Method for extracting and recovering lithium from lithium-containing wastewater
By using the combination of organic extraction reagents of phosphine and ketone extractants and organic acid stripping agents in lithium battery wastewater, the low selectivity and equipment corrosion problems of lithium in lithium battery wastewater are solved, and high efficiency and low cost are achieved Lithium recycling.
Patent Information
- Application Number
- CN202411135512.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing lithium battery wastewater extraction system has low selectivity for lithium, and the extractant is easy to degrade, the equipment is corrosive and costly, so it is necessary to seek methods that are highly selective, clear phase separation interface, and can reduce the dissolution of the extractant.
The neutral or alkaline lithium-containing wastewater is extracted using organic extraction reagents of phosphine extractants and ketone extractants. Organic acid is used as a stripping agent. The extraction agent is used multiple cycles to simplify the process flow and reduce equipment corrosion.
Lithium recovery with high selectivity and high extraction rate under neutral or weak alkaline conditions is achieved, which slows down the dissolution of the extractant, reduces the corrosion and cost of the equipment, and improves the safety and economic benefits of the process.
Smart Images

Figure CN118979160A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium-containing wastewater recovery, and in particular to a method for extracting and recovering lithium from lithium-containing wastewater. Background Art
[0002] Lithium is widely used in medicine, glass, ceramics, grease, alloys and new energy, and is known as "white oil". In the field of new energy, about 60% of lithium consumption is related to batteries. The adoption of personal electronics, electronic cars and energy storage systems driven by lithium batteries has steadily increased. The battery of an electric car requires about 20 kilograms of lithium. A 10-megawatt-hour energy storage system requires at least 700 kilograms of lithium. With the increase in demand for lithium batteries, it is very necessary to develop and extract lithium resources and recycle lithium resources.
[0003] There are many methods for lithium extraction at present, and solvent extraction has great advantages in lithium extraction technology due to its high separation coefficient for metal ions, high selectivity, simple operation, low energy consumption, low cost and large processing volume.
[0004] The extraction system for extracting lithium is usually TBP (tributyl phosphate) + FeCl3 system. In the TBP + FeCl3 extraction system, the extractant TBP is easy to prepare, low in price and the selectivity of the extraction system to lithium is high, but the solubility of TBP in water is large. In addition, to prevent the hydrolysis of iron, brine needs to maintain a certain acidity, and a higher concentration of acid is needed to strip metal ions during stripping, and the high concentration of acid can break the phosphine oxygen bond of TBP, causing the degradation of TBP. In addition, the extractant TBP needs to add ferric chloride to promote the extraction rate of lithium. Therefore, it is urgent to provide a method for recovering lithium with good lithium selectivity, clear phase separation interface and the ability to slow down the loss of the extractant.
[0005] In addition, the entire process of solvent extraction includes extraction, washing, stripping, regeneration, etc. In the process of stripping lithium ions, acid is usually used to strip lithium to the water phase, and then the pH of the water phase is adjusted, and saturated sodium carbonate is added to convert lithium ions into battery-grade lithium carbonate as the product terminal. However, the above process is highly corrosive to the equipment and shortens the service life of the equipment. Therefore, it is also necessary to find a suitable method to obtain lithium products to reduce corrosion to the equipment and reduce costs.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The purpose of the present invention includes providing a method for extracting and recovering lithium from lithium-containing wastewater to solve or improve at least one of the above-mentioned technical problems.
[0008] The present invention can be implemented like this:
[0009] In a first aspect, the present invention provides a method for extracting and recovering lithium from lithium-containing wastewater, comprising the following steps:
[0010] Extracting neutral or alkaline lithium-containing wastewater with an organic extraction reagent to obtain a first organic phase loaded with lithium after phase separation;
[0011] The first organic phase is washed and separated to obtain a second organic phase;
[0012] Stripping the second organic phase with a stripping agent to obtain a lithium-containing solution and a third organic phase after phase separation;
[0013] The extractants contained in the organic extraction reagent include phosphine extractants and ketone extractants; and the stripping agent is an organic acid.
[0014] In an alternative embodiment, the phosphine-based extractant comprises a phosphine oxide species having three alkyl chains.
[0015] In an optional embodiment, the phosphine extractant includes at least one of trioctylphosphine oxide, trihexylphosphine oxide, trinonylphosphine oxide and tridecylphosphine oxide.
[0016] In an alternative embodiment, the phosphine-based extractant includes at least one of Cyanex 923 and TRPO.
[0017] In an alternative embodiment, the ketone extractant includes at least one of alkylphenyl-methyl-β-diketone and alkylphenyl-ethyl-β-diketone.
[0018] In an alternative embodiment, the alkylphenyl-methyl-β-diketone includes at least one of dodecylphenyl-methyl-β-diketone and tetradecylphenyl-methyl-β-diketone.
[0019] In an alternative embodiment, the dodecylphenyl-methyl-β-diketone includes at least one of LIX 54, LIX 54-100, Metrax 54, and Metrax 54-100.
[0020] In an alternative embodiment, the alkylphenyl-ethyl-β-diketone includes at least one of dodecylphenyl-ethyl-β-diketone, tetradecylphenyl-ethyl-β-diketone, and decylphenyl-ethyl-β-diketone.
[0021] In an optional embodiment, in the extractant, the mass ratio of the phosphine extractant to the ketone extractant is 1:9 to 9:1.
[0022] In an optional embodiment, the mass ratio of the phosphine extractant to the ketone extractant is (1-3):(1-3).
[0023] In an optional embodiment, the volume percentage of the extractant contained in the organic extraction reagent is 10% to 60%.
[0024] In an alternative embodiment, the organic extraction reagent further comprises a diluent.
[0025] In an alternative embodiment, the diluent comprises sulphonated kerosene.
