battery technologies, most notably N-TOPCon, seem to be susceptible to UVID.
[0003] The mechanism of UV-induced degradation of photovoltaic cells has also been reported in the literature, and there are two main mechanisms to explain it. The first mechanism believes that under the action of ultraviolet light, the interface between silicon and the passivation dielectric film changes, the fixed charge decreases or the interface state defect density increases, which in turn affects the passivation of the silicon surface. The second mechanism believes that ultraviolet light excites hot carriers, which have high mobility and sufficient energy to cross the interface barrier. Hot carriers have sufficient kinetic energy to destroy the passivation layer and increase the interface state defect density.
[0004] There are some methods to improve the UV-induced attenuation of photovoltaic modules. The starting point is to allow the UV light to be absorbed by some film layers and not directly act on the cells, such as increasing the UV absorption of the module packaging material, coating a layer of UV-absorbing film on the glass, and increasing the refractive index of the silicon nitride of the photovoltaic cell to absorb UV light. However, these methods will reduce the absorption of sunlight by the module, thereby reducing the current. Summary of the invention
[0005] In order to solve the problem of ultraviolet induced attenuation of the above-mentioned TOPCon cell, the present invention provides a TOPCon cell with reduced ultraviolet induced attenuation and a preparation method thereof, which can improve the effect of ultraviolet light on interface passivation.
[0006] The TOPCon cell for reducing ultraviolet induced attenuation of the present invention comprises a silicon wafer, wherein the front side of the silicon wafer is provided with a first passivation layer, a second passivation layer, and a metal electrode in sequence from the inside to the outside, and the back side of the silicon wafer is provided with a tunneling oxide layer, a doped polysilicon layer, a second passivation layer, and a metal electrode in sequence from the inside to the outside, wherein the first passivation layer comprises a silicon dioxide layer, or a stack of a silicon dioxide layer and an aluminum oxide layer.
[0007] Furthermore, when the first passivation layer is a silicon dioxide layer, the thickness of the silicon dioxide layer is 10-20 nm.
[0008] Furthermore, when the first passivation layer is a stack of a silicon dioxide layer and an aluminum oxide layer, the thickness of the silicon dioxide layer is 1-5 nm, and the thickness of the aluminum oxide layer is 3-10 nm. In this way, oxygen-rich aluminum oxide can increase the fixed charge density of aluminum oxide; combined with the silicon dioxide thin layer, the low interface state defect density and high fixed charge are conducive to the passivation of the interface. After the ultraviolet light acts, the interface passivation can be maintained at a good level, which can improve the ultraviolet induced attenuation.
[0009] Furthermore, the second passivation layer is a silicon nitride layer, or a silicon oxynitride layer, or a stacked layer of a silicon nitride layer and a silicon oxynitride layer, and the thickness of the second passivation layer is 60-80 nm.
[0010] The present invention also provides a method for preparing the above-mentioned TOPCon battery for reducing ultraviolet induced attenuation, comprising the following steps: 1) The front side of the silicon wafer is textured and a PN junction is formed, a tunneling oxide layer and a doped polysilicon layer are prepared on the back side, and the surface is cleaned; 2) growing a first passivation layer on the front side of the silicon wafer, wherein the first passivation layer comprises a silicon dioxide layer, or a stack of a silicon dioxide layer and an aluminum oxide layer; 3) Depositing a second passivation layer on the front and back sides of the silicon wafer; 4) Print metal electrodes on the front and back of the battery, and sinter to complete the TOPCon battery.
[0011] Furthermore, in step 2), when the first passivation layer is a silicon dioxide layer, the silicon dioxide layer is grown by thermal oxidation or ALD.
[0012] The above thermal oxidation method is to place the cleaned silicon wafer in a quartz boat and send it into an oxidation furnace tube, fill it with nitrogen, raise the temperature to 800℃-900℃, then fill it with oxygen, keep it warm for 30min-60min, and grow a silicon dioxide layer with a thickness of 10-20nm on the front of the silicon wafer.
[0013] The above-mentioned ALD method is to load the cleaned silicon wafer into a small boat and send it into the ALD furnace tube, fill it with nitrogen, raise the temperature to 250℃-350℃, and then alternately fill it with silicon precursor and oxidation precursor. Each ALD cycle is set as: silicon precursor 100ms->reaction 7s->nitrogen purge 15s->oxidation precursor 1000ms->reaction 7s->nitrogen purge 15s. After 100-200 ALD cycles, a silicon dioxide layer with a thickness of 10-20nm is grown on the silicon surface.
