Tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine and preparation method thereof

By introducing 3-trifluoromethylpyridine as a dopant in tin perovskite solar cells, the problems of stannous ion instability and poor film quality are solved, and efficient photoelectric conversion efficiency and stability are achieved.

CN118973277AActive Publication Date: 2024-11-15JIAXING UNIV

Patent Information

Application Number
CN202410924481.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-15
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

Due to the instability of stannous ion and poor film quality, tin-containing perovskite solar cells have caused performance attenuation. The existing additives are mainly concentrated on reducing organic compounds, and there is a lack of new and efficient additives to improve photovoltaic performance and stability.

Method used

3-trifluoromethylpyridine (3-TFMP) is introduced as a dopant to form a complex by coordinating with SnI2 in the tin perovskite precursor, thereby increasing the redox potential of the tin adduct and inhibiting stannous ion oxidation , and prolong the perovskite crystallization time window to prepare high-quality films.

Benefits of technology

It significantly improves the photoelectric conversion efficiency and stability of perovskite solar cells, reduces the defect state density, extends the carrier life, and optimizes the surface morphology and crystallinity of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973277A_ABST
    Figure CN118973277A_ABST
Patent Text Reader

Abstract

The invention discloses a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine and a preparation method thereof, and the preparation process comprises the steps: cleaning and pretreating a transparent conductive substrate, depositing a hole transport layer, carrying out annealing treatment, adding 3-TFMP into a tin-containing perovskite precursor solution, carrying out uniform stirring, depositing on the surface of the hole transport layer, and carrying out vacuum drying, thereby obtaining the tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine. And annealing to obtain a tin-containing perovskite active layer, and continuously depositing an electron transport layer, a hole blocking layer and a top electrode in sequence to obtain the tin-containing perovskite solar cell based on 3-TFMP doped perovskite. Additive molecules containing a strong electron-withdrawing functional group trifluoromethyl can coordinate and interact with SnI2 in a perovskite precursor to form a compound (namely a tin adduct), so that the redox potential of the tin adduct is improved, the highest occupied molecular orbital (HOMO) energy level is reduced, the oxidation of stannous ions (Sn < 2 + >) is inhibited, and the photoelectric conversion efficiency is improved. And the photoelectric conversion efficiency and the stability of the perovskite solar cell are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of perovskite solar cell manufacturing, and specifically relates to a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine and a preparation method thereof. Background Art

[0002] The efficient use of solar energy has always been the focus of researchers. Metal halide perovskites have become the most promising materials for the new generation of thin-film solar cells due to their excellent optoelectronic properties. Currently, the photoelectric conversion efficiency (PCE) of single-junction perovskite solar cells (PSCs) has reached 26.1%. However, due to their ionic crystal characteristics, perovskites generally exhibit poor stability, especially in the presence of environmental substances.

[0003] In recent years, tin-based perovskites have attracted widespread attention due to their low toxicity and narrow band gap. In particular, tin-lead mixed metal halide perovskites can obtain a narrow optical band gap of about 1.2eV, which is crucial for the development of all-perovskite tandem solar cells. By combining narrow-bandgap tin-lead mixed perovskites with wide-bandgap lead-based perovskites to prepare tandem devices, it is expected to break the theoretical efficiency limit of single-junction solar cells. However, tin-based perovskites inevitably bring two key problems: one is that stannous ions (Sn 2+ ) is particularly unstable and easily oxidized to form Sn 4+ First, the tin-based perovskite crystallizes faster, resulting in poor film quality. These problems are accompanied by the generation of a large number of defects in the perovskite, which changes the carrier type, thereby aggravating the carrier recombination of the device and causing the performance of tin-containing PSCs to decay. Therefore, despite the ideal band gap, the performance of tin-containing PSCs is not particularly satisfactory.

[0004] From the above, it can be seen that inhibiting the oxidation of tin perovskite, reducing the defects in perovskite, and obtaining perovskite films with high crystalline quality are the key to improving the photovoltaic performance and stability of tin-containing PSCs. Among the various strategies that have been developed, additive engineering is considered to be a simple and effective method to improve the performance of PSCs devices, but the current research on tin-containing perovskite additives is more focused on reducing organic compounds. Therefore, in order to further improve the photovoltaic performance and stability of tin-containing PSCs, it is urgent to develop a new and efficient additive molecule to introduce into the perovskite layer to optimize the properties of the above-mentioned film. Summary of the invention

[0005] In view of the above problems, the object of the present invention is to provide a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine and a preparation method thereof.