[0026] In an optional embodiment, the extraction includes at least one of the following characteristics:
[0027] Feature 1: The volume ratio of the organic extraction reagent to the lithium-containing wastewater is 5:1 to 1:5;
[0028] Feature 2: The extraction temperature is 20℃~70℃;
[0029] Feature 3: Extraction time is 0.05h~5h;
[0030] Feature 4: The number of extraction stages is 1 to 10;
[0031] Feature 5: The extraction is carried out at a rotation speed of 150 rpm to 450 rpm.
[0032] In an optional embodiment, the pH value of the lithium-containing wastewater is first adjusted to neutral or alkaline before extraction.
[0033] In an optional embodiment, an alkaline solution is used to adjust the pH value of the lithium-containing wastewater.
[0034] In alternative embodiments, the alkaline solution comprises a carbonate solution or a hydroxide solution.
[0035] In an optional embodiment, the concentration of carbonate in the lithium-containing wastewater after the pH value is adjusted using a carbonate solution is 0.5 to 1.5 times the concentration of lithium; or, the concentration of hydroxide in the lithium-containing wastewater after the pH value is adjusted using a hydroxide solution is 1 to 3 times the concentration of lithium.
[0036] In an optional embodiment, washing includes at least one of the following features:
[0037] Feature 6: The washing agent used for washing includes at least one of water, a lithium salt solution and an acid;
[0038] Feature 7: The volume ratio of the first organic phase to the washing reagent is 20:1 to 1:5;
[0039] Feature 8: Washing temperature is 20℃~70℃;
[0040] Feature 9: Washing time is 0.05h~5h;
[0041] Feature 10: The number of washing stages is 1 to 10;
[0042] Feature 11: Washing is carried out at a rotation speed of 150 rpm to 450 rpm.
[0043] In an optional embodiment, the lithium salt concentration of the lithium salt-containing solution is greater than 0 mol / L and not more than 1 mol / L, or the acid concentration is greater than 0 mol / L and not more than 1 mol / L;
[0044] In an optional embodiment, the stripping includes at least one of the following features:
[0045] Feature 12: The stripping agent used in stripping is an organic acid aqueous solution;
[0046] Feature 13: The volume ratio of the second organic phase to the stripping agent is 20:1 to 1:5;
[0047] Feature 14: The stripping temperature is 20°C to 70°C;
[0048] Feature 15: Stripping time is 0.05h~5h;
[0049] Feature 16: The number of stripping stages is 1 to 10;
[0050] Feature 17: The stripping is carried out at a rotation speed of 150 rpm to 450 rpm.
[0051] In an optional embodiment, the concentration of the organic acid aqueous solution is 0.1 mol / L to 6 mol / L.
[0052] In an optional embodiment, the method further comprises: regenerating the third organic phase.
[0053] In an optional embodiment, the regeneration agent used for regeneration includes at least one of water, an inorganic salt and an alkali.
[0054] In an alternative embodiment, the inorganic salt comprises a carbonate salt.
[0055] In an alternative embodiment, the inorganic salt comprises at least one of sodium carbonate and potassium carbonate.
[0056] In an alternative embodiment, the base comprises at least one of sodium hydroxide and potassium hydroxide.
[0057] In an optional embodiment, the lithium-containing wastewater includes lithium-containing wastewater generated during the recovery process of ternary battery powder.
[0058] The beneficial effects of the present invention include:
[0059] By using organic extraction reagents including phosphine extractants and ketone extractants to extract lithium-containing wastewater, it is possible to have high selectivity and high extraction rate for lithium ions in lithium-containing wastewater under neutral or weakly alkaline conditions without adding ferric chloride as a co-extractant. In addition, the above-mentioned extractant can be recycled for many times, and the extraction operation is simple. Correspondingly, the recovery process is simple, easy to operate, and low in cost. In addition, compared with the use of inorganic acids such as sulfuric acid or hydrochloric acid as stripping agents in the prior art, the use of organic acids as stripping agents reduces the corrosion of equipment during the stripping process, and improves safety and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0061] Figure 1 The main process flow chart of the method for extracting and recovering lithium from lithium-containing wastewater provided by the present invention. DETAILED DESCRIPTION
[0062] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0063] The method for extracting and recovering lithium from lithium-containing wastewater provided by the present invention is described in detail below.
[0064] The present invention provides a method for extracting and recovering lithium from lithium-containing wastewater. Figure 1 , which comprises the following steps:
[0065] Extracting neutral or alkaline lithium-containing wastewater with an organic extraction reagent to obtain a first organic phase loaded with lithium after phase separation;
[0066] The first organic phase is washed and separated to obtain a second organic phase;
[0067] Stripping the second organic phase with a stripping agent to obtain a lithium-containing solution and a third organic phase after phase separation;
[0068] The extractants contained in the organic extraction reagent include phosphine extractants and ketone extractants; the stripping agent is an organic acid.
[0069] Among the above-mentioned organic extraction reagents, phosphine extractants are mainly used to extract lithium ions in coordination with ketone extractants, and can improve the phase interface. In the present invention, phosphine extractants are a general term, including both extractants containing PC bonds and extractants without PC bonds (this type of extractant is also often called "phosphorus extractants"). Ketone extractants mainly play the role of extracting lithium ions. Under alkaline conditions, ketone extractants undergo enol conversion, hydrolyze hydrogen ions, and exchange cations with lithium ions in the aqueous phase, thereby completing the extraction of lithium ions. After the phosphine extractant provided by the present invention is combined with the ketone extractant, lithium ions in lithium-containing wastewater can be effectively extracted.
[0070] By adopting the above-mentioned specific organic extraction reagent, high selectivity and high extraction rate can be achieved for lithium ions in lithium-containing wastewater under neutral or weakly alkaline conditions without adding ferric chloride as a co-extraction agent. In addition, the extraction agent used in the whole process of the present invention can be recycled for multiple times, and the extraction operation is simple.
