Titanium alloy surface heat-corrosion-resistant coating as well as preparation method and application thereof

By spraying the Ti/Al bonding layer and the Ti-Al-Si composite coating on the titanium alloy substrate, Na2O-Al2O3-TiO2-SiO2 composite oxide is formed, and the lack of high-temperature thermal corrosion resistance in the prior art is solved. The problem is that the high-efficiency heat corrosion resistance of the surface of titanium alloy is achieved.

CN118979216AActive Publication Date: 2024-11-19HEBEI UNIV OF TECH

Patent Information

Application Number
CN202411071968.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The existing Ti-Al-Si composite coating cannot effectively improve the high-temperature thermal corrosion resistance of titanium alloys.

Method used

The Ti/Al bonding layer and Ti-Al-Si composite coating are sprayed successively on the titanium alloy matrix to control the molar ratio of Ti, Al and Si to form composite oxides of Na2O-Al2O3-TiO2-SiO2 to hinder the thermal corrosion salt The coating is prepared by spray granulation and plasma spraying technology.

Benefits of technology

The dense Al2O3 and SiO2 protective films are formed under high temperature environments, which significantly improves the heat corrosion resistance of titanium alloys, and can effectively hinder the diffusion of molten salts in the NaCl and NaSO4 molten salt environments, showing good thermal corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979216A_ABST
    Figure CN118979216A_ABST
Patent Text Reader

Abstract

The invention provides a heat-resistant and corrosion-resistant coating on the surface of a titanium alloy and a preparation method and application, and belongs to the technical field of high-temperature protective coating preparation, and the heat-resistant and corrosion-resistant coating on the surface of the titanium alloy is obtained by sequentially spraying a Ti / Al bonding layer and a Ti-Al-Si composite coating on a titanium alloy matrix. According to the Ti-Al-Si composite coating, titanium powder, aluminum powder and silicon powder are mechanically mixed and then subjected to spray granulation to form titanium-aluminum-silicon composite agglomerated powder, and the Ti-Al-Si composite coating containing a TiAl3 ternary compound, a Ti5Si3 ternary compound and a Ti-Al-Si ternary compound is obtained after plasma spraying. The heat-corrosion-resistant coating on the surface of the titanium alloy has good heat-corrosion-resistant performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of high-temperature protective coating preparation, and specifically relates to a heat-resistant corrosion-resistant coating on the surface of a titanium alloy, a preparation method thereof, and an application thereof. Background Art

[0002] Titanium alloys are widely used in the aviation field due to their excellent comprehensive properties such as low specific gravity, high specific strength, corrosion resistance, and wear resistance. For example, they are used in parts such as compressor plates, blades, and casings of aircraft engines. When used as parts such as compressor plates and blades of aircraft engines, titanium alloys often face high temperature problems. At present, the operating temperature of titanium alloys is generally lower than 650°C. When the temperature exceeds 650°C, the surface of titanium alloys will face high-temperature oxidation and thermal corrosion problems, and its performance will be greatly affected. Surface coatings can provide high-temperature protection for hot end components of gas turbines in the aviation and modern energy industries.

[0003] In response to the above problems, a large number of studies on high-temperature protective coatings on titanium alloy surfaces have been carried out at home and abroad. Among them, Ti-Al-Si composite coatings have been widely studied because of their excellent high-temperature stability, good bonding with the titanium alloy matrix, and small diffusion due to similar elements. At present, Ti-Al-Si composite coatings are obtained by mixing titanium powder, aluminum powder and silicon powder in a molar ratio of 1:1:1 and ball milling to obtain a mixed powder, and the mixed powder is sprayed on the surface of the titanium alloy to obtain a Ti-Al-Si composite coating. The Ti-Al-Si composite coating is used to improve the high-temperature oxidation resistance of the titanium alloy. However, in actual application, the surface of the titanium alloy will face the problem of thermal corrosion, but the Ti-Al-Si composite coating prepared in the prior art cannot improve the high-temperature thermal corrosion resistance of the titanium alloy.

