Preparation method of light conversion antireflection film and light conversion antireflection film
By forming the light-to-reflective film of YVO4:Eu3+, Bi3+ and SiO2@YVO4:Eu3+ sol on the glass of photovoltaic module, the problem of narrow absorption range and poor UV resistance in industrial production is solved. Efficient optical performance improvement and cost reduction are achieved.
Patent Information
- Application Number
- CN202411070515.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
Existing rare earth doped downconversion materials have problems in industrial production, such as narrow absorption range, high cost and poor UV resistance, especially in photovoltaic module glasses.
The synthesis of YVO4:Eu3+, Bi3+ sol and SiO2@YVO4:Eu3+, Bi3+ solutions is adopted to form a double-layer light-to-reflection coating technology on the glass substrate, including plating an anti-reflection film layer, to improve the Light transmittance and UV resistance.
It significantly improves the power output of photovoltaic modules, expands the light conversion range, enhances the UV resistance, improves the optical utilization efficiency, and reduces the preparation cost, making it suitable for large-scale industrial applications.
Smart Images

Figure CN118978343A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of optical thin film materials, and in particular to a preparation method of a light-converting anti-reflection film and the light-converting anti-reflection film. Background Art
[0002] The application of rare earth doped down conversion materials in crystalline silicon solar cells is mainly to improve the performance of the cells by increasing the absorption efficiency and conversion efficiency of sunlight.
[0003] However, despite the remarkable progress made in the laboratory, rare earth doped down-conversion materials still face some challenges in industrial production, such as the absorption range, cost and preparation process of down-conversion materials. Prior art CN115557709A discloses an anti-reflection type light-converting glass film layer and a preparation method thereof, which uses a coating liquid as a carrier, combines it with a precursor of a down-conversion material, and evenly coats it on the glass surface, and then prepares an anti-reflection type light-converting glass film layer in situ by co-firing. Compared with traditional coated glass, the light transmittance is greatly improved. However, the light-converting glass film layer prepared by this method has poor anti-ultraviolet effect, obvious emission spectrum decay, and an excitation peak at 280nm, with a narrow absorption wavelength range. Summary of the invention
[0004] In order to solve the problems in the prior art, the first aspect of the present invention provides a method for preparing a light-converting anti-reflection film, which comprises at least a down-conversion sol YVO4:Eu 3+ ,Bi 3+ Synthesis of SiO2@YVO4:Eu 3+ ,Bi 3+ The steps of solution synthesis and light conversion anti-reflection coating are described; the anti-reflection coating step includes coating an anti-reflection film layer.
[0005] In one embodiment, the method for preparing the light-converting anti-reflection film specifically comprises the following steps:
[0006] (1) Down-conversion sol YVO4:Eu 3+ ,Bi 3+ Synthesis: rare earth metal oxide 1, sensitizer, acid solution, metal chelator 1 are mixed and dissolved to obtain solution A; rare earth metal oxide 2 and acid solution are mixed and dissolved to obtain solution B; solution A is mixed with solution B, ammonium salt and caustic soda are added to pH 4, and then reacted for 1 h, and cooled to room temperature to obtain down-conversion sol YVO4:Eu 3+ ,Bi 3+ .
[0007] (2)SiO2@YVO4:Eu 3+ ,Bi 3+Solution synthesis: After ethyl orthosilicate, deionized water, organic solvent, and metal chelating agent 2 are mixed to form sol 1, the sol 1 is mixed with the down-conversion sol obtained in step (1) until the solution is clear, transparent, and uniform to obtain SiO2@YVO4:Eu 3+ ,Bi 3+ Solution.
[0008] (3) Light conversion anti-reflection coating: After cleaning the glass substrate, place it in a glass substrate containing the SiO2@YVO4:Eu prepared in step (2) 3 + ,Bi 3+ The solution is placed in an immersion and pulling box, and after immersion, curing and sintering, an anti-reflection film layer is plated to obtain a light conversion and anti-reflection film.
[0009] In one embodiment, the acid solution in step (1) is a mixed solution of a strong acid and deionized water.
[0010] In one embodiment, the mass ratio of the strong acid to deionized water is (0.1-1):(1-100).
[0011] In one embodiment, the strong acid is selected from one or more of nitric acid, sulfuric acid, and hydrochloric acid.