[0071] In some embodiments, the lithium-containing wastewater includes lithium-containing wastewater generated during the recovery of ternary battery powder, for example, it may be sulfate extraction wastewater generated during the recovery of ternary battery powder. In addition, it is not ruled out that it may be lithium-containing wastewater from other sources.
[0072] In some embodiments, the phosphine extractant may include a phosphine oxide substance having three alkyl chains, for example, at least one of trioctylphosphine oxide, trihexylphosphine oxide, trinonylphosphine oxide and tridecylphosphine oxide. In some specific embodiments, the phosphine extractant may include at least one of Cyanex 923 and TRPO.
[0073] In some embodiments, the ketone extractant may include at least one of alkylphenyl-methyl-β-diketone and alkylphenyl-ethyl-β-diketone. Among them, the alkylphenyl-methyl-β-diketone may exemplarily but not limitatively include at least one of dodecylphenyl-methyl-β-diketone and tetradecylphenyl-methyl-β-diketone. Dodecylphenyl-methyl-β-diketone may exemplarily but not limitatively include at least one of LIX 54, LIX 54-100, Metrax 54 and Metrax 54-100. Alkylphenyl-ethyl-β-diketone may exemplarily but not limitatively include at least one of dodecylphenyl-ethyl-β-diketone, tetradecylphenyl-ethyl-β-diketone and decylphenyl-ethyl-β-diketone.
[0074] In some embodiments, in the extractant, the mass ratio of the phosphine extractant to the ketone extractant can be 1:9 to 9:1, such as 1:9, 1:8, 1:7, 1:6, 1:5, 1:4, 1:3, 1:2, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1 or 9:1, etc., or other values within the range of 1:9 to 9:1. When the mass ratio of the phosphine extractant to the ketone extractant is (1-3): (1-3), such as 1:1, 1:2, 1:3, 2:1, 2:3, 3:1, 3:2, etc., it can have a better extraction effect on lithium ions.
[0075] In some embodiments, the volume percentage of the extractant contained in the organic extraction reagent can be 10% to 60%, such as 10%, 20%, 30%, 40%, 50% or 60%, etc., or other values within the range of 10% to 60%.
[0076] If the volume percentage of the extractant contained in the organic extraction reagent is less than 10%, it is not conducive to the extraction of lithium; if the volume percentage of the extractant contained in the organic extraction reagent is higher than 60%, it is easy to cause excessive viscosity of the organic phase, affecting mass transfer and reducing lithium extraction.
[0077] The organic extraction reagent also includes a diluent, which may include sulfonated kerosene, for example but not limited thereto.
[0078] In the extraction stage, the volume ratio of the organic extraction reagent to the lithium-containing wastewater can be 5:1 to 1:5, such as 5:1, 4:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:4 or 1:5, or other values within the range of 5:1 to 1:5.
[0079] If the volume ratio of the organic extraction reagent to the lithium-containing wastewater is greater than 5:1 (such as 8:1), the organic reagent is excessive, resulting in poor selectivity for lithium ions in the extracted wastewater. If the volume ratio of the organic extraction reagent to the lithium-containing wastewater is less than 1:5 (such as 1:8), the extraction depth of the extractant for lithium ions will be affected to a certain extent.
[0080] The extraction temperature can be 20°C to 70°C, such as 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C or 70°C, etc., or other values within the range of 20°C to 70°C.
[0081] If the extraction temperature is lower than 20°C, it will affect the fluidity of the liquid and reduce the extraction effect; since extraction is an exothermic reaction, if the extraction temperature is higher than 70°C, it will also affect the extraction effect.
[0082] The extraction time can be 0.05h to 5h, such as 0.05h, 0.1h, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, or other values within the range of 0.05h to 5h.
[0083] The number of extraction stages may be 1 or multiple, and the number of multi-stage extraction stages may be 2, 3, 4 or more. In some optional embodiments, the number of multi-stage extraction stages may be 2 to 10. The multi-stage extraction may be performed in a multi-stage countercurrent extraction manner.
[0084] The extraction can be carried out at a rotation speed of 150 rpm to 450 rpm (such as 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm or 450 rpm, etc.).
[0085] Through the above extraction treatment, lithium can be effectively separated to obtain a first organic phase loaded with a large amount of lithium. If the lithium-containing wastewater contains sodium, the first organic phase obtained by the extraction treatment not only carries a large amount of lithium, but also carries a small amount or trace amount of sodium. At the same time, in addition to obtaining the first organic phase, a first solution is also obtained by phase separation, and the subsequent treatment of the first solution is not limited.
[0086] In some embodiments, the pH value of the lithium-containing wastewater may be adjusted to neutral or alkaline before performing the above extraction operation.
[0087] Illustratively, the adjusted pH value of the lithium-containing wastewater is 9.5 to 13.5, such as 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13 or 13.5.
[0088] Exemplarily, an alkaline solution can be used to adjust the pH value of lithium-containing wastewater. The alkaline solution may include a carbonate solution (such as a sodium carbonate solution and a potassium carbonate solution, etc.) or a hydroxide solution (such as a potassium hydroxide or sodium hydroxide solution, etc.). By using a carbonate solution or a hydroxide solution to adjust the pH value of the lithium-containing solution, the acidity of the lithium-containing wastewater is adjusted at low cost and high efficiency.
[0089] In lithium-containing wastewater after pH value is adjusted by carbonate solution, the concentration of carbonate can be 0.5 to 1.5 times (such as 0.5, 1 or 1.5 times) of the concentration of lithium. In lithium-containing wastewater after pH value is adjusted by hydroxide solution, the concentration of hydroxide can be 1 to 3 times (such as 1, 1.5, 2, 2.5 or 3 times) of the concentration of lithium. At the above concentration, better selectivity for lithium can be achieved.