[0004] Therefore, it is necessary to provide a Ti-Al-Si composite coating with excellent hot corrosion resistance at high temperatures to improve the high temperature hot corrosion resistance of titanium alloys. Summary of the invention

[0005] In order to solve the problem that the Ti-Al-Si composite coating in the prior art cannot improve the high-temperature thermal corrosion resistance of titanium alloy, the present invention provides a Ti-Al-Si based heat-resistant corrosion coating on the surface of titanium alloy and a preparation method thereof.

[0006] To achieve the above objectives, the specific technical solutions of the present invention are as follows.

[0007] The first aspect of the present invention provides a titanium alloy surface heat-resistant corrosion coating, wherein the titanium alloy surface heat-resistant corrosion coating is obtained by sequentially spraying a Ti / Al bonding layer and a Ti-Al-Si composite coating on a titanium alloy substrate; the Ti-Al-Si coating in the present invention can react with hot corrosion sodium salt to form Na 2O-Al 2 O 3 -TiO 2 -SiO 2 Composite oxides are used to resist thermal corrosion. The sodium salts are NaCl, NaSO 4 At least one of .

[0008] In the Ti-Al-Si composite coating, the molar ratio of Ti, Al and Si is 3:1-2:1-2. By adjusting the Al content, more dense Al can be formed in a high temperature environment. 2 O 3 The control of Si content can form a relatively dense SiO 2 On the other hand, it will also promote Al 2 O 3 Formation further hinders the penetration of hot corrosion salts and improves the hot corrosion resistance of the coating.

[0009] In a preferred embodiment, the Ti-Al-Si composite coating is prepared by mechanically mixing titanium powder, aluminum powder and silicon powder and then spraying and granulating to form a titanium-aluminum-silicon composite agglomerated powder, and spraying the composite agglomerated powder to obtain a TiAl-Si composite coating. 3 、Ti 5 Si 3 And coating of Ti-Al-Si ternary compound.

[0010] The present invention obtains titanium-aluminum-silicon composite agglomerated powder by mechanically mixing titanium powder, aluminum powder and silicon powder and then spraying and granulating the powder. 3 、Ti 5 Si 3 As well as the composite coating of Ti-Al-Si ternary compound, it can form Al under high temperature oxygen conditions. 2 O 3 and SiO 2 Under high temperature thermal corrosion, the Ti-Al-Si composite coating can react with the hot corrosion molten salt to form Na 2 O-Al 2 O 3 -TiO 2 -SiO 2 The composite oxides are deposited in the micropores of the coating, thereby hindering the inward diffusion of molten salts and achieving good hot corrosion resistance.

[0011] In a preferred embodiment, the Ti-Al-Si composite coating is obtained by mixing titanium powder, aluminum powder and silicon powder and then ball milling to obtain a mixed powder; the mixed powder is sprayed and granulated to form a titanium-aluminum-silicon composite agglomerated powder; and the TiAl-Si composite coating is obtained by plasma spraying.3 、Ti 5 Si 3 And Ti-Al-Si composite coating of Ti-Al-Si ternary compound.

[0012] In a preferred embodiment, in the Ti / Al bonding layer, the mass ratio of Ti to Al is 3:1.

[0013] In a preferred embodiment, the mechanical mixing is ball milling, with a ball-to-material ratio of 3:1, a rotation speed of 200-400 rpm, and a time of 1 hour.

[0014] The granulation is spray granulation, and the parameters of the spray granulation are: atomizer speed of 18000 rpm, air inlet temperature of 250°C to 300°C, and air outlet temperature of 80°C to 120°C.

[0015] In a preferred embodiment, the thickness of the Ti / Al bonding layer is 80 μm to 100 μm; the thickness of the Ti-Al-Si composite coating is 250 μm to 300 μm.