[0012] In one embodiment, the strong acid is nitric acid; the nitric acid is concentrated nitric acid with a mass fraction of 68%.
[0013] In one embodiment, the mixing reaction temperature of solution A and solution B in step (1) is 40°C-90°C.
[0014] In one embodiment, the glass substrate in step (3) is ultra-white glass with a size of 4.5 cm*9 cm.
[0015] In one embodiment, the cleaning step in step (3) is as follows: taking ultra-white glass of 4.5 cm*9 cm in size, ultrasonically shaking with alkaline solution for 20 minutes, and rinsing with deionized water and ethanol.
[0016] In one embodiment, the specific steps of step (3) are as follows: take ultra-white glass of 4.5 cm*9 cm, use alkaline solution for ultrasonic vibration for 20 minutes, rinse with deionized water and ethanol, and then put in the glass containing SiO2@YVO4:Eu prepared in step (2) 3 + ,Bi 3+The solution is immersed in a pulling box with a humidity of 30% to 40%. The solution is immersed for 1 min to 3 min and the pulling speed is 3000 μm / s. After curing in the air for 1 min to 5 min, it is sintered at 700°C to 1300°C for 2 min to 10 min. After natural cooling to obtain a light-converting glass film layer, an anti-reflection film layer is plated, immersed for 1 min to 3 min, cured in the air, and sintered again at 700°C to 1300°C for 2 min to 10 min. After cooling, the coating process is completed to obtain a light-converting anti-reflection film.
[0017] In one embodiment, the anti-reflection coating layer is prepared from a photovoltaic anti-reflection coating liquid.
[0018] In one embodiment, the photovoltaic anti-reflection coating liquid is purchased from Chenguang (Changzhou) New Material Technology Co., Ltd. with the product number CG105.
[0019] In one embodiment, in step (1), the mass ratio of rare earth metal oxide 1, rare earth metal oxide 2, sensitizer, metal chelating agent 1, and ammonium salt is (1-3):(1-20):(1-10):(1-20):(1-20).
[0020] In one embodiment, in step (1), the mass ratio of rare earth metal oxide 1, rare earth metal oxide 2, sensitizer, metal chelating agent 1, and ammonium salt is 0.84:8.6:3.3:5.6:9.2.
[0021] Rare earth metal oxide 1 acts as a luminescent center and can emit long waves for absorption by solar cells. Rare earth metal oxide 2 and ammonium salt act as stable matrices, maintaining chemical stability while absorbing ultraviolet light to a large extent. On the one hand, the sensitizer can red-shift the absorbed ultraviolet light, increase the excitation range, and conform to the absorption range of solar cells. On the other hand, it can absorb ultraviolet light and transmit it to the luminescent center. The present application has found that when the mass ratio of rare earth metal oxide 1, rare earth metal oxide 2, sensitizer, metal chelator 1, and ammonium salt is (1-3): (1-20): (1-10): (1-20): (1-20), especially when the mass ratio of the four is 0.84: 8.6: 3.3: 5.6: 9.2, the rare earth metal oxide can be prevented from quenching, and the down-conversion material can be made to emit light efficiently.
[0022] In one embodiment, in step (2), the mass ratio of ethyl orthosilicate, deionized water, organic solvent, and metal chelating agent 2 is (1-3): (1-20): (1-100): (0.5-5).
[0023] In one embodiment, in step (2), the mass ratio of ethyl orthosilicate: deionized water: organic solvent: metal chelating agent 2 is 2:10:40:1.
[0024] In one embodiment, the mass ratio of the down-conversion sol in step (1) to the sol 1 in step (2) is (1-10):(0.1-1).
[0025] In one embodiment, the mass ratio of the down-conversion sol in step (1) to the sol 1 in step (2) is 10:1.
[0026] The present application study found that when the mass ratio of the lower conversion sol to sol 1 is (1-10):(0.1-1), especially when the mass ratio of the lower conversion sol to sol 1 is 10:1, large-area agglomeration on the film surface can be prevented, ensuring good film formation and uniform luminescence.
[0027] In one embodiment, the rare earth metal oxide 1 or the rare earth metal oxide 2 is selected from one or more of yttrium oxide, lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, samarium oxide, europium oxide, gadolinium oxide, thulium oxide, dysprosium oxide, holmium oxide, erbium oxide, thulium oxide, ytterbium oxide, and lutetium oxide.