[0090] If the pH value of the lithium-containing wastewater is not adjusted first, when the lithium-containing wastewater is acidic, the organic extraction reagent provided by the present invention is used to extract the lithium-containing wastewater, which may result in a poor extraction effect on lithium.
[0091] In some embodiments, the washing reagent used for washing includes at least one of water, a lithium salt solution and an acid. Wherein, the water may be pure water. The lithium salt concentration of the lithium salt solution is greater than 0 mol / L and does not exceed 1 mol / L (such as 0.1 mol / L, 0.2 mol / L, 0.5 mol / L, 0.8 mol / L or 1 mol / L, etc.). The concentration of the acid is greater than 0 mol / L and does not exceed 1 mol / L (such as 0.1 mol / L, 0.2 mol / L, 0.5 mol / L, 0.8 mol / L or 1 mol / L, etc.).
[0092] The first organic phase is washed with the above-mentioned washing reagent to remove as much sodium as possible in the first organic phase. The lithium salt solution can exchange sodium ions with lithium ions, and the hydrogen ions in the acid can also exchange sodium ions.
[0093] The volume ratio of the first organic phase to the washing reagent can be 20:1 to 1:5, such as 20:1, 18:1, 15:1, 10:1, 5:1, 4:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:4 or 1:5, or other values within the range of 20:1 to 1:5.
[0094] The washing temperature can be 20°C to 70°C, such as 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C or 70°C, etc., or other values within the range of 20°C to 70°C.
[0095] The washing time can be 0.05h to 5h, such as 0.05h, 0.1h, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, or other values within the range of 0.05h to 5h.
[0096] The number of washing stages may be 1 or multiple, and the number of multi-stage washing stages may be 2, 3, 4 or more. In some optional embodiments, the number of multi-stage washing stages may be 2 to 10. The multi-stage washing may be performed in a multi-stage countercurrent washing manner.
[0097] Washing can be carried out at a rotation speed of 150 rpm to 450 rpm (such as 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm or 450 rpm, etc.).
[0098] Through the above washing treatment, a second organic phase loaded with lithium is obtained. Meanwhile, in addition to obtaining the second organic phase, a second solution is also obtained through phase separation, and the subsequent treatment of the second solution is not limited.
[0099] In some embodiments, the stripping agent used for stripping is an organic acid aqueous solution. The concentration of the organic acid aqueous solution can be 0.1mol / L to 6mol / L, such as 0.1mol / L, 0.5mol / L, 1mol / L, 2mol / L, 3mol / L, 4mol / L, 5mol / L or 6mol / L. The organic acid can exemplarily but not limitatively include at least one of oxalic acid (oxalic acid), benzenesulfonic acid, citric acid and lactic acid.
[0100] By using an organic acid aqueous solution as a stripping agent, the corrosion of the equipment during the stripping process is greatly reduced, which is beneficial to extending the service life of the equipment and improving safety and economic benefits. In addition, by using an organic acid aqueous solution as a stripping agent, the organic acid lithium obtained by stripping can be directly used as an electrolyte for lithium-ion batteries, which is beneficial to reducing the complexity of the components of the entire extraction system.
[0101] The volume ratio of the second organic phase to the stripping agent can be from 20:1 to 1:5, such as 20:1, 15:1, 10:1, 5:1, 4:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:4 or 1:5, or other values within the range of 20:1 to 1:5.
[0102] The stripping temperature can be 20°C to 70°C, such as 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C or 70°C, etc., or other values within the range of 20°C to 70°C.
[0103] The stripping time can be 0.05h to 5h, such as 0.05h, 0.1h, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, or other values within the range of 0.05h to 5h.
[0104] The number of stripping stages may be 1 or multiple, and the number of multi-stage stripping stages may be 2, 3, 4 or more. In some optional embodiments, the number of multi-stage stripping stages may be 2 to 10. The multi-stage stripping may be performed in a multi-stage countercurrent stripping manner.
[0105] The stripping can be carried out at a rotation speed of 150 rpm to 450 rpm (such as 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm or 450 rpm, etc.).
[0106] Through the above-mentioned stripping treatment and phase separation treatment, a lithium-containing solution and a third organic phase can be obtained.
[0107] In some embodiments, the third organic phase may be regenerated.
[0108] The regeneration agent used for regeneration may include at least one of water, inorganic salt and alkali. Among them, water can be pure water. The inorganic salt may include carbonate, such as sodium carbonate and potassium carbonate. The alkali may include at least one of sodium hydroxide and potassium hydroxide.
[0109] The regenerated organic phase obtained by regeneration can be recycled to the extraction stage to serve as an extraction reagent.
[0110] As mentioned above, the method for extracting and recovering lithium from lithium-containing wastewater provided by the present invention has good selectivity for lithium, clear phase separation interface, and can slow down the dissolution loss of the extractant. In addition, the method has a simple process, is easy to operate, has low cost, is less corrosive to equipment, and is conducive to extending the service life of the equipment.
[0111] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0112] Example 1
[0113] This embodiment provides a method for recovering lithium from lithium-containing wastewater after recovering nickel, cobalt and manganese from ternary battery powder, comprising the following steps:
[0114] S1: Adjusting the pH value of the lithium-containing solution.
[0115] The pH value of the lithium-containing solution is adjusted to 10.5 using a saturated sodium carbonate solution, wherein in the lithium-containing solution after the pH value is adjusted, the concentration of carbonate ions is 0.6 times the concentration of lithium.
[0116] S2: Extraction.
[0117] The lithium-containing wastewater after adjusting the pH value in S1 is extracted with an organic extraction reagent, wherein the organic extraction reagent is obtained by mixing an extractant (TRPO and LIX 54 in a mass ratio of 1:1) and sulfonated kerosene in a volume ratio of 40:60.