[0016] The second aspect of the present invention provides a method for preparing a heat-resistant corrosion coating on the surface of a titanium alloy, wherein the heat-resistant corrosion coating on the surface of the titanium alloy is provided by the first aspect of the present invention, and comprises the following steps:

[0017] Spraying titanium-aluminum mixed powder on a titanium alloy substrate to obtain a titanium alloy substrate with a Ti / Al bonding layer on the surface;

[0018] The titanium-aluminum-silicon composite agglomerated powder is sprayed on the Ti / Al bonding layer to obtain a titanium alloy substrate with the surface sequentially loaded with Ti-Al-Si composite coating-Ti / Al bonding layer, that is, a heat-resistant corrosion coating on the titanium alloy surface.

[0019] In a preferred embodiment, the mass ratio of titanium powder to aluminum powder in the titanium-aluminum mixed powder is 3:1; wherein the particle size of the titanium powder is 20 μm to 50 μm, the particle size of the aluminum powder is 10 μm to 30 μm; and the particle size of the silicon powder is 10 μm to 30 μm.

[0020] In a preferred embodiment, the spraying is plasma spraying;

[0021] The plasma spraying conditions of the Ti / Al bonding layer are: voltage 60V, current 500A, main gas Ar and auxiliary gas H 2 The flow rates are 80L / min and 3L / min respectively, the powder feeding gas Ar flow rate is 5L / min, the spraying distance is 100mm, the walking speed is 10cm / s, and the bonding layer thickness is 84μm.

[0022] In a preferred embodiment, the plasma spraying conditions of the Ti-Al-Si composite coating are: voltage of 55-65V, current of 500-550A, main gas Ar and auxiliary gas H 2 The flow rates are 80-90 L / min and 2.5-3.5 L / min respectively, the powder feeding gas Ar flow rate is 5-7 L / min, the spraying distance is 80-100 mm, and the walking speed is 10-20 cm / s.

[0023] In a preferred embodiment, the titanium alloy substrate is ground step by step, cleaned, and sandblasted to obtain a pretreated titanium alloy substrate.

[0024] The third aspect of the present invention provides an application of a heat-resistant and corrosion-resistant coating on the surface of a titanium alloy in the preparation of a heat-resistant and corrosion-resistant titanium alloy, wherein the heat-resistant and corrosion-resistant coating on the surface of the titanium alloy is provided by the first aspect of the present invention.

[0025] The heat-resistant temperature of the heat-resistant corrosion titanium alloy is 200-1100°C; the heat-resistant corrosion titanium alloy can be molten in NaCl, NaSO 4 The heat-resistant corrosion can be achieved in at least one molten salt environment. This is mainly because the heat-resistant corrosion coating on the surface of the titanium alloy is resistant to NaCl, NaSO 4 reacts and forms Na 2 O-Al 2 O 3 -TiO 2 -SiO 2 The composite oxide is deposited in the micropores of the coating to hinder the inward diffusion of molten salt, thereby achieving heat corrosion resistance.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The Ti-Al-Si composite coating of the present invention can form a large amount of dense Al by controlling the Al content in a high temperature environment. 2 O 3 The precise control of Si content can form a relatively dense SiO 2 On the other hand, it will also promote Al 2 O 3 Formation, further hindering the penetration of hot corrosion salts and improving the hot corrosion resistance of the coating. In a high temperature oxygen environment, the Ti-Al-Si composite coating can generate Al 2 O 3 and SiO 2 The protective film can effectively alleviate the oxidation process; Ti-Al-Si composite coating in NaCl molten salt, NaSO 4 In the molten salt environment, Na 2O-Al 2 O 3 -TiO 2 -SiO 2 The composite oxides are deposited in the micropores, thereby hindering the inward diffusion of molten salt and showing good heat resistance and corrosion resistance.

[0028] (2) The present invention adopts reactive plasma spraying technology to prepare Ti-Al-Si composite coating, which has simple production process, high efficiency, good and stable performance, can be prepared on a large area, and exhibits good heat corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is the sample of heat-resistant corrosion coating on the surface of titanium alloy in Example 3 of the present invention.

