Anti-adhesion biaxially oriented matte BOPA film and preparation method thereof

By using laminated structure of frosted surface layer and smooth surface layer and cage polyhedral oligosilsesquioxane as anti-adhesive agent in BOPA film, the adhesion problem is solved and barrier properties and anti-adhesion properties are improved, providing matte light The effect has improved the application value and competitiveness of packaging materials.

CN118977496APending Publication Date: 2024-11-19HESHAN YUNCHENG NEW MATERIAL CO LTD

Patent Information

Application Number
CN202411033277.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

BOPA films are prone to adhesion problems during production and use, and existing anti-adhesion agents may affect other properties when improving resistance to adhesion, such as barrier properties, mechanical properties, etc., and the commonly used coating methods are unstable in product quality and yield. Low and high cost.

Method used

Using a laminated structure of frosted surface layer and smooth surface layer, cage polyhedral oligosilsesquioxane (POSS) is used as the anti-adhesive agent, and anti-adhesive bidirectional stretched matte BOPA film is prepared through the twin-screw extrusion mechanism to add The roughness and hydrophobicity of the film surface reduce the friction coefficient and no additional additives are required to be added in the masterbatch production.

Benefits of technology

Improves the anti-adhesion and barrier properties of BOPA films, reduces hydrophilicity, increases the contact angle of water, extends the shelf life of food, protects pharmaceutical products from moisture, and provides matte effects, improving packaging The market competitiveness of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004970453030000111
    Figure BDA0004970453030000111
  • Figure BDA0004970453030000121
    Figure BDA0004970453030000121
Patent Text Reader

Abstract

The invention relates to the technical field of BOPA films, and discloses an anti-adhesion biaxially oriented matte BOPA film and a preparation method thereof.The anti-adhesion biaxially oriented matte BOPA film is composed of a frosted surface layer and a smooth surface layer, a matting agent, a dispersing agent, an anti-adhesion agent and a slipping agent are added to the frosted surface layer, and the smooth surface layer contains the anti-adhesion agent and the slipping agent. The nylon master batch is prepared from nylon 6 and cage-shaped polyhedral oligomeric silsesquioxane, so that the adhesion resistance and barrier property of the film are improved. The preparation method comprises the steps of raw material mixing, melt extrusion, cooling molding, two-way stretching and the like. The product is suitable for the packaging field with high barrier property requirements, such as food, medicine and cosmetic packaging, and has anti-adhesion and matte effects and excellent barrier property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of BOPA films, and in particular relates to an anti-adhesion biaxially stretched matte BOPA film and a preparation method thereof. Background Art

[0002] Biaxially oriented nylon film (BOPA) is a high-grade packaging material with high barrier properties, excellent crack resistance, impact resistance, tensile strength and puncture resistance, as well as wide resistance to acids, alkalis, greases and various common organic solvents, especially excellent barrier properties to greases and gases, and can extend the shelf life by more than double that of ordinary packaging materials. However, BOPA film also has some disadvantages, such as poor moisture absorption resistance, and the barrier properties will decrease after moisture absorption.

[0003] In recent years, BOPA film has been increasingly used in the fields of food, medicine, cosmetics, and mechanical and electronic packaging. It is especially suitable for frozen packaging, vacuum packaging, and steaming packaging, and the market prospects are very promising. With the rapid development of pre-prepared food and new energy vehicle industries, the domestic BOPA film market demand has risen. Therefore, the production and development of BOPA film has important practical significance.

[0004] In the production and use of BOPA film, the problem of film adhesion leading to film scrapping is often encountered. Especially in the automated, high-speed and high-quality plastic processing, factors such as static electricity, temperature and pressure generated by friction are more likely to cause adhesion between films. In order to solve this problem, anti-adhesion agents are usually added to BOPA films. By adding anti-adhesion agents to PA, blending, granulating and drying by a twin-screw extruder, anti-adhesion masterbatch is obtained. It is an important additive for the production of high-quality BOPA film.