[0118] Specifically, the organic extraction reagent and the lithium-containing wastewater after pH adjustment were mixed in a volume ratio of 1:4, and four-stage countercurrent extraction was performed at 25°C and 350rpm, and the total extraction time was 0.1h. After phase separation, a first solution and a first organic phase loaded with a large amount of lithium and a trace amount of sodium were obtained.
[0119] S3: Washing.
[0120] The first organic phase was mixed with a washing agent (a lithium sulfate solution with a concentration of 0.1 mol / L) at a volume ratio of 10:1, and six-stage countercurrent washing was performed at 25°C and 350 rpm for a total washing time of 0.2 h to remove the trace amount of sodium ions carried. After phase separation, a second solution and a second organic phase carrying high-purity lithium were obtained.
[0121] S4: Stripping.
[0122] The second organic phase was mixed with a stripping agent (aqueous solution of oxalic acid with a concentration of 2 mol / L) at a volume ratio of 5:1, and three-stage countercurrent stripping was performed at 25°C and 350 rpm. The total stripping time was 0.2 h. After phase separation, a lithium oxalate solution and a third organic phase were obtained.
[0123] Example 2
[0124] This embodiment provides a method for recovering lithium from lithium-containing wastewater after recovering nickel, cobalt and manganese from ternary battery powder, comprising the following steps:
[0125] S1: Adjusting the pH value of the lithium-containing solution.
[0126] The pH value of the lithium-containing solution was adjusted to 10.5 using a saturated sodium carbonate solution, wherein in the lithium-containing solution after the pH value was adjusted, the concentration of carbonate ions was 0.65 times the concentration of lithium.
[0127] S2: Extraction.
[0128] The lithium-containing wastewater after adjusting the pH value in S1 is extracted with an organic extraction reagent, wherein the organic extraction reagent is obtained by mixing an extractant (TRPO and Metrax 54 in a mass ratio of 1:3) and sulfonated kerosene in a volume ratio of 40:60.
[0129] Specifically, the organic extraction reagent and the lithium-containing wastewater after pH adjustment were mixed in a volume ratio of 1:4, and four-stage countercurrent extraction was performed at 30°C and 300rpm, and the total extraction time was 0.1h. After phase separation, a first solution and a first organic phase loaded with a large amount of lithium and a trace amount of sodium were obtained.
[0130] S3: Washing.
[0131] The first organic phase was mixed with a washing agent (a lithium sulfate solution with a concentration of 0.05 mol / L) at a volume ratio of 10:1, and six-stage countercurrent washing was performed at 30°C and 300 rpm for a total washing time of 0.2 h to remove the trace amount of sodium ions carried. After phase separation, a second solution and a second organic phase loaded with high-purity lithium were obtained.
[0132] S4: Stripping.
[0133] The second organic phase was mixed with a stripping agent (1 mol / L oxalic acid aqueous solution) at a volume ratio of 5:1, and three-stage countercurrent stripping was performed at 30°C and 300 rpm for a total stripping time of 0.2 h. After phase separation, a lithium oxalate solution and a third organic phase were obtained.
[0134] Example 3
[0135] This embodiment provides a method for recovering lithium from lithium-containing wastewater after recovering nickel, cobalt and manganese from ternary battery powder, comprising the following steps:
[0136] S1: Adjusting the pH value of the lithium-containing solution.
[0137] The pH value of the lithium-containing solution is adjusted to 10 using a saturated sodium carbonate solution, wherein in the lithium-containing solution after the pH value is adjusted, the concentration of carbonate ions is 0.6 times the concentration of lithium.
[0138] S2: Extraction.
[0139] The lithium-containing wastewater after adjusting the pH value in S1 is extracted with an organic extraction reagent, wherein the organic extraction reagent is obtained by mixing an extractant (Cyanex 923 and Metrax 54-100 in a mass ratio of 1:3) and sulfonated kerosene in a volume ratio of 30:70.
[0140] Specifically, the organic extraction reagent and the lithium-containing wastewater after pH adjustment were mixed in a volume ratio of 1:2, and five-stage countercurrent extraction was performed at 30°C and 300rpm, and the total extraction time was 0.2h. After phase separation, a first solution and a first organic phase loaded with a large amount of lithium and a trace amount of sodium were obtained.
[0141] S3: Washing.
[0142] The first organic phase was mixed with a washing agent (a lithium sulfate solution with a concentration of 0.03 mol / L) at a volume ratio of 15:1, and four-stage countercurrent washing was performed at 25°C and 350 rpm for a total washing time of 0.1 h to remove the trace amount of sodium ions carried. After phase separation, a second solution and a second organic phase loaded with high-purity lithium were obtained.
[0143] S4: Stripping.
[0144] The second organic phase was mixed with a stripping agent (a 6 mol / L benzenesulfonic acid aqueous solution) at a volume ratio of 15:1, and three-stage countercurrent stripping was performed at 25°C and 350 rpm for a total stripping time of 0.1 h. After phase separation, a lithium benzenesulfonate solution and a third organic phase were obtained.
[0145] Example 4
[0146] This embodiment provides a method for recovering lithium from lithium-containing wastewater after recovering nickel, cobalt and manganese from ternary battery powder, comprising the following steps:
[0147] S1: Adjusting the pH value of the lithium-containing solution.
[0148] The pH value of the lithium-containing solution is adjusted to 11 using a saturated sodium carbonate solution, wherein in the lithium-containing solution after the pH value is adjusted, the concentration of carbonate ions is 0.7 times the concentration of lithium.
[0149] S2: Extraction.
[0150] The lithium-containing wastewater after adjusting the pH value in S1 is extracted with an organic extraction reagent, wherein the organic extraction reagent is obtained by mixing an extractant (trioctylphosphine oxide and LIX 54 in a mass ratio of 1:3) and sulfonated kerosene in a volume ratio of 45:55.