[0014] Furthermore, in step 2), when the first passivation layer is a stack of a silicon dioxide layer and an aluminum oxide layer, the silicon dioxide layer is grown by thermal oxidation or ALD and the aluminum oxide layer is grown by ALD.
[0015] The above thermal oxidation method is to place the cleaned silicon wafer in a quartz boat and send it into an oxidation furnace tube, fill it with nitrogen, raise the temperature to 550℃-650℃, then fill it with oxygen, keep it warm for 20min-60min, and grow a silicon dioxide layer with a thickness of 1-5nm on the front of the silicon wafer.
[0016] The above-mentioned ALD method is to load the cleaned silicon wafer into a small boat and send it into the ALD furnace tube, fill it with nitrogen, raise the temperature to 250℃-350℃, and then alternately fill it with silicon precursor and oxidation precursor. Each ALD cycle is set as: silicon precursor 100ms->reaction 7s->nitrogen purge 15s->oxidation precursor 1000ms->reaction 7s->nitrogen purge 15s. After 10-50 ALD cycles, a silicon dioxide layer with a thickness of 1-5nm is grown on the silicon surface.
[0017] The above-mentioned aluminum oxide layer is formed using the ALD method: a silicon wafer with a silicon dioxide layer grown on the front is loaded into a small boat and sent into the ALD furnace tube, the temperature is raised to 250°C-350°C, and then aluminum precursor and oxidation precursor are alternately filled in. Each ALD cycle is set as: aluminum precursor 100ms->reaction 7s->nitrogen purge 12s->oxidation precursor 1000ms->reaction 7s->nitrogen purge 12s. After 30-100 ALD cycles, a 3-10nm thick aluminum oxide layer is grown on the silicon dioxide layer on the front of the silicon wafer.
[0018] Beneficial effects: The present invention grows a 10-20nm silicon dioxide layer on the front of the silicon wafer, and oxygen atoms can effectively saturate the dangling bonds on the silicon surface. The defect state density of the silicon dioxide-silicon interface is extremely low, which is conducive to the passivation of the interface; at the same time, silicon dioxide can block the hot carriers excited by ultraviolet light in the silicon body from crossing the interface, thereby protecting the interface from being destroyed; after the ultraviolet light acts, the interface can still maintain a low interface state density, and the interface passivation can be maintained at a good level, which can improve the ultraviolet induced attenuation. When the silicon dioxide layer and the aluminum oxide layer are stacked on the front of the silicon wafer, as mentioned above, the silicon dioxide layer can reduce the defect state density of the silicon dioxide-silicon interface and block the hot carriers from crossing the interface, and the aluminum oxide layer contains a large amount of fixed charge density. The superposition of the silicon dioxide layer can make the aluminum oxide layer oxygen-enriched, and the fixed charge density in the oxygen-enriched aluminum oxide layer is higher; when the silicon dioxide layer is very thin (1-5nm), the fixed charge in the aluminum oxide layer can provide a good field passivation effect for the silicon surface. Therefore, the thin silicon dioxide and aluminum oxide stack can not only passivate the silicon surface well, but also block hot carriers from crossing the silicon interface. When exposed to ultraviolet light, the passivation of the silicon dioxide-silicon interface can be maintained at a good level, which can improve ultraviolet induced attenuation. DETAILED DESCRIPTION
[0019] The present invention will now be further described in detail by way of examples, but the present invention is not limited to the examples. Example 1
[0020] 1. The front side of the silicon wafer is textured to form a PN junction, and a silicon dioxide layer and a doped polysilicon layer as a tunneling oxide layer are prepared on the back side, and the surface is cleaned.
[0021] 2. Use thermal oxidation to place the cleaned silicon wafer in a quartz boat and send it into an oxidation furnace tube, fill it with nitrogen, raise the temperature to 800°C, then fill it with oxygen, keep it warm for 60 minutes, and grow a thick silicon dioxide layer on the front of the silicon wafer. The thickness of the silicon dioxide layer is about 10nm and the refractive index is 1.48.