[0006] Specific technical solutions:

[0007] A method for preparing a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine comprises the following steps:

[0008] 1) Ultrasonic cleaning of the transparent conductive substrate, drying the transparent conductive substrate with a nitrogen stream before use, and then treating the surface of the transparent conductive substrate with a plasma cleaner or ozone;

[0009] 2) depositing a hole transport layer HTL solution on the surface of the transparent conductive substrate treated in step 1), and performing annealing treatment to obtain a HTL film;

[0010] 3) adding 3-trifluoromethylpyridine (3-TFMP) to a tin-containing perovskite precursor solution and stirring the mixture evenly to prepare a 3-trifluoromethylpyridine-doped tin-containing perovskite precursor solution, depositing the solution on the surface of the HTL film, and obtaining a tin-containing perovskite active layer after annealing;

[0011] 4) subsequently depositing an electron transport layer and a hole blocking layer on the surface of the tin-containing perovskite active layer obtained in step 3);

[0012] 5) depositing a top electrode on the surface of the thin film obtained in step 4), and finally obtaining a tin-containing perovskite solar cell based on 3-trifluoromethylpyridine-doped perovskite.

[0013] Furthermore, the deposition method is one or a combination of spin coating, blade coating, inkjet printing, slit coating, and vacuum evaporation.

[0014] Furthermore, the transparent conductive substrate in step 1) is Glass / ITO or FTO, plastic flexible substrate / ITO or FTO, and the transparent conductive substrate is ultrasonically cleaned using distilled water, acetone, and isopropanol solvents in sequence.

[0015] Furthermore, the HTL solution in step 2) is a mixed material of one or more of PEDOT:PSS, PTAA, MeO-2PACz, and 4PACz.

[0016] Further, the HTL solution is spin-coated on the surface treated transparent conductive substrate, and then annealed to obtain a hole transport layer, the spin coating speed is 5000-6000 rpm, the spin coating time is 30-40 seconds; the annealing temperature is 90-110°C, and the annealing time is 5-10 minutes.

[0017] The tin-containing perovskite precursor solution in step 3) is any organic-inorganic hybrid perovskite or inorganic perovskite containing metallic tin, and the thickness of the tin-containing perovskite active layer is 600-800 nm.

[0018] Preferably, the tin-containing perovskite precursor solution in step 3) is FAx MA 1-x Sn y Pb 1-y I 3 , 0 ≤ x ≤ 1, 0 < y ≤ 1 or CsSn x Pb 1-x I 2.7 Br 0.3 , 0 < x ≤ 1.

[0019] Preferably, when the tin-containing perovskite precursor solution is FA 0.7 MA 0.3 Sn 0.5 Pb 0.5 I 3 , the specific process is as follows: Dissolve FAI, MAI, SnI 2 , PbI 2 and SnF 2 mixture in a mixed solvent of DMF and DMSO with a volume ratio of 2:1 - 4:1 to obtain a perovskite precursor solution with a concentration of 1.5 - 2.5 M, and the content of SnF 2 is 5 - 15 mol% of SnI 2 .

[0020] Preferably, when the tin-containing perovskite precursor solution is CsPb 0.5 Sn 0.5 I 2.7 Br 0.3 , the specific process is as follows: Dissolve CsI, CsBr, PbBr 2 and PbI 2 in a mixed solvent of DMF and DMSO (v / v, 4:1) to form 0.8 M CsPbI 2.4 Br 0.6 , dissolve CsI, SnI 2 and SnF 2 with a molar ratio of 1:1:0.1 in a mixed solvent of DMF and DMSO (v / v, 4:1) to form a 0.8 M CsSnI 3 precursor solution, and prepare the CsPb 2.4 Br 0.6 and CsSnI 3 precursor solution by mixing the CsPb 0.5 Sn 0.5 I 2.7 Br 0.3 precursor solutions in a volume ratio of 1:1.

[0021] Furthermore, in step 3), the doping amount of 3-trifluoromethylpyridine is 1-5 mol% of the tin-containing perovskite precursor solution, 3-trifluoromethylpyridine is added to the tin-containing perovskite precursor solution and stirred for 0.5-1.5 h, and then filtered through a polytetrafluoroethylene membrane to obtain a 3-trifluoromethylpyridine-doped tin-containing perovskite precursor solution.