[0151] Specifically, the organic extraction reagent and the lithium-containing wastewater after pH adjustment were mixed in a volume ratio of 1:4, and five-stage countercurrent extraction was performed at 25°C and 350rpm, and the total extraction time was 0.1h. After phase separation, a first solution and a first organic phase loaded with a large amount of lithium and a trace amount of sodium were obtained.
[0152] S3: Washing.
[0153] The first organic phase was mixed with a washing agent (a lithium sulfate solution with a concentration of 0.05 mol / L) at a volume ratio of 15:1, and three-stage countercurrent washing was performed at 25°C and 350 rpm for a total washing time of 0.1 h to remove the trace amount of sodium ions carried. After phase separation, a second solution and a second organic phase carrying high-purity lithium were obtained.
[0154] S4: Stripping.
[0155] The second organic phase was mixed with a stripping agent (a citric acid aqueous solution with a concentration of 2 mol / L) at a volume ratio of 20:1, and three-stage countercurrent stripping was performed at 25°C and 350 rpm. The total stripping time was 0.1 h. After phase separation, a lithium citrate solution and a third organic phase were obtained.
[0156] Example 5
[0157] This embodiment provides a method for recovering lithium from lithium-containing wastewater after recovering nickel, cobalt and manganese from ternary battery powder, comprising the following steps:
[0158] S1: Adjusting the pH value of the lithium-containing solution.
[0159] The pH value of the lithium-containing solution is adjusted to 10 using a saturated sodium carbonate solution, wherein in the lithium-containing solution after the pH value is adjusted, the concentration of carbonate ions is 0.55 times the concentration of lithium.
[0160] S2: Extraction.
[0161] The lithium-containing wastewater after adjusting the pH value in S1 is extracted with an organic extraction reagent, wherein the organic extraction reagent is obtained by mixing an extractant (tridecylphosphine oxide and LIX 54 in a mass ratio of 1:2) and sulfonated kerosene in a volume ratio of 40:60.
[0162] Specifically, the organic extraction reagent and the lithium-containing wastewater after pH adjustment were mixed in a volume ratio of 1:4, and four-stage countercurrent extraction was performed at 30°C and 350rpm, and the total extraction time was 0.2h. After phase separation, a first solution and a first organic phase loaded with a large amount of lithium and a trace amount of sodium were obtained.
[0163] S3: Washing.
[0164] The first organic phase was mixed with a washing agent (a lithium sulfate solution with a concentration of 0.02 mol / L) at a volume ratio of 10:1, and four-stage countercurrent washing was performed at 30°C and 350 rpm for a total washing time of 0.2 h to remove the trace amount of sodium ions carried. After phase separation, a second solution and a second organic phase loaded with high-purity lithium were obtained.
[0165] S4: Stripping.
[0166] The second organic phase was mixed with a stripping agent (a 4 mol / L aqueous lactic acid solution) at a volume ratio of 10:1, and three-stage countercurrent stripping was performed at 30°C and 350 rpm for a total stripping time of 0.2 h. After phase separation, a lithium lactate solution and a third organic phase were obtained.
[0167] Example 6
[0168] This embodiment provides a method for recovering lithium from lithium-containing wastewater after recovering nickel, cobalt and manganese from ternary battery powder, comprising the following steps:
[0169] S1: Adjusting the pH value of the lithium-containing solution.
[0170] The pH value of the lithium-containing solution is adjusted to 12.5 using a saturated sodium carbonate solution, wherein in the lithium-containing solution after the pH value is adjusted, the concentration of carbonate ions is 1 times the concentration of lithium.
[0171] S2: Extraction.
[0172] The lithium-containing wastewater after adjusting the pH value in S1 is extracted with an organic extraction reagent, wherein the organic extraction reagent is obtained by mixing an extractant (trinonylphosphine oxide and LIX 54-100 in a mass ratio of 1:3) and sulfonated kerosene in a volume ratio of 10:90.
[0173] Specifically, the organic extraction reagent and the lithium-containing wastewater after pH adjustment were mixed in a volume ratio of 5:1, and ten-stage countercurrent extraction was performed at 20° C. and 450 rpm, and the total extraction time was 5 hours. After phase separation, a first solution and a first organic phase were obtained.
[0174] S3: Washing.
[0175] The first organic phase was mixed with a washing agent (a 0.05 mol / L sulfuric acid aqueous solution) at a volume ratio of 10:1, and subjected to ten-stage countercurrent washing at 20°C and 450 rpm for a total washing time of 5 hours. After phase separation, a second solution and a second organic phase were obtained.
[0176] S4: Stripping.
[0177] The second organic phase was mixed with a stripping agent (aqueous solution of oxalic acid with a concentration of 2 mol / L) at a volume ratio of 5:1, and ten-stage countercurrent stripping was performed at 20°C and 450 rpm for a total stripping time of 5 hours. After phase separation, a lithium oxalate solution and a third organic phase were obtained.
[0178] S5: Regeneration.
[0179] The third organic phase is regenerated with sodium hydroxide.
[0180] Example 7
[0181] This embodiment provides a method for recovering lithium from lithium-containing wastewater after recovering nickel, cobalt and manganese from ternary battery powder, comprising the following steps:
[0182] S1: Adjusting the pH value of the lithium-containing solution.
[0183] The pH value of the lithium-containing solution is adjusted to 13 using a sodium hydroxide solution, wherein in the lithium-containing solution after the pH value is adjusted, the concentration of hydroxide is 3 times the concentration of lithium.
[0184] S2: Extraction.
[0185] The lithium-containing wastewater after adjusting the pH value in S1 is extracted with an organic extraction reagent, wherein the organic extraction reagent is obtained by mixing an extractant (tridecylphosphine oxide and Metrax 54 in a mass ratio of 3:1) and sulfonated kerosene in a volume ratio of 60:40.