[0022] 3. Using PECVD (plasma enhanced chemical vapor deposition), silicon nitride and silicon oxynitride layers are deposited on the silicon dioxide layer on the front of the silicon wafer. The thickness of the silicon nitride layer is 30nm, with a refractive index of 2.1, and the thickness of the silicon oxynitride layer is 40nm, with a refractive index of 1.9. A silicon nitride layer is deposited on the back, with a thickness of 80nm and a refractive index of 2.1.
[0023] 4. Print metal electrodes on the front and back of the battery, and sinter to complete the TOPCon battery. That is, the front of the silicon wafer of the TOPCon battery is provided with a silicon dioxide layer, a silicon nitride layer, and a silicon oxynitride layer from the inside to the outside, and the back of the silicon wafer is provided with a silicon dioxide layer as a tunneling oxide layer, a doped polysilicon layer, and a silicon nitride layer from the inside to the outside. Example 2
[0024] Step 2 in Example 1 is changed to "Using thermal oxidation method, the cleaned silicon wafer is placed in a quartz boat and sent into an oxidation furnace tube, filled with nitrogen, heated to 850°C, and then filled with oxygen. Keep warm for 60 minutes to grow a thick silicon dioxide layer on the front of the silicon wafer. The silicon dioxide layer is about 15nm thick and has a refractive index of 1.48." Otherwise, a TOPCon battery is obtained in the same manner as in Example 1. Example 3
[0025] Step 2 in Example 1 is changed to "using thermal oxidation method, placing the cleaned silicon wafer in a quartz boat and sending it into an oxidation furnace tube, filling it with nitrogen, raising the temperature to 900°C, and then filling it with oxygen, keeping it warm for 60 minutes, and growing a thick silicon dioxide layer on the front side of the silicon wafer. The thickness of the silicon dioxide layer is about 20nm and the refractive index is 1.48." Except for this, a TOPCon battery is obtained in the same manner as in Example 1. Example 4
[0026] 1. The front side of the silicon wafer is textured to form a PN junction, and a silicon dioxide layer and a doped polysilicon layer as a tunneling oxide layer are prepared on the back side, and the surface is cleaned.
[0027] 2. Using ALD (atomic layer deposition), the cleaned silicon wafer is placed in a small boat and sent into the ALD furnace tube, filled with nitrogen, heated to 250°C, and then alternately filled with silicon precursor (bis-tert-butylaminosilane, molecular formula SiH2[NH(C4H9)]2) and oxidation precursor (O3). Each ALD cycle is set as follows: silicon precursor 100ms->reaction 7s->nitrogen purge 15s->oxidation precursor 1000ms->reaction 7s->nitrogen purge 15s. After 100 ALD cycles, a thick silicon dioxide layer is grown on the front of the silicon wafer. The thickness of the silicon dioxide layer is about 10nm and the refractive index is 1.45.
[0028] 3. Using PECVD, silicon nitride and silicon oxynitride layers are deposited on the silicon dioxide layer on the front of the silicon wafer. The thickness of the silicon nitride layer is 30nm, and the refractive index is 2.1. The thickness of the silicon oxynitride layer is 40nm, and the refractive index is 1.9. A silicon nitride layer is deposited on the back. The thickness of the silicon nitride layer is 80nm, and the refractive index is 2.1.
[0029] 4. Print metal electrodes on the front and back of the battery, and sinter to complete the TOPCon battery. That is, the front of the silicon wafer of the TOPCon battery is provided with a silicon dioxide layer, a silicon nitride layer, and a silicon oxynitride layer from the inside to the outside, and the back of the silicon wafer is provided with a silicon dioxide layer as a tunneling oxide layer, a doped polysilicon layer, and a silicon nitride layer from the inside to the outside. Example 5
[0030] Step 2 in Example 4 is changed to "using ALD (atomic layer deposition) to place the cleaned silicon wafer in a small boat and send it into the ALD furnace tube, fill it with nitrogen, raise the temperature to 350°C, and then alternately fill it with silicon precursor (bis-tert-butylaminosilane, molecular formula SiH2[NH(C4H9)]2) and oxidation precursor (O3). Each ALD cycle is set as follows: silicon precursor 100ms->reaction 7s->nitrogen purge 15s->oxidation precursor 1000ms->reaction 7s->nitrogen purge 15s. After 200 ALD cycles, a thick silicon dioxide layer is grown on the front side of the silicon wafer. The thickness of the silicon dioxide layer is about 20nm and the refractive index is 1.45." In addition, a TOPCon battery is obtained in the same manner as in Example 4. Example 6
[0031] 1. The front side of the silicon wafer is textured to form a PN junction, and a silicon dioxide layer and a doped polysilicon layer as a tunneling oxide layer are prepared on the back side, and the surface is cleaned.