[0028] In one embodiment, the rare earth metal oxide 1 is europium oxide.
[0029] In one embodiment, the rare earth metal oxide 2 is yttrium oxide.
[0030] In one embodiment, the metal chelator 1 or the metal chelator 2 is selected from one or more of ethylenediaminetetraacetic acid, citric acid, ethylenediaminetetraacetic acid, ethylenediaminetetraacetic acid disodium salt, ethylenediaminetetraacetic acid tetrasodium salt, and disodium nitrilotriacetate.
[0031] In one embodiment, the metal chelator 1 and the metal chelator 2 are the same substance, both of which are citric acid.
[0032] In one embodiment, the citric acid is anhydrous citric acid.
[0033] In one embodiment, the sensitizer is selected from one or more of bismuth oxide, calcium oxide, magnesium oxide, and barium oxide.
[0034] In one embodiment, the sensitizer is bismuth oxide.
[0035] In one embodiment, the organic solvent is selected from one or more of styrene, perchloroethylene, trichloroethylene, ethylene glycol ether, triethanolamine, ethanol, methanol, and isopropanol.
[0036] In one embodiment, the organic solvent is ethanol.
[0037] In one embodiment, the ammonium salt is selected from one or more of ammonium chloride, ammonium sulfate, ammonium bisulfate, ammonium nitrate, ammonium carbonate, ammonium bicarbonate, ammonium fluoride, ammonium iodide, ammonium bromide, and ammonium metavanadate.
[0038] In one embodiment, the ammonium salt is ammonium metavanadate.
[0039] A second aspect of the present invention provides a light-conversion anti-reflection film, which is prepared by adopting the above-mentioned method for preparing the light-conversion anti-reflection film.
[0040] Beneficial Effects
[0041] 1. The present invention solves the shading problem when the down-conversion material is applied to the glass of photovoltaic modules, and at the same time improves the efficiency of the conversion material, thereby increasing the power of the applied photovoltaic modules.
[0042] 2. The present invention coats a solution containing SiO2 sol and down-conversion sol material on the surface of photovoltaic glass, and then calcines it to obtain a bottom-coated light-conversion glass film layer. After cooling, an anti-reflection layer is plated on the structure of the bottom film layer. The double-layer structure of the light-conversion glass film layer and the anti-reflection layer is adopted. Compared with traditional coated glass, the light transmittance is maintained at a higher level and the anti-ultraviolet effect is significant. At the same time, part of the ultraviolet light can be converted into red light with a wavelength of 600 to 700 nm, thereby improving the optical utilization efficiency of the photovoltaic cell.
[0043] 3. The light-converting anti-reflection film prepared by the present invention has a good light-conversion effect, and the light-conversion range is expanded from 250nm to 360nm to 250nm to 400nm, thereby effectively adjusting the solar spectrum; and the average transmittance is higher than that of a simple anti-reflection film structure; the film layer emits light uniformly, has good stability, and has excellent aging resistance. After a high-voltage accelerated aging test, the degree of transmittance decay is much lower than that of an anti-reflection film.
[0044] 4. The preparation process of the present invention is simple and low-cost, and it is expected to be widely used in the photovoltaic industry and has good practical value.
[0045] 5. The raw materials of the light-converting anti-reflection film of the present invention are easily available, easy to prepare, low in cost, and easy to industrially produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a schematic diagram of the structure of the light-converting anti-reflection film prepared in Example 1, in which (1) is the anti-reflection film layer, (2) is the light-converting glass film layer, and (3) is the ultra-white glass.
[0047] Figure 2 This is the SEM image of the sample prepared in Example 1.
[0048] Figure 3 These are the transmittance and high temperature and high humidity PCT test charts of the sample prepared in Example 1, the anti-reflection film, and the glass.
[0049] Figure 4 This is a fluorescence spectrum test chart of the samples prepared in Example 1 and Example 2 when the excitation wavelength is 619 nm.
[0050] Figure 5 This is a fluorescence spectrum test chart of the samples prepared in Example 1 and Example 2 when the excitation wavelength is 305 nm.