[0030] Figure 2 The heat-resistant corrosion coating on the titanium alloy surface and Na 2 SO 4 Image of hot corrosion in molten salt at 850℃ for 100h. DETAILED DESCRIPTION

[0031] The exemplary embodiments of the present disclosure will be described in detail below. However, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art. It should be noted that, in the absence of conflict, the embodiments of the present disclosure and the features in the embodiments can be combined with each other.

[0032] The present invention will be described in detail below with reference to embodiments.

[0033] The titanium alloy substrates in the following examples are all Ti-6Al-4V, referred to as TC4, and the sample size is Φ16mm×6mm. Figure 1 As shown, its chemical composition is Fe≤0.30wt.%, C≤0.10wt.%, N≤0.05wt.%, H≤0.015wt.%, O≤0.20wt.%, Al 5.5~6.75wt.%, V 3.5~4.5wt.%, and the remainder is Ti, totaling 100%.

[0034] Example 1

[0035] A heat-resistant corrosion coating on a titanium alloy surface, wherein the heat-resistant corrosion coating on the titanium alloy surface is obtained by sequentially spraying a Ti / Al bonding layer and a Ti-Al-Si composite coating on a titanium alloy substrate;

[0036] In the Ti-Al-Si composite coating, the molar ratio of Ti, Al, and Si is 3:2:1;

[0037] In the Ti / Al bonding layer, the mass ratio of Ti to Al is 3:1.

[0038] The Ti-Al-Si composite coating is prepared by mechanically mixing titanium powder, aluminum powder and silicon powder and then spraying and granulating them to form a titanium-aluminum-silicon composite agglomerated powder. 3 、Ti 5 Si 3 And coating of Ti-Al-Si ternary compound.

[0039] The method for preparing the Ti-Al-Si based heat-resistant corrosion-resistant coating on the surface of the titanium alloy comprises the following steps:

[0040] S1. After polishing the titanium alloy substrate step by step, the substrate is ultrasonically cleaned with alcohol for 20 minutes and blown dry; the surface of the titanium alloy substrate is sandblasted for 10 minutes to obtain a titanium alloy substrate with a roughened surface;

[0041] S2, put the titanium-aluminum mixed powder into an oven and keep it at 80°C for 2h, then take out the powder and put it into a powder feeder, and start spraying the titanium-aluminum mixed powder on the surface of the titanium alloy by plasma spraying to obtain a Ti / Al intermediate bonding layer with a thickness of 84μm, and take it out and put it to room temperature for use;

[0042] The parameters of plasma spraying are voltage 60V, current 500A, main gas Ar and auxiliary gas H 2 The flow rates are 80L / min and 3L / min respectively, the powder feeding gas Ar flow rate is 5L / min, the spraying distance is 100mm, and the travel speed is 10cm / s;

[0043] S3, titanium powder, aluminum powder and silicon powder are mixed in a molar ratio of 3:2:1, the mixed powder is mechanically mixed, and a titanium-aluminum-silicon composite agglomerated powder is obtained by a spray granulation method, and the mixed powder is put into an oven and kept warm at 80°C for 2 hours, then the powder is taken out and put into a powder feeder, and the titanium-aluminum-silicon composite agglomerated powder is sprayed on the surface of the Ti / Al bonding layer by plasma spraying to obtain a Ti-Al-Si composite coating with a thickness of 284 μm;

[0044] The parameters of plasma spraying are voltage 60V, current 500A, main gas Ar and auxiliary gas H 2 The flow rates are 80L / min and 3L / min respectively, the powder feeding gas Ar flow rate is 3L / min, the spraying distance is 100mm, and the walking speed is 12cm / s.