[0005] At present, the commonly used anti-adhesion agents are mainly divided into two categories: inorganic and organic. Inorganic anti-adhesion agents include algae earth, talc, calcium carbonate, synthetic silica or glass beads, etc.; organic anti-adhesion agents are mainly represented by silicone polymers and methacrylates. The mechanism of action of these anti-adhesion agents is to form an uneven surface morphology on the surface of the film, thereby forming an air layer between the films to prevent adhesion. However, while improving the anti-adhesion properties of the film, other properties such as mechanical properties, optical properties, barrier properties, aging properties, etc. may be negatively affected. Therefore, other additives such as dispersants, lubricants, antioxidants, etc. need to be added to maintain the comprehensive performance of film products.

[0006] At present, matting material is usually applied on the surface of ordinary BOPA film by coating. This method requires two steps: production of ordinary BOPA film and coating of matting material on BOPA film on a coating machine. The product quality is unstable, the output is low, the process is cumbersome and the cost is high. Therefore, if a BOPA film with improved anti-blocking properties and barrier properties can be prepared, the added value and competitiveness of the product will be greatly improved.

[0007] Therefore, in order to solve the adhesion problem encountered in the production and use of the existing BOPA film and improve the barrier performance of the film, an anti-adhesion biaxially stretched matte BOPA film is proposed. Summary of the invention

[0008] In order to make up for the deficiencies of the prior art, the present invention provides an anti-adhesion biaxially stretched matte BOPA film and a preparation method thereof.

[0009] To achieve the above object, the present invention provides the following technical solutions:

[0010] An anti-adhesion biaxially stretched matte BOPA film comprises a frosted surface layer and a smooth surface layer, and the frosted surface layer and the smooth surface layer are stacked;

[0011] The frosted surface layer is prepared from the following raw materials in weight percentage: a dispersant, 0-2wt% of an anti-adhesive agent, 0-3wt% of a lubricant, 0.05-50wt% of a matting agent, and the balance is nylon resin, wherein the amount of the dispersant is 0-50wt% of the matting agent;

[0012] The smooth surface layer is prepared from the following raw materials in weight percentage: 0-2wt% of anti-adhesive agent, 0-2wt% of lubricant, and the balance is nylon resin.

[0013] Preferably, the matting agent is an inorganic filler and is selected from a mixture of any one or more of silicon dioxide, talc, calcium carbonate, titanium dioxide, aluminum oxide, and diatomaceous earth.

[0014] Preferably, the dispersant is selected from any one or more mixtures of polyethylene glycol, polyvinyl pyrrolidone, polyacrylates, polyisobutylene, surfactants, and fatty acid esters.

[0015] Preferably, the lubricant is selected from any one or more mixtures of zinc stearate, calcium stearate, dimethyl silicone oil, methylphenyl silicone oil, stearic acid, oleic acid, polytetrafluoroethylene, and polyethylene wax.

[0016] Preferably, the anti-adhesive agent is a nylon masterbatch, and its raw materials include the following components in mass percentage: 90-95% PA6 (nylon 6), 5-10% cage-shaped polyhedral oligomeric silsesquioxane (POSS). The typical molecular formula of cage-shaped polyhedral oligomeric silsesquioxane (POSS) is R7R'(SiO1.5)8, and its core is a cage-shaped inorganic skeleton composed of silicon and oxygen, and the vertex Si is connected to the group R extending into the space, R is H, alkyl, alkenyl, aryl, aralkenyl or its derivative group, and R' is an active functional group.

[0017] Cage-shaped polyhedral oligomeric silsesquioxane (POSS) is used as an anti-adhesion agent, and its nano effect is utilized to form fine aggregated micro-regions on the surface of the BOPA film, thereby increasing the roughness of the film surface and reducing the friction coefficient between the films; on the other hand, the addition of POSS can reduce the surface polarity of the BOPA film, increase the hydrophobicity of the BOPA film, reduce water penetration, and thus improve the barrier properties of the BOPA film, while not adversely affecting its mechanical properties; furthermore, no other additives need to be added during the production process of the masterbatch.

[0018] Preferably, the method for preparing the nylon masterbatch comprises the following steps:

[0019] a) using a precision loss-in-weight self-feeding system, nylon 6 (PA6) and cage-shaped polyhedral oligomeric silsesquioxane (POSS) are added by weight to a twin-screw extruder;

[0020] b) after being fully mixed, the melt is extruded and granulated;

[0021] c) placing the produced masterbatch into a vacuum dryer for drying to obtain a finished nylon masterbatch.