[0032] 2. Using thermal oxidation, the cleaned silicon wafer is placed in a quartz boat and sent into an oxidation furnace tube, filled with nitrogen, heated to 550°C, and then filled with oxygen. The temperature is kept at this temperature for 20 minutes, and a thin silicon dioxide layer is grown on the front of the silicon wafer. The thickness of the silicon dioxide layer is about 1 nm.
[0033] 3. Using the ALD method again, the silicon wafer with a silicon dioxide layer grown on the front side is loaded into a small boat and sent into the ALD furnace tube. The temperature is raised to 250°C, and then aluminum precursor (trimethylaluminum) and oxidation precursor (H2O) are alternately filled in. Each ALD cycle is set as follows: aluminum precursor 100ms->reaction 7s->nitrogen purge 12s->oxidation precursor 1000ms->reaction 7s->nitrogen purge 12s. After 30 ALD cycles, a layer of aluminum oxide is grown on the silicon dioxide layer on the front side of the silicon wafer. The thickness of the aluminum oxide layer is about 3nm, and the refractive index is 1.6.
[0034] 4. Using PECVD, silicon nitride and silicon oxynitride layers are deposited on the aluminum oxide layer on the front of the silicon wafer. The thickness of the silicon nitride layer is 30nm, and the refractive index is 2.1. The thickness of the silicon oxynitride layer is 40nm, and the refractive index is 1.9. A silicon nitride layer is deposited on the back. The thickness of the silicon nitride layer is 80nm, and the refractive index is 2.1.
[0035] 5. Print metal electrodes on the front and back of the battery, and sinter to complete the TOPCon battery. That is, the front of the silicon wafer of the TOPCon battery is provided with a silicon dioxide layer, an aluminum oxide layer, a silicon nitride layer, and a silicon oxynitride layer from the inside to the outside, and the back of the silicon wafer is provided with a silicon dioxide layer as a tunneling oxide layer, a doped polysilicon layer, and a silicon nitride layer from the inside to the outside. Example 7
[0036] Step 2 in Example 6 is changed to "Using thermal oxidation, the cleaned silicon wafer is placed in a quartz boat and sent into an oxidation furnace tube, filled with nitrogen, heated to 650°C, and then filled with oxygen, kept warm for 60 minutes, and a thin silicon dioxide layer is grown on the front side of the silicon wafer, the thickness of the silicon dioxide layer is about 5 nm." Step 3 in Example 6 is changed to "Using ALD again, the silicon wafer with a silicon dioxide layer grown on the front side is loaded into a small boat and sent into the ALD furnace tube, the temperature is raised to 300°C, and then an aluminum precursor (trimethylaluminum) and an oxidation precursor (H2O) are alternately charged, and each ALD cycle is set as follows: aluminum precursor 100ms->reaction 7s->nitrogen purge 12s->oxidation precursor 1000ms->reaction 7s->nitrogen purge 12s. After 50 ALD cycles, a layer of aluminum oxide is grown on the silicon dioxide layer on the front side of the silicon wafer. The thickness of the aluminum oxide layer is about 5nm and the refractive index is 1.6." Except for this, a TOPCon battery was obtained in the same manner as in Example 6. Example 8
[0037] 1. The front side of the silicon wafer is textured and a PN junction is formed. A tunneling oxide layer and a doped polysilicon layer are prepared on the back side, and the surface is cleaned.
[0038] 2. Using the ALD method, the cleaned silicon wafer is placed in a small boat and sent into the ALD furnace tube, filled with nitrogen, heated to 300°C, and then alternately filled with silicon precursor (bis-tert-butylaminosilane, molecular formula SiH2[NH(C4H9)]2) and oxidation precursor (O3). Each ALD cycle is set as follows: silicon precursor 100ms->reaction 7s->nitrogen purge 15s->oxidation precursor 1000ms->reaction 7s->nitrogen purge 15s. After 30 ALD cycles, a layer of silicon dioxide with a thickness of about 3nm is grown on the silicon surface.