[0045] Example 2

[0046] A heat-resistant corrosion coating on a titanium alloy surface, wherein the heat-resistant corrosion coating on the titanium alloy surface is obtained by sequentially spraying a Ti / Al bonding layer and a Ti-Al-Si composite coating on a titanium alloy substrate;

[0047] In the Ti-Al-Si composite coating, the molar ratio of Ti, Al, and Si is 3:1:1;

[0048] In the Ti / Al bonding layer, the mass ratio of Ti to Al is 3:1.

[0049] The Ti-Al-Si composite coating is prepared by mechanically mixing titanium powder, aluminum powder and silicon powder and then spraying and granulating them to form a titanium-aluminum-silicon composite agglomerated powder. 3 、Ti 5 Si 3 And coating of Ti-Al-Si ternary compound.

[0050] The method for preparing the Ti-Al-Si based heat-resistant corrosion-resistant coating on the surface of the titanium alloy comprises the following steps:

[0051] S1. After polishing the titanium alloy substrate step by step, the substrate is ultrasonically cleaned with alcohol for 20 minutes and blown dry; the surface of the titanium alloy substrate is sandblasted for 10 minutes to obtain a titanium alloy substrate with a roughened surface;

[0052] S2, put the nickel-aluminum mixed powder into an oven and keep it at 80°C for 2h, then take out the powder and put it into a powder feeder, and start spraying the titanium-aluminum mixed powder on the surface of the titanium alloy by plasma spraying to obtain a Ti / Al intermediate bonding layer with a thickness of 90μm, and take it out and put it to room temperature for use;

[0053] The parameters of plasma spraying are voltage 60V, current 500A, main gas Ar and auxiliary gas H 2 The flow rates are 80L / min and 3L / min respectively, the powder feeding gas Ar flow rate is 5L / min, the spraying distance is 100mm, and the travel speed is 10cm / s;

[0054] S3, titanium powder, aluminum powder and silicon powder are mixed in a molar ratio of 3:1:1, the mixed powder is mechanically mixed, and a titanium-aluminum-silicon composite agglomerated powder is obtained by a spray granulation method, and the powder is put into an oven and kept warm at 80°C for 2 hours, then the powder is taken out and put into a powder feeder, and the titanium-aluminum-silicon composite agglomerated powder is sprayed on the surface of the Ni / Al bonding layer by plasma spraying to obtain a Ti-Al-Si composite coating with a thickness of 290 μm;

[0055] The parameters of plasma spraying are voltage 60V, current 500A, main gas Ar and auxiliary gas H 2The flow rates are 80L / min and 3L / min respectively, the powder feeding gas Ar flow rate is 3L / min, the spraying distance is 100mm, and the walking speed is 12cm / s.

[0056] Example 3

[0057] A heat-resistant corrosion coating on a titanium alloy surface, wherein the heat-resistant corrosion coating on the titanium alloy surface is obtained by sequentially spraying a Ti / Al bonding layer and a Ti-Al-Si composite coating on a titanium alloy substrate;

[0058] In the Ti-Al-Si composite coating, the molar ratio of Ti, Al, and Si is 3:1:2;

[0059] In the Ti / Al bonding layer, the mass ratio of Ti to Al is 3:1.

[0060] The Ti-Al-Si composite coating is prepared by mechanically mixing titanium powder, aluminum powder and silicon powder and then spraying and granulating them to form a titanium-aluminum-silicon composite agglomerated powder. 3 、Ti 5 Si 3 And coating of Ti-Al-Si ternary compound.