[0051] Figure 6 These are the fluorescence spectrum test graphs of the sample prepared in Example 1 when the excitation wavelength is 305 nm and the fluorescence spectrum test graphs of the sample prepared in Example 2 when the excitation wavelength is 280 nm.
[0052] Figure 7 The fluorescence spectra of the samples prepared in Example 1 and Example 3 after UV aging resistance test. DETAILED DESCRIPTION
[0053] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the examples and drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The experimental methods for which specific conditions are not specified in the examples are carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be purchased commercially.
[0054] Example 1
[0055] The first aspect of the present embodiment provides a method for preparing a light-converting anti-reflection film, which comprises at least a down-conversion sol YVO4:Eu 3+ ,Bi 3+ Synthesis of SiO2@YVO4:Eu 3+ ,Bi 3+ Solution synthesis and light conversion anti-reflection coating steps.
[0056] The method for preparing the light-converting anti-reflection film specifically comprises the following steps:
[0057] (1) Down-conversion sol YVO4:Eu 3+ ,Bi 3+Synthesis: Take 800g of deionized water, add 20g of concentrated nitric acid with a mass fraction of 68%, stir evenly, weigh 0.84g of europium oxide and 3.3g of bismuth oxide and dissolve them in the above-mentioned diluted strong acid, add 5.6g of anhydrous citric acid to obtain solution A; take 8.60g of yttrium oxide and add it to diluted nitric acid (800g of deionized water, add 20g of concentrated nitric acid with a mass fraction of 68%), the color of the solution changes from milky white to transparent, and solution B is obtained. Solution B is added to solution A, the temperature is set to 50°C, 9.2g of ammonium metavanadate and sodium hydroxide are added to the pH of 4, and then react for 6h, and then cool to room temperature to obtain the down-conversion sol YVO4:Eu 3+ ,Bi 3+ .
[0058] (2)SiO2@YVO4:Eu 3+ ,Bi 3+ Solution synthesis: 10 g of ethyl orthosilicate was added to a solution containing 50 g of deionized water and 200 g of anhydrous ethanol for hydrolysis, and 5 g of anhydrous citric acid was added and stirred for 10 min to form sol 1; 10 g of sol 1 was mixed with 100 g of the down-conversion sol obtained in step (1) and stirred for 20 min until the solution was clear, transparent and homogeneous, to obtain SiO2@YVO4:Eu 3+ ,Bi 3+ Solution.
[0059] (3) Light conversion anti-reflection coating: Take ultra-white glass with a size of 4.5 cm*9 cm, use alkaline solution for ultrasonic vibration for 20 minutes, rinse with deionized water and ethanol, and then put it into the glass containing SiO2@YVO4:Eu prepared in step (2). 3+ ,Bi 3+ The solution was immersed in a pulling box with a humidity of 35%. The solution was immersed for 1 minute and the pulling speed was 3000 μm / s. After curing in the air for 5 minutes, it was sintered at 700°C for 2 minutes. After natural cooling, an anti-reflection film was plated. The solution was immersed for 1 minute, cured in the air, and sintered at 700°C for 2 minutes. After cooling, the coating process was completed to obtain a light-converting anti-reflection film.
[0060] The anti-reflection film layer is prepared from a photovoltaic anti-reflection coating liquid; the photovoltaic anti-reflection coating liquid is purchased from Chenguang (Changzhou) New Material Technology Co., Ltd., with the product number CG105.
[0061] A second aspect of the present embodiment provides a light-conversion anti-reflection film, which is prepared by adopting the above-mentioned method for preparing a light-conversion anti-reflection film.
[0062] Figure 1 This is a schematic diagram of the structure of the light-converting anti-reflection film prepared in Example 1, in which (1) is the anti-reflection film layer, (2) is the light-converting glass film layer, and (3) is the ultra-white glass.
[0063] Figure 2 This is the SEM image of the sample prepared in Example 1.