[0039] 3. Using the ALD method again, the silicon wafer with silicon dioxide grown on the front side is loaded into a small boat and sent into the ALD furnace tube. The temperature is raised to 300°C, and then aluminum precursor (trimethylaluminum) and oxidation precursor (H2O) are alternately filled in. Each ALD cycle is set as follows: aluminum precursor 100ms->reaction 7s->nitrogen purge 12s->oxidation precursor 1000ms->reaction 7s->nitrogen purge 12s. After 70 ALD cycles, a layer of aluminum oxide is grown on the silicon dioxide layer on the front side of the silicon wafer. The thickness of the aluminum oxide layer is about 7nm, and the refractive index is 1.6.
[0040] 4. Using PECVD, a silicon nitride layer and a silicon nitride oxide layer are sequentially deposited on the aluminum oxide layer on the front side of the silicon wafer. The silicon nitride layer is 30nm thick and has a refractive index of 2.1, and the silicon nitride oxide layer is 40nm thick and has a refractive index of 1.9. A silicon nitride layer is deposited on the back side. The silicon nitride layer is 80nm thick and has a refractive index of 2.1.
[0041] 5. Print metal electrodes on the front and back of the battery, and sinter to complete the TOPCon battery. That is, the front of the silicon wafer of the TOPCon battery is sequentially provided with silicon dioxide layer, aluminum oxide layer, silicon nitride layer and silicon oxynitride layer from the inside to the outside, and the back of the silicon wafer is sequentially provided with tunneling oxide layer, doped polysilicon layer and silicon nitride layer from the inside to the outside. Example 9
[0042] Step 2 in Example 8 is changed to "Using ALD, the cleaned silicon wafer is placed in a small boat and sent into the ALD furnace tube, filled with nitrogen, heated to 350°C, and then alternately filled with silicon precursor (bis-tert-butylaminosilane, molecular formula SiH2[NH(C4H9)]2) and oxidation precursor (O3), each ALD cycle is set as: silicon precursor 100ms->reaction 7s->nitrogen purge 15s->oxidation precursor 1000ms->reaction 7s->nitrogen purge 15s, after 50 ALD cycles, a silicon dioxide layer of about 5nm is grown on the silicon surface." Step 3 in Example 8 is changed to "Using the ALD method again, the silicon wafer with silicon dioxide grown on the front side is loaded into a small boat and sent into the ALD furnace tube, and the temperature is raised to 350°C, and then the aluminum precursor (trimethylaluminum) and the oxidation precursor (H2O) are alternately charged, and each ALD cycle is set as follows: aluminum precursor 100ms->reaction 7s->nitrogen purge 12s->oxidation precursor 1000ms->reaction 7s->nitrogen purge 12s. After 100 ALD cycles, a layer of aluminum oxide is grown on the silicon dioxide layer on the front side of the silicon wafer. The thickness of the aluminum oxide layer is about 10nm, and the refractive index is 1.6." Except for this, a TOPCon battery was obtained in the same manner as in Example 8.
[0043] Comparative Example 1 1. The front side of the silicon wafer is textured to form a PN junction, and a silicon dioxide layer and a doped polysilicon layer as a tunneling oxide layer are prepared on the back side, and the surface is cleaned.
[0044] 2. Using the ALD method, the above silicon wafer was loaded into a small boat and sent into the ALD furnace tube, the temperature was raised to 300°C, and then the aluminum precursor (trimethylaluminum) and the oxidation precursor (H2O) were alternately filled in. Each ALD cycle was set as follows: aluminum precursor 100ms->reaction 7s->nitrogen purge 12s->oxidation precursor 1000ms->reaction 7s->nitrogen purge 12s. After 40 ALD cycles, a layer of aluminum oxide was grown on the front of the silicon wafer. The thickness of the aluminum oxide layer was about 4 nm and the refractive index was 1.6.
[0045] 3. Using PECVD, silicon nitride and silicon oxynitride layers are deposited on the aluminum oxide layer on the front of the silicon wafer. The thickness of the silicon nitride layer is 30nm, and the refractive index is 2.1. The thickness of the silicon oxynitride layer is 40nm, and the refractive index is 1.9. A silicon nitride layer is deposited on the back. The thickness of the silicon nitride layer is 80nm, and the refractive index is 2.1.