[0061] The method for preparing the Ti-Al-Si based heat-resistant corrosion-resistant coating on the surface of the titanium alloy comprises the following steps:

[0062] S1. After polishing the titanium alloy substrate step by step, the substrate is ultrasonically cleaned with alcohol for 20 minutes and blown dry; the surface of the titanium alloy substrate is sandblasted for 10 minutes to obtain a titanium alloy substrate with a roughened surface;

[0063] S2, put the nickel-aluminum mixed powder into an oven, keep it at 80°C for 2h, then take out the powder and put it into a powder feeder, use plasma spraying to start spraying the nickel-aluminum mixed powder on the surface of the titanium alloy to obtain a Ti / Al intermediate bonding layer with a thickness of 90μm, take it out after preparation and put it to room temperature for use;

[0064] The parameters of plasma spraying are voltage 60V, current 500A, main gas Ar and auxiliary gas H 2 The flow rates are 80L / min and 3L / min respectively, the powder feeding gas Ar flow rate is 5L / min, the spraying distance is 100mm, and the travel speed is 10cm / s;

[0065] S3, titanium powder, aluminum powder and silicon powder are mixed in a molar ratio of 3:1:2, the mixed powder is mechanically mixed, and a titanium-aluminum-silicon composite agglomerated powder is obtained by a spray granulation method, and the mixed powder is put into an oven and kept warm at 80°C for 2 hours, then the powder is taken out and put into a powder feeder, and the titanium-aluminum-silicon composite agglomerated powder is sprayed on the surface of the Ni / Al bonding layer by plasma spraying to obtain a Ti-Al-Si composite coating with a thickness of 280 μm, such as Figure 1 As shown;

[0066] The parameters of plasma spraying are voltage 60V, current 500A, main gas Ar and auxiliary gas H 2 The flow rates are 80L / min and 3L / min respectively, the powder feeding gas Ar flow rate is 5L / min, the spraying distance is 100mm, and the walking speed is 15cm / s.

[0067] Example 4

[0068] A heat-resistant corrosion coating on a titanium alloy surface, wherein the heat-resistant corrosion coating on the titanium alloy surface is obtained by sequentially spraying a Ti / Al bonding layer and a Ti-Al-Si composite coating on a titanium alloy substrate;

[0069] In the Ti-Al-Si composite coating, the molar ratio of Ti, Al, and Si is 3:1:1.5;

[0070] In the Ti / Al bonding layer, the mass ratio of Ti to Al is 3:1.

[0071] The Ti-Al-Si composite coating is prepared by mechanically mixing titanium powder, aluminum powder and silicon powder and then spraying and granulating them to form a titanium-aluminum-silicon composite agglomerated powder. 3 、Ti 5 Si 3 And coating of Ti-Al-Si ternary compound.

[0072] The method for preparing the Ti-Al-Si based heat-resistant corrosion-resistant coating on the surface of the titanium alloy comprises the following steps:

[0073] S1. After polishing the titanium alloy substrate step by step, the substrate is ultrasonically cleaned with alcohol for 20 minutes and blown dry; the surface of the titanium alloy substrate is sandblasted for 10 minutes to obtain a titanium alloy substrate with a roughened surface;

[0074] S2, putting the nickel-aluminum mixed powder into an oven, keeping it at 80°C for 2h, then taking out the powder and putting it into a powder feeder, using plasma spraying to start spraying the nickel-aluminum mixed powder on the surface of the titanium alloy to obtain a Ti / Al intermediate bonding layer with a thickness of 100μm, and taking it out and putting it to room temperature for use;

[0075] The parameters of plasma spraying are voltage 60V, current 500A, main gas Ar and auxiliary gas H 2 The flow rates are 80L / min and 3L / min respectively, the powder feeding gas Ar flow rate is 5L / min, the spraying distance is 100mm, and the travel speed is 10cm / s;

[0076] S3, titanium powder, aluminum powder and silicon powder are mixed in a molar ratio of 3:1:1.5, the mixed powder is mechanically mixed, and a titanium-aluminum-silicon composite agglomerated powder is obtained by a spray granulation method, and the powder is put into an oven and kept warm at 80°C for 2 hours, then the powder is taken out and put into a powder feeder, and the titanium-aluminum-silicon composite agglomerated powder is sprayed on the surface of the Ni / Al bonding layer by plasma spraying to obtain a Ti-Al-Si composite coating with a thickness of 270 μm;

[0077] The parameters of plasma spraying are voltage 60V, current 500A, main gas Ar and auxiliary gas H 2 The flow rates are 80L / min and 3L / min respectively, the powder feeding gas Ar flow rate is 5L / min, the spraying distance is 100mm, and the walking speed is 20cm / s.