[0022] Furthermore, in step 3), two-step spin coating deposition is performed, first at a rotation speed of 500-1000 rpm for 5-10 seconds, and then at a rotation speed of 4000-5000 rpm for 30-50 seconds. 100-300 μL of ethyl acetate anti-solvent is dripped on the rotating substrate 10-20 seconds before the end of the second spin coating, and then the substrate is annealed to obtain the final perovskite film at a temperature of 90-110°C for 5-20 minutes.

[0023] Further, the electron transport layer in step 4) is PC 61 BM, PC 71 BM, C 60 , C 70 One or more mixed materials in, the hole blocking layer is BCP.

[0024] Furthermore, the top electrode in step 5) is a combination of one or more materials selected from the group consisting of Ag, Au, Cu, AZO, carbon materials, and conductive polymers.

[0025] A tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine prepared by the preparation method.

[0026] The beneficial effects of the present invention are:

[0027] (1) The method for preparing a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine (3-TFMP) provided by the present invention comprises preparing a perovskite film by dissolving 3-TFMP in a perovskite precursor solution, wherein the trifluoro-substituted (having strong electron-withdrawing properties) additive molecule can react with SnI in the perovskite precursor. 2 The coordination interaction forms a complex (i.e., tin adduct), which increases the redox potential of the tin adduct and reduces the highest occupied molecular orbital (HOMO) energy level. In addition, the introduction of the fluorine-substituted molecule leads to an increase in the ionization potential of the perovskite structure, thereby greatly suppressing the stannous ions (Sn 2+ ) oxidation, thereby reducing the defect state density, suppressing the non-radiative recombination in the perovskite and extending the carrier lifetime. Ultimately, the photoelectric conversion efficiency and stability of perovskite solar cells have been significantly improved.

[0028] (2) The method for preparing a 3-TFMP-doped tin-containing perovskite solar cell provided by the present invention comprises preparing a perovskite film by dissolving a 3-TFMP-containing perovskite precursor solution, wherein the 3-TFMP ligand molecule binds to SnI via a pyridine group. 2 The interaction extends the time window for perovskite crystallization, and a perovskite film with better crystallinity, fewer grain boundaries and lower residual stress is prepared. In addition, the surface morphology and crystallinity of the perovskite active layer can be adjusted by adjusting the amount of 3-TFMP added, thereby affecting the light absorption performance, the transmission and collection efficiency of photogenerated carriers, and the stability of the perovskite film, providing a new method for the preparation of high-efficiency and high-stability tin-containing perovskite solar cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Steady-state fluorescence spectra of tin-containing perovskite films doped with 3-trifluoromethylpyridine and undoped with 3-trifluoromethylpyridine;

[0030] Figure 2 JV curves of tin-containing perovskite single hole carrier devices doped with 3-trifluoromethylpyridine and undoped with 3-trifluoromethylpyridine;

[0031] Figure 3 Surface SEM images of tin-containing perovskite films doped with 3-trifluoromethylpyridine and undoped with 3-trifluoromethylpyridine;

[0032] Figure 4 JV curves of tin-containing perovskite solar cells doped with 3-trifluoromethylpyridine and undoped with 3-trifluoromethylpyridine;

[0033] Figure 5 This is a comparison chart of the stability of tin-containing perovskite solar cells doped with 3-trifluoromethylpyridine and undoped with 3-trifluoromethylpyridine. DETAILED DESCRIPTION

[0034] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited thereto.

[0035] Example 1

[0036] Based on Glass / ITO / PEDOT:PSS / 3-trifluoromethylpyridine doped perovskite / C 60 The preparation process of tin-lead perovskite solar cells with / BCP / Cu device structure is as follows:

[0037] Step 1: Use distilled water, acetone, and isopropanol solvents to ultrasonically clean the Glass / ITO transparent conductive anode substrate for 30 minutes in sequence, blow dry the anode substrate with a nitrogen flow, and then use a plasma cleaner to treat the substrate surface for 10 minutes.

[0038] Step 2: Spin coating the PEDOT:PSS solution on the surface treated anode substrate, and then annealing to obtain the hole transport layer; wherein the spin coating speed is 5000 rpm, the spin coating time is 40 seconds; the annealing temperature is 110°C, and the annealing time is 10 minutes.