[0022] Preferably, the screw temperature of the twin-screw extruder is 230-260°C, the main engine speed is controlled at 50-120 rpm, the feeding speed is 50-100 kg / h; the pelletizer speed is set at 16-21HZ;

[0023] Preferably, the masterbatch is dried in a vacuum dryer at 100-150° C. for 16-24 hours.

[0024] A method for preparing an anti-adhesion biaxially stretched matte BOPA film comprises the following steps:

[0025] S1. Mix the raw materials of the frosted surface layer and the smooth surface layer evenly;

[0026] S2, placing the mixed raw materials of each layer in a corresponding extruder, melting the raw materials by heating and rotating the screw, and extruding the molten raw materials through a common die head to form a layered structure;

[0027] S3, cooling and molding the layered structure to obtain a crude nylon film;

[0028] S4, biaxially stretching the crude nylon film, heat-setting, corona treating, and rolling up to obtain a matte BOPA film product.

[0029] Preferably, the extruder temperature is 200-290°C, the die temperature of the extruder is 230-270°C, and the cooling molding temperature is 20-30°C;

[0030] The biaxial stretching is synchronous biaxial stretching or step-by-step biaxial stretching;

[0031] The synchronous biaxial stretching temperature is 60-180℃, the longitudinal stretching multiple and the transverse stretching multiple are 2.8-3.5 times, and the heat setting temperature is 150-220℃;

[0032] The longitudinal stretching temperature of the step-by-step biaxial stretching is 45-100°C, the longitudinal stretching multiple is 2.8-3.5 times, the transverse stretching temperature is 80-160°C, the transverse stretching multiple is 2.8-3.5 times; the heat setting temperature is 150-220°C.

[0033] Compared with the prior art, the technical effects and advantages of the present invention are as follows: the anti-adhesion biaxially stretched matte BOPA film and its preparation method are prepared by mixing nylon masterbatch prepared from nylon 6 and cage-shaped polyhedral oligomeric silsesquioxane with additives (dispersant, lubricant) and nylon resin to prepare the anti-adhesion biaxially stretched matte BOPA film, and the BOPA film prepared from the nylon masterbatch improves the anti-adhesion property while reducing the hydrophilicity of the BOPA film, increasing the contact angle with water, thereby improving the barrier performance of the BOPA film, and thus obtaining an anti-adhesion biaxially stretched matte BOPA film. Such innovation helps to enhance the application value of BOPA film in the packaging industry, especially in fields with high requirements for the barrier performance of packaging materials, such as food, medicine and cosmetics packaging.

[0034] By using anti-blocking functional masterbatch to prepare BOPA film, the hydrophilicity of the film can be reduced while improving the anti-blocking property. Reduced hydrophilicity means that the contact angle between the film and water increases, which helps to reduce the adsorption and penetration of water molecules, thereby improving the barrier properties of the film. In food packaging, this can extend the shelf life of food and prevent food deterioration caused by moisture and oxygen. In pharmaceutical packaging, it can protect drugs from moisture and maintain the effectiveness and stability of drugs.

[0035] In addition, the preparation of anti-blocking biaxially oriented matte BOPA film not only solves the blocking problem, but also provides a matte effect, which makes the film more attractive in the high-end packaging material market. The matte surface can reduce light reflection and improve the brand recognition of packaging materials, while also potentially providing additional protection for certain products.

[0036] In short, by developing anti-adhesion BOPA film functional masterbatch and preparing anti-adhesion biaxially oriented matte BOPA film, the barrier properties of BOPA film can be improved without sacrificing other properties, meeting the packaging industry's demand for high-performance packaging materials, thereby increasing the added value and market competitiveness of the product. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] The present application discloses an anti-adhesion biaxially stretched matte BOPA film, comprising a frosted surface layer and a smooth surface layer, and the frosted surface layer and the smooth surface layer are stacked;

[0039] The frosted surface layer is prepared from the following raw materials in weight percentage: a dispersant, 0-2wt% of an anti-adhesive agent, 0-3wt% of a lubricant, 0.05-50wt% of a matting agent, and the balance is nylon resin, wherein the amount of the dispersant is 0-50wt% of the matting agent;

[0040] The smooth surface layer is prepared from the following raw materials in weight percentage: 0-2wt% of anti-adhesive agent, 0-2wt% of lubricant, and the balance is nylon resin.