[0064] Example 2
[0065] A first aspect of the present embodiment provides a method for preparing a light-converting anti-reflection film, which specifically comprises the following steps:
[0066] (1) Down-conversion sol YVO4:Eu 3+ Synthesis: Take 800g of deionized water, add 20g of concentrated nitric acid with a mass fraction of 68%, stir evenly, weigh 0.84g of europium oxide and dissolve it in the above diluted strong acid, add 5.6g of anhydrous citric acid to obtain solution A; take 8.60g of yttrium oxide and add it to diluted nitric acid (800g of deionized water, add 20g of concentrated nitric acid with a mass fraction of 68%), the color of the solution changes from milky white to transparent, and solution B is obtained. Solution B is added to solution A, the temperature is set to 50°C, 9.2g of ammonium metavanadate and sodium hydroxide are added to the pH of 4, and then react for 6h, and then cool to room temperature to obtain the down-conversion sol YVO4:Eu 3+ ,Bi 3+ .
[0067] (2)SiO2@YVO4:Eu 3+ Solution synthesis: 10 g of ethyl orthosilicate was added to a solution containing 50 g of deionized water and 200 g of anhydrous ethanol for hydrolysis, and 5 g of anhydrous citric acid was added and stirred for 10 min to form sol 1; 10 g of sol 1 was mixed with 100 g of the down-conversion sol obtained in step (1) and stirred for 20 min until the solution was clear, transparent and homogeneous, to obtain SiO2@YVO4:Eu 3+ ,Bi 3+ Solution.
[0068] (3) Light conversion anti-reflection coating: Take ultra-white glass with a size of 4.5 cm*9 cm, use alkaline solution for ultrasonic vibration for 20 minutes, rinse with deionized water and ethanol, and then put it into the glass containing SiO2@YVO4:Eu prepared in step (2). 3+ ,Bi 3+ The solution was immersed in a pulling box with a humidity of 35%. The solution was immersed for 1 minute and the pulling speed was 3000 μm / s. After curing in the air for 1 minute, it was sintered at 700°C for 2 minutes. After natural cooling, an anti-reflection film was plated. The solution was immersed for 1 minute, cured in the air, and sintered at 700°C for 2 minutes. After cooling, the coating process was completed to obtain a light-converting anti-reflection film.
[0069] A second aspect of the present embodiment provides a light-conversion anti-reflection film, which is prepared by adopting the above-mentioned method for preparing the light-conversion anti-reflection film.
[0070] Example 3
[0071] A first aspect of the present embodiment provides a method for preparing a light-converting anti-reflection film, which specifically comprises the following steps:
[0072] (1) Down-conversion sol YVO4:Eu 3+ ,Bi 3+ Synthesis: Take 800g of deionized water, add 20g of concentrated nitric acid with a mass fraction of 68%, stir evenly, weigh 0.84g of europium oxide and 3.3g of bismuth oxide and dissolve them in the above-mentioned diluted strong acid, add 5.6g of anhydrous citric acid to obtain solution A; take 8.60g of yttrium oxide and add it to diluted nitric acid (800g of deionized water, add 20g of concentrated nitric acid with a mass fraction of 68%), the color of the solution changes from milky white to transparent, and solution B is obtained. Solution B is added to solution A, the temperature is set to 50°C, 9.2g of ammonium metavanadate and sodium hydroxide are added to the pH of 4, and then react for 6h, and then cool to room temperature to obtain the down-conversion sol YVO4:Eu 3+ ,Bi 3+ .
[0073] (2)SiO2@YVO4:Eu 3+ ,Bi 3+ Solution synthesis: 10 g of ethyl orthosilicate was added to a solution containing 50 g of deionized water and 200 g of anhydrous ethanol for hydrolysis, and 5 g of anhydrous citric acid was added and stirred for 10 min to form sol 1; 10 g of sol 1 was mixed with 100 g of the down-conversion sol obtained in step (1) and stirred for 20 min until the solution was clear, transparent and homogeneous, to obtain SiO2@YVO4:Eu 3+ ,Bi 3+ Solution.
[0074] (3) Light conversion anti-reflection coating: Take ultra-white glass with a size of 4.5 cm*9 cm, use alkaline solution for ultrasonic vibration for 20 minutes, rinse with deionized water and ethanol, and then put it into the glass containing SiO2@YVO4:Eu prepared in step (2). 3+ ,Bi 3+ The solution was placed in an immersion and pulling box with a humidity of 35%, immersed for 1 minute, and pulled at a speed of 3000 μm / s. After curing in the air for 5 minutes, the solution was sintered at 700° C. for 2 minutes. After natural cooling, a light conversion anti-reflection film was obtained.