[0186] Specifically, the organic extraction reagent and the lithium-containing wastewater after pH adjustment were mixed in a volume ratio of 1:5, and two-stage countercurrent extraction was performed at 70° C. and 150 rpm, with a total extraction time of 0.05 h. After phase separation, a first solution and a first organic phase were obtained.
[0187] S3: Washing.
[0188] The first organic phase was mixed with a washing agent (pure water) at a volume ratio of 10:1, and two-stage countercurrent washing was performed at 70°C and 150 rpm for a total washing time of 0.05 h. After phase separation, a second solution and a second organic phase were obtained.
[0189] S4: Stripping.
[0190] The second organic phase was mixed with a stripping agent (aqueous solution of oxalic acid with a concentration of 2 mol / L) at a volume ratio of 5:1, and two-stage countercurrent stripping was performed at 70°C and 150 rpm. The total stripping time was 0.05 h. After phase separation, a lithium oxalate solution and a third organic phase were obtained.
[0191] S5: Regeneration.
[0192] The third organic phase is regenerated with sodium carbonate.
[0193] Comparative Example 1
[0194] The difference between this comparative example and Example 1 is that the extractant is only TRPO.
[0195] Comparative Example 2
[0196] The difference between this comparative example and Example 1 is that the extractant is only LIX 54.
[0197] Comparative Example 3
[0198] The difference between this comparative example and Example 1 is that the ketone extractant in the extractant is 1,1,1-trifluoro-5,5-dimethyl-2,4-hexanedione.
[0199] Comparative Example 4
[0200] The difference between this comparative example and Example 1 is that the ketone extractant in the extractant is benzoyltrifluoroacetone.
[0201] Comparative Example 5
[0202] The difference between this comparative example and Example 1 is that the phosphine extractant in the extractant is dibutyl butyl phosphate.
[0203] Comparative Example 6
[0204] The difference between this comparative example and Example 1 is that in the extractant, the mass ratio of the phosphine extractant to the ketone extractant is 0.5:9.5.
[0205] Comparative Example 7
[0206] The difference between this comparative example and Example 1 is that in the extractant, the mass ratio of the phosphine extractant to the ketone extractant is 9.5:0.5.
[0207] Comparative Example 8
[0208] The difference between this comparative example and Example 1 is that the volume percentage of the extractant contained in the organic extraction reagent is 5%.
[0209] Comparative Example 9
[0210] The difference between this comparative example and Example 1 is that the volume percentage of the extractant contained in the organic extraction reagent is 70%.
[0211] Comparative Example 10
[0212] The difference between this comparative example and Example 1 is that the volume ratio of the organic extraction reagent to the lithium-containing wastewater is 8:1.
[0213] Comparative Example 11
[0214] The difference between this comparative example and Example 1 is that the pH value of the lithium-containing wastewater is not adjusted, and the lithium-containing wastewater with a pH value of 5 to 6 is directly extracted.
[0215] Comparative Example 12
[0216] The difference between this comparative example and Example 1 is that the extraction temperature is 75°C.
[0217] Comparative Example 13
[0218] The difference between this comparative example and Example 1 is that the extraction system is replaced by TBP (tributyl phosphate) + FeCl3 system, specifically, the mass ratio of TBP (tributyl phosphate) to FeCl3 is 1:1.5.
[0219] Test example
[0220] The lithium ion and sodium ion contents in the lithium-containing solution after adjusting the pH value in the methods provided in Examples 1 to 7 and Comparative Examples 1 to 13 (Comparative Example 11 corresponds to the lithium ion and sodium ion contents of the initial lithium-containing wastewater), the lithium ion and sodium ion contents in the first organic phase and the first solution obtained after extraction, and the lithium-containing solution obtained after stripping (i.e., stripping solution) are compared, and the results are shown in Table 1.
[0221] Table 1 Test results
[0222]
[0223]
[0224] It can be seen from Table 1 that the method provided in the embodiment of the present invention can have a higher selectivity and a higher extraction rate for lithium ions in lithium-containing wastewater, and the oil content in the first solution is low.
[0225] Among them, Example 6 uses the limit value of the volume ratio of the organic phase to the aqueous phase of 5:1. Even if 0.7 g / L of lithium all enters the organic phase from the aqueous phase, and the volume of the organic phase is five times that of the aqueous phase, the concentration of all lithium is diluted five times to 0.14 g / L.
[0226] The diketone used in Comparative Example 2 is relatively hydrophilic. Although it is an effective component for extracting lithium, it will be lost a lot with the water phase. That is, although it can extract lithium ions, the oil content in the first solution is too high, and the application scenario is unrealistic.
[0227] The extractant used in Comparative Example 3 has a smaller molecular weight than the extractant in Comparative Example 2, and the loss of the aqueous phase is more serious, so the application scenario is unrealistic.
[0228] By comparing other comparative examples with Example 1, it can be seen that when the extraction reagent or extraction conditions are changed, the selectivity and extraction rate of lithium ions will be reduced.
[0229] In summary, the method provided by the present invention has at least the following characteristics:
[0230] (1) The present invention uses a carbonate solution or a hydroxide solution to adjust the pH value of the lithium-containing solution, thereby achieving low-cost and high-efficiency adjustment of the acidity of the lithium-containing wastewater.
[0231] (2) The present invention adopts a specific organic extraction reagent, which can have high selectivity and high extraction rate for lithium ions in lithium-containing wastewater under neutral or weakly alkaline conditions without adding ferric chloride as a co-extraction agent. In addition, the extraction agent used in the whole process of the present invention can be recycled for multiple times, and the extraction operation is simple.