[0041] The matting agent is an inorganic filler and is selected from a mixture of any one or more of silicon dioxide, talc, calcium carbonate, titanium dioxide, aluminum oxide, and diatomaceous earth. The matting agent is an additive used to reduce the surface gloss of the material and make it present a matte effect. In the production of nylon film, the matting agent can be used to be evenly dispersed in the frosted surface layer, thereby forming tiny unevenness on the surface of the film, reducing the reflection of light, and making the surface of the film present a matte effect.

[0042] The dispersant is selected from any one or more mixtures of polyethylene glycol, polyvinyl pyrrolidone, polyacrylates, polyisobutylene, surfactants, and fatty acid esters. In the production of nylon film, the dispersant can be used to help inorganic powders (such as silicon dioxide, talcum powder, etc.) to be evenly dispersed in the nylon resin, thereby improving the performance of the film. The selection and dosage of the dispersant have an important influence on the performance and quality of the final product.

[0043] The lubricant is selected from any one or more of zinc stearate, calcium stearate, dimethyl silicone oil, methylphenyl silicone oil, stearic acid, oleic acid, polytetrafluoroethylene, and polyethylene wax. The lubricant is an additive used to reduce friction between materials and improve the sliding properties of the material surface. In the production of nylon film, the lubricant can be used to improve the fluidity of the film during processing, reduce friction between the film and equipment, thereby improving production efficiency and reducing wear.

[0044] The frosted surface layer is designed to form roughness on the surface of the film, thereby increasing the air layer, reducing direct contact between films, and preventing adhesion. The smooth surface layer is used to provide a matte effect to the film while maintaining other properties of the film, such as mechanical properties and barrier properties. The two layers are superimposed and reorganized to form a matte BOPA film. This design not only solves the adhesion problem, but also provides a matte effect, improving the market competitiveness of the film.

[0045] The anti-adhesive agent is a nylon masterbatch. A precision weightless self-metering feeding system is used to add 90-95% of PA6 (nylon 6) and 5-10% of cage-shaped polyhedral oligomeric silsesquioxane (POSS) in a weight ratio into a twin-screw extruder; after being fully mixed, the melt is extruded into granules; the screw temperature is 230-260° C., the main engine speed is controlled at 50-120 rpm, the feeding speed is 50-100 kg / hour, the pelletizer speed is set at 16-21 Hz, and the produced masterbatch is placed in a vacuum dryer and dried in the vacuum dryer at 100-150° C. for 16-24 hours to obtain a nylon masterbatch finished product.

[0046] A method for preparing an anti-adhesion biaxially stretched matte BOPA film comprises the following steps:

[0047] S1. Mix the raw materials of the frosted surface layer and the smooth surface layer evenly;

[0048] In this step, the raw materials of the frosted surface layer and the smooth surface layer need to be mixed together in the required ratio. Generally, the raw materials of the frosted surface layer include dispersants, anti-blocking agents, lubricants and matting agents, while the raw materials of the smooth surface layer mainly include anti-blocking agents, lubricants and nylon resins. These raw materials should be mixed evenly to ensure the surface quality and performance of the final film.

[0049] S2. Place the mixed raw materials of each layer in a corresponding extruder, melt the raw materials by heating and rotating the screw, and extrude the molten raw materials through a common die to form a layered structure; the extruder temperature is 200-290°C, and the die temperature of the extruder is 230-270°C.

[0050] S3, cooling and molding the layered structure to obtain a crude nylon film; the cooling and molding temperature is 20-30°C;

[0051] S4. Biaxially stretch the crude nylon film to make it have better mechanical and physical properties, heat set and corona treat to make the surface of the matte BOPA film smoother, while improving its barrier properties and anti-adhesion properties, and then roll up to obtain the matte BOPA film product.