[0046] 4. Print metal electrodes on the front and back of the battery, and sinter to complete the TOPCon battery. That is, the front of the silicon wafer of the TOPCon battery is sequentially provided with an aluminum oxide layer, a silicon nitride layer, and a silicon oxynitride layer from the inside to the outside, and the back of the silicon wafer is sequentially provided with a silicon dioxide layer as a tunneling oxide layer, doped polysilicon, and a silicon nitride layer from the inside to the outside.
[0047] In the above examples, the thickness of the silicon dioxide layer and the doped polysilicon layer of the tunnel oxide layer may refer to the prior art.
[0048] Performance Testing The IV performance of the TOPCon cells obtained in the above Examples 1-9 and the cell obtained in Comparative Example 1 was tested before and after ultraviolet irradiation, and the efficiency difference before and after ultraviolet irradiation was calculated, which is the ultraviolet induced attenuation. In the experiment, the ultraviolet irradiation conditions were: ultraviolet wavelength of 360nm, lamp power of 1000W, irradiation for 60 hours, nitrogen atmosphere in the irradiation box to prevent oxidation of the battery electrodes, and the surface temperature of the battery sample was 65°C. The results of ultraviolet induced attenuation are shown in Table 1.
[0049] Table 1 UV-induced degradation results of different battery samples
[0050] It can be seen from Table 1 that the present invention can improve the ultraviolet induced degradation of the battery cell.
[0051] The above-mentioned technologies not specifically mentioned are all referred to the prior art.
[0052] Based on the above-mentioned ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above-mentioned description. The technical scope of the present invention is not limited to the contents of the specification.
Claims
1. A TOPCon cell for reducing UV-induced degradation, characterized in that: It includes a silicon wafer, wherein the front side of the silicon wafer is provided with a first passivation layer, a second passivation layer, and a metal electrode in sequence from the inside to the outside, and the back side of the silicon wafer is provided with a tunneling oxide layer, a doped polysilicon layer, a second passivation layer, and a metal electrode in sequence from the inside to the outside, wherein the first passivation layer includes a silicon dioxide layer, or a stack of a silicon dioxide layer and an aluminum oxide layer.
2. The TOPCon cell for reducing UV-induced degradation according to claim 1, characterized in that: When the first passivation layer is a silicon dioxide layer, the thickness of the silicon dioxide layer is 10-20 nm.
3. The TOPCon cell for reducing UV-induced degradation according to claim 1, characterized in that: When the first passivation layer is a stack of a silicon dioxide layer and an aluminum oxide layer, the thickness of the silicon dioxide layer is 1-5 nm, and the thickness of the aluminum oxide layer is 3-10 nm.
4. The TOPCon cell for reducing UV-induced degradation according to claim 1, characterized in that: The second passivation layer is a silicon nitride layer, or a silicon nitride oxide layer, or a stacked layer of a silicon nitride layer and a silicon nitride oxide layer. The thickness of the second passivation layer is 60-80 nm.
5. The method for preparing a TOPCon battery with reduced UV-induced attenuation according to claim 1, characterized in that: The following steps are involved: 1) The front side of the silicon wafer is textured and a PN junction is formed, a tunneling oxide layer and a doped polysilicon layer are prepared on the back side, and the surface is cleaned; 2) growing a first passivation layer on the front side of the silicon wafer, wherein the first passivation layer comprises a silicon dioxide layer, or a stack of a silicon dioxide layer and an aluminum oxide layer; 3) Depositing a second passivation layer on the front and back sides of the silicon wafer; 4) Print metal electrodes on the front and back of the battery, and sinter to complete the TOPCon battery.
6. The method for preparing a TOPCon cell with reduced UV-induced degradation according to claim 5, characterized in that: In step 2), when the first passivation layer is a silicon dioxide layer, the silicon dioxide layer is grown by thermal oxidation or ALD.
7. The method for preparing a TOPCon cell with reduced UV-induced degradation according to claim 5, characterized in that: In step 2), when the first passivation layer is a stack of a silicon dioxide layer and an aluminum oxide layer, the silicon dioxide layer is grown by thermal oxidation or ALD and the aluminum oxide layer is grown by ALD.
Citation Information
Cited By
Anti-UVID anti-reflection passivation film and preparation method thereof
CN121793516A
Solar cell, preparation method thereof, and photovoltaic module
EP4797914A1