[0039] Step 3: Spin-coat the perovskite precursor solution on the surface of the hole transport layer, wherein the perovskite active layer is FA 0.7 MA 0.3 Sn 0.5 Pb 0.5 I 3 The specific process is: FAI, MAI, SnI 2 、PbI 2 and SnF 2 The mixture was dissolved in a mixed solvent of DMF and DMSO with a volume ratio of 3:1 to prepare a perovskite precursor solution with a concentration of 2 M. SnF 2 Content is SnI 2 10 mol % was added to the perovskite precursor solution. Subsequently, 2 mol % (relative to the proportion of the perovskite precursor solution) of 3-trifluoromethylpyridine was added to the perovskite precursor solution. The precursor solution was stirred at room temperature for 0.5 h, then filtered through a polytetrafluoroethylene membrane with a pore size of 0.22 μm, and the perovskite active layer was deposited by a two-step spin coating process: (1) 800 rpm for 10 seconds, (2) 5000 rpm for 30 seconds, and 300 μL of ethyl acetate antisolvent was dripped on the rotating substrate 15 seconds before the end of the second spin coating step, and then the substrate was annealed to obtain the final tin-containing perovskite film, the annealing temperature was 100 ° C, and the time was 10 minutes.

[0040] Step 4: Sequentially evaporate the electron transport layer C on the surface of the above-mentioned Sn-Pb perovskite active layer 60 , the thickness of which is 25nm; and a vapor-deposited hole blocking layer BCP, the thickness of which is 6nm;

[0041] Step 5: Vapor-deposit a cathode electrode layer of Cu on the surface of the hole blocking layer, with a thickness of 90 nm;

[0042] After the above steps are completed, a tin-lead perovskite solar cell with a perovskite layer doped with 3-trifluoromethylpyridine is obtained.

[0043] Example 2

[0044] Based on Glass / ITO / PEDOT:PSS / Perovskite / C 60 The preparation process of tin-lead perovskite solar cells with / BCP / Cu device structure is as follows:

[0045] Step 1: Use distilled water, acetone, and isopropanol solvents to ultrasonically clean the Glass / ITO transparent conductive anode substrate for 30 minutes in sequence, blow dry the anode substrate with a nitrogen flow, and then use a plasma cleaner to treat the substrate surface for 10 minutes.

[0046] Step 2: Spin coating the PEDOT:PSS solution on the surface treated anode substrate, and then annealing to obtain the hole transport layer; wherein the spin coating speed is 5000 rpm, the spin coating time is 40 seconds; the annealing temperature is 110°C, and the annealing time is 10 minutes.

[0047] Step 3: Spin-coat the perovskite precursor solution on the surface of the hole transport layer, wherein the perovskite active layer is FA 0.7 MA 0.3 Sn 0.5 Pb 0.5 I 3 The specific process is: FAI, MAI, SnI 2 、PbI 2 and SnF 2 The mixture was dissolved in a mixed solvent of DMF and DMSO with a volume ratio of 3:1 to prepare a perovskite precursor solution with a concentration of 2 M. SnF 2 Content is SnI 2 The precursor mixture solution was stirred at room temperature for 0.5 h, then filtered through a polytetrafluoroethylene membrane with a pore size of 0.22 μm, and the perovskite active layer was deposited by a two-step spin coating process: (1) 800 rpm for 10 seconds, (2) 5000 rpm for 30 seconds, and 300 μL of ethyl acetate anti-solvent was dripped on the rotating substrate 15 seconds before the end of the second spin coating. The substrate was then annealed at a temperature of 100° C. for 10 minutes to obtain the final tin-containing perovskite film.

[0048] Step 4: Sequentially evaporate the electron transport layer C on the surface of the above-mentioned Sn-Pb perovskite active layer 60 , the thickness of which is 25nm; and a vapor-deposited hole blocking layer BCP, the thickness of which is 6nm;

[0049] Step 5: Vapor-deposit a cathode electrode layer of Cu on the surface of the hole blocking layer, with a thickness of 90 nm;

[0050] After the above steps are completed, a tin-lead perovskite solar cell without a perovskite layer is obtained.