[0052] The crude nylon film is biaxially stretched to give it better mechanical and physical properties. The stretched film is heat-set to eliminate deformation caused by temperature changes, and finally corona treated to improve the surface smoothness and hydrophilicity of the film, thereby improving its barrier properties and anti-adhesion properties.

[0053] The biaxial stretching is synchronous biaxial stretching or step-by-step biaxial stretching;

[0054] The synchronous biaxial stretching temperature is 60-180℃, the longitudinal stretching multiple and the transverse stretching multiple are 2.8-3.5 times, and the heat setting temperature is 150-220℃;

[0055] The longitudinal stretching temperature of the step-by-step biaxial stretching is 45-100°C, the longitudinal stretching multiple is 2.8-3.5 times, the transverse stretching temperature is 80-160°C, the transverse stretching multiple is 2.8-3.5 times; the heat setting temperature is 150-220°C.

[0056] Example 1

[0057] A frosted surface layer raw material consisting of 2wt% of an anti-blocking agent, 3wt% of a lubricant, 50wt% of a matting agent, a balance of nylon resin, and a dispersant in an amount of 50wt% of the matting agent, and a smooth surface layer raw material consisting of 2wt% of an anti-blocking agent, 2wt% of a lubricant, and a balance of nylon resin are mixed evenly, and the mixed raw materials of each layer are placed in an extruder with an extruder temperature of 200°C and a die temperature of 230°C, and the raw materials are melted by heating and screw rotation, and the molten raw materials are extruded through a common die to form a layered structure, and the layered structure is cooled and formed at 20°C to obtain a crude nylon film, and the crude nylon film is biaxially stretched at a longitudinal stretching temperature of 45°C and a longitudinal stretching multiple of 2.8 times, and a transverse stretching temperature of 80°C and a transverse stretching multiple of 2.8 times, and heat-set at 150°C, corona-treated, and rolled to obtain a matte BOPA film product.

[0058] Example 2

[0059] A frosted surface layer raw material consisting of 2wt% of an anti-blocking agent, 3wt% of a lubricant, 50wt% of a matting agent, a balance of nylon resin, and a dispersant in an amount of 50wt% of the matting agent, and a smooth surface layer raw material consisting of 2wt% of an anti-blocking agent, 2wt% of a lubricant, and a balance of nylon resin are mixed evenly, and the mixed raw materials of each layer are placed in an extruder with an extruder temperature of 290°C and a die head temperature of 270°C, and the raw materials are melted by heating and screw rotation, and the molten raw materials are extruded through a common die head to form a layered structure, and the layered structure is cooled and formed at 30°C to obtain a crude nylon film, and the crude nylon film is biaxially stretched at a longitudinal stretching temperature of 100°C and a longitudinal stretching multiple of 3.5 times, and a transverse stretching temperature of 160°C and a transverse stretching multiple of 3.5 times, and heat-set and corona-treated at 220°C, and rolled to obtain a matte BOPA film product.

[0060] Example 3

[0061] A frosted surface layer raw material consisting of 1wt% of an anti-blocking agent, 2wt% of a lubricant, 40wt% of a matting agent, a balance of nylon resin, and a dispersant in an amount of 25wt% of the matting agent, and a smooth surface layer raw material consisting of 1wt% of an anti-blocking agent, 1wt% of a lubricant, and a balance of nylon resin are mixed evenly, and the mixed raw materials of each layer are placed in an extruder with an extruder temperature of 200°C and a die temperature of 230°C, and the raw materials are melted by heating and screw rotation, and the molten raw materials are extruded through a common die to form a layered structure, and the layered structure is cooled and formed at 20°C to obtain a crude nylon film, and the crude nylon film is biaxially stretched at a longitudinal stretching temperature of 45°C and a longitudinal stretching multiple of 2.8 times, and a transverse stretching temperature of 80°C and a transverse stretching multiple of 2.8 times, and heat-set at 150°C, corona-treated, and rolled to obtain a matte BOPA film product.