[0232] (3) The present invention uses an organic acid aqueous solution as a stripping agent, which greatly reduces the corrosion of the equipment during the stripping process, which is beneficial to extending the service life of the equipment and improving safety and economic benefits. In addition, by using an organic acid aqueous solution as a stripping agent, the organic acid lithium obtained by stripping can be directly used as an electrolyte for lithium-ion batteries, which is beneficial to reducing the complexity of the components of the entire extraction system.
[0233] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for extracting and recovering lithium from lithium-containing wastewater, characterized in that: The following steps are involved: Extracting neutral or alkaline lithium-containing wastewater with an organic extraction reagent to obtain a first organic phase loaded with lithium after phase separation; Washing the first organic phase and obtaining a second organic phase after phase separation; Stripping the second organic phase with a stripping agent to obtain a lithium-containing solution and a third organic phase after phase separation; The extractant contained in the organic extraction reagent includes a phosphine extractant and a ketone extractant; and the stripping agent is an organic acid.
2. The method according to claim 1, characterized in that The phosphine extractant includes a phosphine oxide substance having three alkyl chains; preferably, the phosphine extractant includes at least one of trioctylphosphine oxide, trihexylphosphine oxide, trinonylphosphine oxide and tridecylphosphine oxide; more preferably, the phosphine extractant includes at least one of Cyanex 923 and TRPO; And / or, the ketone extractant includes at least one of alkylphenyl-methyl-β-diketone and alkylphenyl-ethyl-β-diketone; preferably, the alkylphenyl-methyl-β-diketone includes at least one of dodecylphenyl-methyl-β-diketone and tetradecylphenyl-methyl-β-diketone; the alkylphenyl-ethyl-β-diketone includes at least one of dodecylphenyl-ethyl-β-diketone, tetradecylphenyl-ethyl-β-diketone and decylphenyl-ethyl-β-diketone; more preferably, the dodecylphenyl-methyl-β-diketone includes at least one of LIX 54, LIX 54-100, Metrax 54 and Metrax 54-100.
3. The method according to claim 1 or 2, characterized in that: In the extractant, the mass ratio of the phosphine extractant to the ketone extractant is 1:9 to 9:1; Preferably, the mass ratio of the phosphine extractant to the ketone extractant is (1-3):(1-3).
4. The method according to claim 1 or 2, characterized in that: The volume percentage of the extractant contained in the organic extraction reagent is 10% to 60%; Preferably, the organic extraction reagent further comprises a diluent; Preferably, the diluent comprises sulphonated kerosene.
5. The method according to claim 1 or 2, characterized in that: The extraction includes at least one of the following characteristics: Feature 1: The volume ratio of the organic extraction reagent to the lithium-containing wastewater is 5:1 to 1:5; Feature 2: The extraction temperature is 20°C to 70°C; Feature 3: The extraction time is 0.05h to 5h; Feature 4: The extraction stage is 1 to 10; Feature 5: The extraction is carried out at a rotation speed of 150 rpm to 450 rpm.
6. The method according to claim 1 or 2, characterized in that: Firstly, the pH value of the lithium-containing wastewater is adjusted to neutral or alkaline, and then extraction is performed; Preferably, an alkaline solution is used to adjust the pH value of the lithium-containing wastewater; Preferably, the alkaline solution comprises a carbonate solution or a hydroxide solution; more preferably, in the lithium-containing wastewater after the pH value is adjusted using a carbonate solution, the concentration of carbonate is 0.5 to 1.5 times the concentration of lithium; or, in the lithium-containing wastewater after the pH value is adjusted using a hydroxide solution, the concentration of hydroxide is 1 to 3 times the concentration of lithium.
7. The method according to claim 1 or 2, characterized in that: The washing includes at least one of the following features: Feature 6: The washing agent used for the washing comprises at least one of water, a lithium salt solution and an acid; preferably, the lithium salt concentration of the lithium salt solution is greater than 0 mol / L and not more than 1 mol / L, or the concentration of the acid is greater than 0 mol / L and not more than 1 mol / L; Feature 7: The volume ratio of the first organic phase to the washing reagent is 20:1 to 1:5; Feature 8: The washing temperature is 20°C to 70°C; Feature 9: The washing time is 0.05h to 5h; feature 10: The number of washing stages is 1 to 10; Feature 11: The washing is carried out at a rotation speed of 150 rpm to 450 rpm.
8. The method according to claim 1 or 2, characterized in that: The stripping comprises at least one of the following features: Feature 12: The stripping agent used in the stripping is an organic acid aqueous solution; preferably, the concentration of the organic acid aqueous solution is 0.1 mol / L to 6 mol / L; feature 13: The volume ratio of the second organic phase to the stripping agent is 20:1 to 1:5; Feature 14: The stripping temperature is 20°C to 70°C; Feature 15: The stripping time is 0.05h to 5h; Feature 16: The number of stripping stages is 1 to 10; Feature 17: The stripping is carried out at a rotation speed of 150 rpm to 450 rpm.
9. The method according to claim 1 or 2, characterized in that: Also includes: regenerating the third organic phase; Preferably, the regeneration agent used for the regeneration includes at least one of water, an inorganic salt and an alkali; Preferably, the inorganic salt comprises carbonate; more preferably comprises at least one of sodium carbonate and potassium carbonate; Preferably, the base comprises at least one of sodium hydroxide and potassium hydroxide.
10. The method according to claim 1 or 2, characterized in that: The lithium-containing wastewater includes lithium-containing wastewater generated during the recovery process of ternary battery powder.
Citation Information
Patent Citations
Extraction solvent for extracting separating lithium element and method for extracting separating lithium element thereof
CN109852797A
Method for recovering lithium from lithium-containing wastewater
CN118421969A
Applications of carboxylic compound serving as extracting agent and metal ion extraction method
WO2021238738A1
Cited By
Method for extracting lithium from clay type lithium resource
CN120796740A