[0075] A second aspect of the present embodiment provides a light-conversion anti-reflection film, which is prepared by adopting the above-mentioned method for preparing the light-conversion anti-reflection film.
[0076] Performance Testing
[0077] The test samples are the samples prepared in Examples 1-3, anti-reflection films, and ultra-clear glass (with a specification of 4.5 cm*9 cm).
[0078] The anti-reflection film is prepared using the photovoltaic glass coating liquid CG105 produced by Chenguang (Changzhou) New Material Technology Co., Ltd.
[0079] 1. Transmittance and high temperature and high humidity PCT test
[0080] The samples, anti-reflection film and ultra-white glass prepared in Example 1 were tested for transmittance using a UV-visible spectrophotometer (Lambda 750S). The test results are shown in Figure 3 .
[0081] Test results: The sample prepared in Example 1, i.e., the light-converting anti-reflection film, has a much higher transmittance than the anti-reflection film at long wavelengths. The decrease in transmittance at short wavelengths is due to the ultraviolet absorption effect of the down-conversion material. When the down-conversion material converts ultraviolet light into red light, the spectral response intensity will also increase, increasing the power of the heterojunction solar cell. After the high-temperature and high-humidity PCT test, the decrease in transmittance of the light-converting anti-reflection film is less than that of the anti-reflection film and the ultra-white glass. It can be seen that the light-converting anti-reflection film has excellent weather resistance.
[0082] 2. Optical performance
[0083] (1) Fluorescence spectrum test
[0084] The samples prepared in Example 1 and Example 2 were tested for fluorescence spectrum at an excitation wavelength of 619 nm using a high-resolution transient fluorescence spectrometer (FS5; Edinburgh). The test results are shown in Figure 4 .
[0085] Test results: The sample prepared in Example 1 successfully expanded the light conversion range from 250nm-350nm to 250nm-380nm, better matching the quantum efficiency curve of the heterojunction solar cell, thereby increasing the short-circuit current density of the heterojunction solar cell.
[0086] The samples prepared in Example 1 and Example 2 were tested for fluorescence spectrum at an excitation wavelength of 305 nm using a high-resolution transient fluorescence spectrometer (FS5; Edinburgh). The test results are shown in Figure 5 .
[0087] Test results: When the excitation wavelength is 305 nm, the emission intensity of Example 1 is much greater than that of Example 2, indicating that the sample prepared in Example 1 is more beneficial to increasing the power of the heterojunction solar cell module.
[0088] The sample prepared in Example 2 was tested for fluorescence spectrum at an excitation wavelength of 280 nm using a high-resolution transient fluorescence spectrometer (FS5; Edinburgh), and the sample prepared in Example 1 was tested for fluorescence spectrum at an excitation wavelength of 305 nm using a high-resolution transient fluorescence spectrometer (FS5; Edinburgh). The test results are shown in Figure 6 .
[0089] Test results: When the excitation wavelength is 305nm, the emission intensity of Example 1 is higher than that of Example 2 when the excitation wavelength is 280nm. In the solar spectrum, glass itself absorbs a large amount of ultraviolet photons, especially at a wavelength of 280nm. Therefore, when the excitation peak shifts to the right, it is more beneficial to increase the power of the heterojunction solar cell.
[0090] (2) UV aging test
[0091] The samples prepared in Example 1 and Example 3 were subjected to aging resistance test using a photovoltaic module UV aging test box under the condition of UV irradiance of 15 kwh, and the samples after aging were tested using a high-resolution transient fluorescence spectrometer (FS5; Edinburgh). The test results are shown in Figure 7 .
[0092] Test results: When only the light conversion layer is provided in Example 3, the UV resistance is poor and the emission spectrum decays significantly. However, when the anti-reflection layer is added, that is, the sample prepared in Example 1, the light conversion layer can be well protected and its UV resistance effect is significantly enhanced.
Claims
1. A method for preparing a light-converting anti-reflection film, It is characterized in that At least down-converting Sol-YVO 4 :Eu 3+ ,Bi 3+ Synthesis of SiO 2 @YVO 4 :Eu 3+ ,Bi 3+ The steps of solution synthesis and light conversion anti-reflection coating are described; the anti-reflection coating step includes coating an anti-reflection film layer.