[0062] Example 4

[0063] A frosted surface layer raw material consisting of 1wt% of an anti-blocking agent, 2wt% of a lubricant, 40wt% of a matting agent, a balance of nylon resin, and a dispersant in an amount of 25wt% of the matting agent, and a smooth surface layer raw material consisting of 1wt% of an anti-blocking agent, 1wt% of a lubricant, and a balance of nylon resin are mixed evenly, and the mixed raw materials of each layer are placed in an extruder with an extruder temperature of 290°C and a die temperature of 270°C, and the raw materials are melted by heating and screw rotation, and the molten raw materials are extruded through a common die to form a layered structure, and the layered structure is cooled and formed at 30°C to obtain a crude nylon film, and the crude nylon film is biaxially stretched at a longitudinal stretching temperature of 100°C and a longitudinal stretching multiple of 3.5 times, and a transverse stretching temperature of 160°C and a transverse stretching multiple of 3.5 times, and heat-set at 220°C, corona treatment, and rolled to obtain a matte BOPA film product.

[0064] Example 5

[0065] A frosted surface layer raw material consisting of 2wt% of an anti-blocking agent, 3wt% of a lubricant, 50wt% of a matting agent, a balance of nylon resin, and a dispersant in an amount of 45wt% of the matting agent, and a smooth surface layer raw material consisting of 2wt% of an anti-blocking agent, 2wt% of a lubricant, and a balance of nylon resin are mixed evenly, and the mixed raw materials of each layer are placed in an extruder with an extruder temperature of 250°C and a die head temperature of 250°C, and the raw materials are melted by heating and screw rotation, and the molten raw materials are extruded through a common die head to form a layered structure, and the layered structure is cooled and formed at 25°C to obtain a crude nylon film, and the crude nylon film is biaxially stretched at a longitudinal stretching temperature of 60°C and a longitudinal stretching multiple of 3.2 times, and a transverse stretching temperature of 110°C and a transverse stretching multiple of 3.1 times, and is heat-set and corona-treated at 195°C, and rolled to obtain a matte BOPA film product.

[0066] Example 6

[0067] A frosted surface layer raw material consisting of 1.5wt% of an anti-blocking agent, 2.5wt% of a lubricant, 5wt% of a matting agent, a balance of nylon resin, and a dispersant in an amount of 50wt% of the matting agent, and a smooth surface layer raw material consisting of 1.5wt% of an anti-blocking agent, 1.5wt% of a lubricant, and a balance of nylon resin are mixed evenly, and the mixed raw materials of each layer are placed in an extruder with an extruder temperature of 260°C and a die temperature of 245°C, and the raw materials are melted by heating and screw rotation, and the molten raw materials are extruded through a common die to form a layered structure, and the layered structure is cooled and formed at 24°C to obtain a crude nylon film, and the crude nylon film is biaxially stretched at a longitudinal stretching temperature of 70°C and a longitudinal stretching multiple of 3.4 times, and a transverse stretching temperature of 130°C and a transverse stretching multiple of 3.0 times, and is heat-set at 180°C, corona-treated, and rolled to obtain a matte BOPA film product.

[0068] In order to draw the conclusion that BOPA film improves anti-blocking property while reducing hydrophilicity of BOPA film, increasing contact angle with water, and thus improving barrier property of BOPA film, a series of performance tests are required for BOPA film. The following are some key test items:

[0069] 1. Anti-adhesion test:

[0070] Adhesion test: Evaluate the degree of adhesion of the film to other materials (such as packaging materials, containers, etc.) under specific conditions.

[0071] Anti-blocking index: Measures the coefficient of friction of a film surface to evaluate its anti-blocking performance in practical applications.

[0072] 2. Hydrophilicity test:

[0073] Contact angle measurement: The hydrophilicity of the film is evaluated by measuring the contact angle between the film surface and a water droplet. The larger the contact angle, the lower the hydrophilicity of the film.

[0074] Water absorption test: Evaluate the degree of water absorption of the film to understand the hydrophilicity of the film.

[0075] 3. Barrier performance test:

[0076] Oxygen permeability test: measures the oxygen barrier properties of the film.

[0077] Water vapor transmission rate test: measure the barrier properties of the film to water vapor.

[0078] Organic gas permeability test: measures the barrier properties of the film to specific organic gases.