[0051] Figure 1 It can be seen that the 3-TFMP-doped SnPb perovskite film has a high steady-state fluorescence intensity, indicating that the perovskite film has lower defect-induced non-radiative recombination. Figure 2The JV curve of single hole carrier device shows that 3-TFMP doped SnPb perovskite film has lower V TFL , indicating that the doped film has a lower defect state density, indicating that the oxidation of stannous ions is effectively suppressed, which once again verifies that 3-TFMP doping has reduced non-radiative recombination. Figure 3 From the SEM surface morphology, it can be seen that the 3-TFMP-doped Sn-Pb perovskite film has relatively larger grains and fewer grain boundaries, indicating that the crystallinity of the perovskite is improved. Figure 4 The results show that the tin-lead perovskite solar cells doped with 3-TFMP have higher open circuit voltage, short circuit current, fill factor and final photoelectric conversion efficiency, indicating that the introduction of 3-TFMP can inhibit the energy loss caused by non-radiative recombination of the device, improve the efficiency of carrier transport and collection, and promote light absorption. Figure 5 It can be intuitively seen that the doped perovskite solar cells can maintain a higher initial efficiency ratio over time, indicating that the stability of perovskite solar cells is significantly improved by introducing 3-TFMP as an antioxidant additive in the tin-lead perovskite active layer.

[0052] Example 3

[0053] Based on Glass / ITO / PEDOT:PSS / 3-trifluoromethylpyridine doped perovskite / C 60 Preparation of Sn-Pb perovskite solar cells with / BCP / Cu device structure

[0054] The amount of 3-trifluoromethylpyridine added to the perovskite precursor mixed solution in step 3 of Example 1 was changed to 1 mol %, and the other operating conditions remained unchanged.

[0055] Example 4

[0056] Based on Glass / ITO / PEDOT:PSS / 3-trifluoromethylpyridine doped perovskite / C 60 Preparation of Sn-Pb perovskite solar cells with / BCP / Cu device structure

[0057] The amount of 3-trifluoromethylpyridine added to the perovskite precursor mixed solution in step 3 of Example 1 was changed to 4 mol %, and the other operating conditions remained unchanged.

[0058] Table 1 Comparison of parameters of tin-lead perovskite solar cells prepared in Examples 1-4

[0059]

[0060] The purpose of Example 1, Example 3 and Example 4 is to show the effect of different 3-trifluoromethylpyridine doping amounts on the photoelectric conversion efficiency of the final device. Compared with Example 1, Example 3 and Example 4 respectively add 2 mol%, 1 mol%, and 4 mol% of 3-trifluoromethylpyridine to a 2M tin-lead perovskite precursor mixed solution to obtain a perovskite precursor solution with a gradient doping amount. It can be found from Table 1 that in Example 1, when the doping amount of 3-trifluoromethylpyridine is 2 mol%, thanks to the effect of 3-trifluoromethylpyridine on the Sn in the perovskite 2+ Oxidation inhibition and film crystallization modulation reduce the defects on the surface and grain boundaries of tin-lead perovskite, improve the film quality, significantly reduce the energy loss caused by non-radiative recombination, and the device has the highest open circuit voltage (V oc ), short circuit current (J sc ), fill factor (FF) and the final photoelectric conversion efficiency; at the same time, compared with Example 2, various parameters of Example 3 and Example 4 are improved to varying degrees, but the effects are not as good as Example 1, so according to the experimental results, it is determined that the additive used in Example 1 is the optimal doping amount.

[0061] Example 5

[0062] Based on Glass / ITO / PEDOT:PSS / 3-trifluoromethylpyridine doped perovskite / C 60 The preparation process of pure inorganic tin-lead perovskite solar cells with / BCP / Cu device structure is as follows:

[0063] Step 1: Use distilled water, acetone, and isopropanol solvents to ultrasonically clean the Glass / ITO transparent conductive anode substrate for 30 minutes in sequence, blow dry the anode substrate with a nitrogen flow, and then use a plasma cleaner to treat the substrate surface for 10 minutes.

[0064] Step 2: Spin coating the PEDOT:PSS solution on the surface treated anode substrate, and then annealing to obtain the hole transport layer; wherein the spin coating speed is 5000 rpm, the spin coating time is 40 seconds; the annealing temperature is 110°C, and the annealing time is 10 minutes.