2. The method for preparing the light-converting anti-reflection film according to claim 1, It is characterized in that The specific steps include: (1) Down-conversion Sol-YVO 4 :Eu 3+ ,Bi 3+ Synthesis: rare earth metal oxide 1, sensitizer, acid solution, and metal chelator 1 are mixed and dissolved to obtain solution A; rare earth metal oxide 2 and acid solution are mixed and dissolved to obtain solution B; solution A is mixed with solution B, and ammonium salt and caustic soda are added to pH 4, and then reacted for 6 hours, and cooled to room temperature to obtain down-conversion sol YVO 4 :Eu 3+ ,Bi 3+ ; (2)SiO 2 @YVO 4 :Eu 3+ ,Bi 3+ Solution synthesis: After ethyl orthosilicate, deionized water, an organic solvent, and a metal chelating agent 2 are mixed to form a sol 1, the sol 1 is mixed with the down-conversion sol obtained in step (1) until the solution is clear, transparent, and uniform, thereby obtaining SiO 2 @YVO 4 :Eu 3+ ,Bi 3+ Solution; (3) Light conversion anti-reflection coating: After cleaning the glass substrate, place it in a glass substrate containing the SiO 2 @YVO 4 :Eu 3+ ,Bi 3+ The solution is placed in an immersion and pulling box, and after immersion, curing and sintering, an anti-reflection film layer is plated to obtain a light conversion and anti-reflection film.
3. The method for preparing the light-converting anti-reflection film according to claim 2, It is characterized in that In the step (1), the mass ratio of rare earth metal oxide 1, rare earth metal oxide 2, sensitizer, metal chelating agent 1, and ammonium salt is (1-3): (1-20): (1-10): (1-20): (1-20).
4. The method for preparing the light-converting anti-reflection film according to claim 2, It is characterized in that In the step (2), the mass ratio of ethyl orthosilicate, deionized water, organic solvent and metal chelating agent 2 is (1-3): (1-20): (1-100): (0.5-5).
5. The method for preparing the light-converting anti-reflection film according to claim 2, It is characterized in that The mass ratio of the down-conversion sol in step (1) to the sol 1 in step (2) is (1-10):(0.1-1).
6. The method for preparing the light-converting anti-reflection film according to claim 2, It is characterized in that The rare earth metal oxide 1 or the rare earth metal oxide 2 is selected from one or more of yttrium oxide, lanthanum oxide, cerium oxide, praseodymium oxide, neodymium oxide, samarium oxide, europium oxide, gadolinium oxide, thulium oxide, dysprosium oxide, holmium oxide, erbium oxide, thulium oxide, ytterbium oxide, and lutetium oxide.
7. The method for preparing the light-converting anti-reflection film according to claim 2, It is characterized in that The metal chelator 1 or the metal chelator 2 is selected from one or more of ethylenediaminetetraacetic acid, citric acid, ethylenediaminetetraacetic acid, ethylenediaminetetraacetic acid disodium salt, ethylenediaminetetraacetic acid tetrasodium salt, and disodium nitrilotriacetate.
8. The method for preparing the light-converting anti-reflection film according to claim 2, It is characterized in that The sensitizer is selected from one or more of bismuth oxide, calcium oxide, magnesium oxide and barium oxide.
9. The method for preparing the light-converting anti-reflection film according to claim 2, It is characterized in that The ammonium salt is selected from one or more of ammonium chloride, ammonium sulfate, ammonium bisulfate, ammonium nitrate, ammonium carbonate, ammonium bicarbonate, ammonium fluoride, ammonium iodide, ammonium bromide, and ammonium metavanadate.
10. A light-conversion anti-reflection film prepared according to the method for preparing a light-conversion anti-reflection film according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of solar cell down-conversion material europium doped yttrium vanadate nanopowder
CN104371724A
High-silica glass capable of emitting red light and preparation method thereof
CN105271735A
Wide-spectrum crystalline silicon solar cell structure
CN105845767A
High-water-resistance light-conversion solar cell packaging material and preparation method thereof
CN107369733A
Anti-reflection type light conversion glass film layer and preparation method thereof
CN115557709A
Cited By
Preparation process of efficient crystalline silicon solar cell
CN119300531A