[0079] 4. Mechanical properties test:

[0080] Tensile strength test: Evaluate the maximum stress of the film during stretching.

[0081] Elongation at Break Test: Evaluates the percentage of elongation a film can achieve before breaking.

[0082] 5. Appearance and gloss test:

[0083] Surface roughness test: Evaluate the surface roughness of the frosted surface layer.

[0084] Gloss test: measure the gloss of the film surface to evaluate the effect of the matting agent.

[0085] By testing and analyzing these properties, it can be concluded whether the addition of specific dispersants, anti-blocking agents and matting agents to BOPA films improves anti-blocking properties while reducing hydrophilicity, thereby improving barrier properties. These tests usually need to be carried out according to specific standards or methods to ensure the accuracy and repeatability of the results. The test results should be compared with BOPA films without specific additives (comparative examples) to evaluate the impact of additives on film properties.

[0086] During the test, the adhesion test is to contact the film with the packaging material for 24 hours; the anti-adhesion index test is to rub the film surface with a specific surface; the contact angle measurement is to contact the film surface with a water droplet; the water absorption test is to immerse the film in water for 2 hours; the oxygen permeability test is to measure the oxygen pressure difference on both sides of the film; the water vapor permeability test is to measure the water vapor pressure difference on both sides of the film; the organic gas permeability test is to measure the specific organic gas pressure difference on both sides of the film; the tensile strength test is to stretch the film at a certain speed, the elongation at break test is to stretch the film at a certain speed, the surface roughness test is to use a surface roughness meter to test the roughness value, and the gloss test is to measure the gloss of the film surface.

[0087]

[0088]

[0089] Based on the test results provided, the following conclusions can be drawn:

[0090] The films of all examples showed no adhesion in the blocking test, while the films of the control group showed slight adhesion. This shows that the added anti-blocking agent effectively improves the anti-blocking performance of the BOPA film. The friction coefficients of the films of all examples are low, especially the friction coefficient μ of Example 6 is 0.09, which is much lower than 3.5μ of the control group. This shows that the friction coefficient of the film surface has been significantly reduced, which helps to improve its slipperiness. The contact angles of the films of all examples are greater than 90°, among which the contact angle of Example 6 is the highest at 92°, while the contact angle of the control group is 65°. This shows that the hydrophobicity of the film has been enhanced, which helps to improve the barrier performance.

[0091] The water absorption rate of the films of all embodiments is low, which indicates that the hydrophilicity of the films is weakened and the hydrophobicity is enhanced, which helps to improve the barrier performance. The OTR values ​​of all embodiments are low, which indicates that the barrier performance of the films to oxygen has been significantly improved. The WVTR values ​​of all embodiments are also low, which indicates that the barrier performance of the films to water vapor has also been improved. The organic gas permeability values ​​of all embodiments are also low, which indicates that the barrier performance of the films to specific organic gases has also been improved. The tensile strength values ​​of all embodiments are high, which indicates that the mechanical strength of the films has been enhanced. The elongation values ​​of all embodiments are also high, which indicates that the toughness of the films has been improved. The surface roughness values ​​of all embodiments are low, which indicates that the flatness of the film surface is improved, which helps to improve the appearance and improve the barrier performance. The gloss values ​​of all embodiments are low, which indicates that the gloss of the film surface is reduced, which helps to provide a matte appearance.

[0092] In summary, the anti-adhesion biaxially stretched matte BOPA film and its preparation method can significantly improve the anti-adhesion performance, reduce the friction coefficient, improve the smoothness, improve the hydrophobicity, reduce the water absorption rate, and improve the barrier performance. Reduce the oxygen and water vapor permeability, improve the gas barrier performance, improve the barrier performance of organic gases, enhance the mechanical strength and toughness, improve the appearance, and provide a matte effect.

[0093] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An anti-adhesion biaxially stretched matte BOPA film, characterized in that: It includes a frosted surface layer and a smooth surface layer, and the frosted surface layer and the smooth surface layer are stacked; The frosted surface layer is prepared from the following raw materials in weight percentage: a dispersant, 0-2wt% of an anti-adhesive agent, 0-3wt% of a lubricant, 0.05-50wt% of a matting agent, and the balance is nylon resin, wherein the amount of the dispersant is 0-50wt% of the matting agent; The smooth surface layer is prepared from the following raw materials in weight percentage: 0-2wt% of anti-adhesive agent, 0-2wt% of lubricant, and the balance is nylon resin.