[0065] Step 3: Spin-coat the perovskite precursor solution on the surface of the hole transport layer, wherein the perovskite active layer is CsPb 0.5 Sn 0.5 I 2.7 Br 0.3 The specific process is: CsI, CsBr, PbBr 2 and PbI 2 Dissolved in a mixed solvent of DMF and DMSO (v / v, 4:1) to form 0.8 M CsPbI2.4 Br 0.6 . CsI and SnI with a molar ratio of 1:1:0.1 2 and SnF 2 Dissolved in a mixed solvent of DMF and DMSO (v / v, 4:1) to form 0.8 M CsSnI 3 Precursor solution. By 2.4 Br 0.6 and CsSnI 3 The precursor solutions were mixed in a volume ratio of 1:1 to prepare CsPb 0.5 Sn 0.5 I 2.7 Br 0.3 Precursor solution. Subsequently, 3.5 mol% (relative to the proportion of the perovskite precursor solution) of 3-trifluoromethylpyridine was added to the perovskite precursor solution. The precursor solution was stirred at room temperature for 0.5 h, then filtered through a polytetrafluoroethylene membrane with a pore size of 0.22 μm, and the perovskite active layer was deposited by a two-step spin coating process: (1) 1000 rpm for 10 seconds, (2) 5000 rpm for 40 seconds, and 300 μL of ethyl acetate antisolvent was dripped on the rotating substrate 15 seconds before the end of the second spin coating step, and then the substrate was annealed to obtain the final tin-containing perovskite film, the annealing temperature was 100°C, and the time was 10 minutes.

[0066] Step 4: Sequentially evaporate the electron transport layer C on the surface of the above-mentioned Sn-Pb perovskite active layer 60 , the thickness of which is 25nm; and a vapor-deposited hole blocking layer BCP, the thickness of which is 6nm;

[0067] Step 5: Vapor-deposit a cathode electrode layer of Cu on the surface of the hole blocking layer, with a thickness of 90 nm;

[0068] After the above steps are completed, a pure inorganic tin-lead perovskite solar cell with a perovskite layer doped with 3-trifluoromethylpyridine is obtained.

[0069] Example 6

[0070] Based on Glass / ITO / PEDOT:PSS / 3-trifluoromethylpyridine doped perovskite / C 60 Preparation of a pure inorganic tin-lead perovskite solar cell with a / BCP / Cu device structure, changing the amount of 3-trifluoromethylpyridine added to the perovskite precursor mixed solution in step 3 in Example 5. In this example, no 3-trifluoromethylpyridine is added, and other operations are the same as in Example 5.

[0071] Example 7

[0072] Based on Glass / ITO / PEDOT:PSS / 3-trifluoromethylpyridine doped perovskite / C 60 Preparation of a pure inorganic tin-lead perovskite solar cell with a / BCP / Cu device structure, changing the amount of 3-trifluoromethylpyridine added to the perovskite precursor mixed solution in step 3 of Example 5 to 2.0%, and other operations are the same as Example 5.

[0073] Example 8

[0074] Based on Glass / ITO / PEDOT:PSS / 3-trifluoromethylpyridine doped perovskite / C 60 Preparation of a pure inorganic tin-lead perovskite solar cell with a Cu / BCP / Cu device structure, changing the amount of 3-trifluoromethylpyridine added to the perovskite precursor mixed solution in step 3 of Example 5 to 5.0%, and other operations are the same as Example 5.

[0075] Table 2 Comparison of parameters of pure inorganic tin-lead perovskite solar cells prepared in Examples 5-8

[0076]

[0077] It can be found from Table 2 that different doping amounts of 3-trifluoromethylpyridine have different effects on the photoelectric conversion efficiency of the final device. Compared with Example 5, Examples 7 and 8 respectively add 3.5 mol%, 2 mol%, and 5 mol% of 3-trifluoromethylpyridine to the pure inorganic tin-lead perovskite precursor mixed solution to obtain a perovskite precursor solution with a gradient doping amount. It can be found from Table 2 that in Example 5, when the doping amount of 3-trifluoromethylpyridine is 3.5 mol%, thanks to the effect of 3-trifluoromethylpyridine on Sn in the perovskite 2+ Oxidation inhibition and film crystallization modulation reduce the defects on the surface and grain boundaries of tin-lead perovskite, improve the film quality, significantly reduce the energy loss caused by non-radiative recombination, and the device has the highest open circuit voltage (V oc ), short circuit current (J sc ), fill factor (FF) and the final photoelectric conversion efficiency; at the same time, compared with Example 6, various parameters of Example 7 and Example 8 are improved to varying degrees, but the effects are not as good as Example 5, so according to the experimental results, it is determined that the additive used in Example 5 is the optimal doping amount.