2. The anti-adhesion biaxially stretched matte BOPA film according to claim 1, characterized in that: The matting agent is an inorganic filler and is selected from any one or more mixtures of silicon dioxide, talc, calcium carbonate, titanium dioxide, aluminum oxide, and diatomaceous earth.

3. The anti-adhesion biaxially stretched matte BOPA film according to claim 1, characterized in that: The dispersant is selected from any one or more mixtures of polyethylene glycol, polyvinyl pyrrolidone, polyacrylates, polyisobutylene, surfactants, and fatty acid esters.

4. The anti-adhesion biaxially stretched matte BOPA film according to claim 1, characterized in that: The lubricant is selected from any one or more mixtures of zinc stearate, calcium stearate, dimethyl silicone oil, methylphenyl silicone oil, stearic acid, oleic acid, polytetrafluoroethylene, and polyethylene wax.

5. The anti-adhesion biaxially stretched matte BOPA film according to claim 1, characterized in that: The anti-adhesive agent is a nylon masterbatch, and its raw materials include the following components in percentage by mass: 90-95% PA6 and 5-10% cage-shaped polyhedral oligomeric silsesquioxane.

6. The anti-adhesion biaxially stretched matte BOPA film according to claim 5, characterized in that: The preparation method of the nylon masterbatch comprises the following steps: a) using a precision loss-in-weight self-metering feeding system, adding nylon 6 and cage-shaped polyhedral oligomeric silsesquioxane according to weight ratio into a twin-screw extruder; b) after being fully mixed, the melt is extruded and granulated; c) placing the produced masterbatch into a vacuum dryer for drying to obtain a finished nylon masterbatch.

7. The anti-adhesion biaxially stretched matte BOPA film according to claim 6, characterized in that: The screw temperature of the twin-screw extruder is 230-260°C, the main engine speed is controlled at 50-120 rpm, the feeding speed is 50-100 kg / h; the pelletizer speed is set at 16-21HZ.

8. The anti-adhesion biaxially stretched matte BOPA film according to claim 6, characterized in that: The masterbatch is dried in a vacuum dryer at 100-150°C for 16-24 hours.

9. A method for preparing the anti-adhesion biaxially stretched matte BOPA film according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1. Mix the raw materials of the frosted surface layer and the smooth surface layer evenly; S2, placing the mixed raw materials of each layer in a corresponding extruder, melting the raw materials by heating and rotating the screw, and extruding the molten raw materials through a common die head to form a layered structure; S3, cooling and molding the layered structure to obtain a crude nylon film; S4, biaxially stretching the crude nylon film, heat-setting, corona treating, and rolling up to obtain a matte BOPA film product.

10. The method for preparing an anti-adhesion biaxially stretched matte BOPA film according to claim 9, characterized in that: The extruder temperature is 200-290°C, the die head temperature of the extruder is 230-270°C, and the cooling molding temperature is 20-30°C; The biaxial stretching is synchronous biaxial stretching or step-by-step biaxial stretching; The synchronous biaxial stretching temperature is 60-180℃, the longitudinal stretching multiple and the transverse stretching multiple are 2.8-3.5 times, and the heat setting temperature is 150-220℃; The longitudinal stretching temperature of the step-by-step biaxial stretching is 45-100°C, the longitudinal stretching multiple is 2.8-3.5 times, the transverse stretching temperature is 80-160°C, the transverse stretching multiple is 2.8-3.5 times; the heat setting temperature is 150-220°C.

Citation Information

Patent Citations

  • Functional master batch for antisticking BOPA film and production process thereof

    CN102206412A

  • Biaxially oriented matte BOPA (Biaxially oriented polyamide film) thin film and preparation method thereof

    CN102924905A

Cited By

  • Special functional masterbatch for biaxially oriented polyamide film and preparation method and application thereof

    CN122854788A