Claims

1. A method for preparing a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine, characterized in that: The steps include: 1) Ultrasonic cleaning of the transparent conductive substrate, drying the transparent conductive substrate with a nitrogen stream before use, and then treating the surface of the transparent conductive substrate with a plasma cleaner or ozone; 2) depositing a hole transport layer HTL solution on the surface of the transparent conductive substrate treated in step 1), and performing annealing treatment to obtain a HTL film; 3) adding 3-trifluoromethylpyridine to the tin-containing perovskite precursor solution and stirring evenly to prepare a 3-trifluoromethylpyridine-doped tin-containing perovskite precursor solution, depositing the solution on the surface of the HTL film, and obtaining a tin-containing perovskite active layer after annealing; 4) subsequently depositing an electron transport layer and a hole blocking layer on the surface of the tin-containing perovskite active layer obtained in step 3); 5) depositing a top electrode on the surface of the thin film obtained in step 4), and finally obtaining a tin-containing perovskite solar cell based on 3-trifluoromethylpyridine-doped perovskite.

2. The method for preparing a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine according to claim 1, characterized in that: The transparent conductive substrate in step 1) is Glass / ITO or FTO, plastic flexible substrate / ITO or FTO, and the transparent conductive substrate is ultrasonically cleaned using distilled water, acetone, and isopropanol solvents in sequence.

3. The method for preparing a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine according to claim 1, characterized in that: The HTL solution in step 2) is one or more mixed materials of PEDOT:PSS, PTAA, MeO-2PACz, and 4PACz.

4. The method for preparing a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine according to claim 3, characterized in that: The HTL solution is spin-coated on the surface treated transparent conductive substrate, and then annealed to obtain a hole transport layer. The spin coating speed is 5000-6000 rpm and the spin coating time is 30-40 seconds. The annealing temperature is 90-110°C and the annealing time is 5-10 minutes.

5. The method for preparing a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine according to claim 1, characterized in that: The tin-containing perovskite precursor solution in step 3) is any organic-inorganic hybrid perovskite or inorganic perovskite containing metallic tin, and the thickness of the tin-containing perovskite active layer is 600-800 nm.

6. The method for preparing a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine according to claim 5, characterized in that: The tin-containing perovskite precursor solution described in step 3) is FA x MA 1-x Sn y Pb 1-y I3, 0 ≤ x ≤ 1, 0 < y ≤ 1 or CsSn x Pb 1-x I 2.7 Br 0.3 , 0 < x ≤ 1.

7. The method for preparing a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine according to claim 5, characterized in that: In step 3), the doping amount of 3-trifluoromethylpyridine is 1-5 mol% of the tin-containing perovskite precursor solution. 3-trifluoromethylpyridine is added to the tin-containing perovskite precursor solution and stirred for 0.5-1.5 hours, and then filtered through a polytetrafluoroethylene membrane to obtain a 3-trifluoromethylpyridine-doped tin-containing perovskite precursor solution.

8. The method for preparing a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine according to claim 5, characterized in that: In step 3), two-step spin coating deposition is performed, first at a rotation speed of 500-1000 rpm for 5-10 seconds, and then at a rotation speed of 4000-5000 rpm for 30-50 seconds. 10-20 seconds before the end of the second spin coating, 100-300 μL of ethyl acetate anti-solvent is dripped on the rotating substrate, and then the substrate is annealed to obtain a perovskite film at a temperature of 90-110° C. for 5-20 minutes.

9. The method for preparing a tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine according to claim 1, characterized in that: The electron transport layer in step 4) is PC 61 BM, PC 71 BM, C 60 , C 70 The hole blocking layer is BCP, and the top electrode in step 5) is a combination of one or more materials selected from Ag, Au, Cu, AZO, carbon materials, and conductive polymers.

10. A tin-containing perovskite solar cell doped with 3-trifluoromethylpyridine prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Perovskite quantum dot-polymer composite film and preparation method thereof

    CN114702949A

  • Perovskite solar cell modified by fluorinated pyridine molecular additive and preparation method thereof

    CN116113245A

Cited By

  • Preparation method of large-area tin-based narrow-band-gap perovskite thin film based on solvent engineering

    CN119836197A

  • Perovskite solar cell based on action of strong electron withdrawing group substituted fluoropyridine additive and preparation method thereof

    CN121152466A

  • Perovskite solar cell based on fluoropyridine additive with strong electron-withdrawing group substitution and preparation method thereof

    CN121152466B

  • SCEC-doped flexible narrow-band-gap perovskite solar cell and preparation method thereof

    CN122180238A

  • Flexible narrow-bandgap perovskite solar cells doped with SCEC and their fabrication method

    CN122180238B