[0078] Example 5

[0079] A heat-resistant corrosion coating on a titanium alloy surface, wherein the heat-resistant corrosion coating on the titanium alloy surface is obtained by sequentially spraying a Ti / Al bonding layer and a Ti-Al-Si composite coating on a titanium alloy substrate;

[0080] In the Ti-Al-Si composite coating, the molar ratio of Ti, Al, and Si is 3:1.5:1;

[0081] In the Ti / Al bonding layer, the mass ratio of Ti to Al is 3:1.

[0082] The Ti-Al-Si composite coating is prepared by mechanically mixing titanium powder, aluminum powder and silicon powder and then spraying and granulating them to form a titanium-aluminum-silicon composite agglomerated powder. 3 、Ti 5 Si 3 And coating of Ti-Al-Si ternary compound.

[0083] The method for preparing the Ti-Al-Si based heat-resistant corrosion-resistant coating on the surface of the titanium alloy comprises the following steps:

[0084] S1. After polishing the titanium alloy substrate step by step, the substrate is ultrasonically cleaned with alcohol for 20 minutes and blown dry; the surface of the titanium alloy substrate is sandblasted for 10 minutes to obtain a titanium alloy substrate with a roughened surface;

[0085] S2, put the nickel-aluminum mixed powder into an oven, keep it at 80°C for 2h, then take out the powder and put it into a powder feeder, use plasma spraying to start spraying the nickel-aluminum mixed powder on the surface of the titanium alloy to obtain a Ti / Al intermediate bonding layer with a thickness of 90μm, take it out after preparation and put it to room temperature for use;

[0086] The parameters of plasma spraying are voltage 60V, current 500A, main gas Ar and auxiliary gas H 2 The flow rates are 80L / min and 3L / min respectively, the powder feeding gas Ar flow rate is 5L / min, the spraying distance is 100mm, and the travel speed is 10cm / s;

[0087] S3, titanium powder, aluminum powder and silicon powder are mixed in a molar ratio of 3:1.5:1, the mixed powder is mechanically mixed, and a titanium-aluminum-silicon composite agglomerated powder is obtained by a spray granulation method, and the powder is put into an oven and kept warm at 80°C for 2 hours, then the powder is taken out and put into a powder feeder, and the titanium-aluminum-silicon composite agglomerated powder is sprayed on the surface of the Ni / Al bonding layer by plasma spraying to obtain a Ti-Al-Si composite coating with a thickness of 290 μm;

[0088] The parameters of plasma spraying are voltage 60V, current 500A, main gas Ar and auxiliary gas H 2 The flow rates are 80L / min and 3L / min respectively, the powder feeding gas Ar flow rate is 5L / min, the spraying distance is 100mm, and the walking speed is 20cm / s.

[0089] The above-mentioned Examples 1 to 5 all prepared a heat-resistant corrosion coating on the surface of a titanium alloy. The high temperature performance and heat corrosion resistance of the heat-resistant corrosion coating on the surface of the titanium alloy were measured below.

[0090] 1. High temperature performance test of heat-resistant corrosion coating on titanium alloy surface

[0091] The heat-resistant corrosion coatings on the titanium alloy surfaces prepared in Examples 1 to 5 were oxidized at 850°C for 100 hours, respectively, wherein each 10 hours was a cycle, the samples were cooled in the furnace, and weighed after being taken out, for a total of ten cycles, the test instrument was a box-type resistance furnace, and the oxidation weight gain data are shown in Table 1. It can be seen from Table 1 that the oxidation rate of the heat-resistant corrosion coating on the titanium alloy surface is relatively low, and has reached a complete oxidation resistance level.

[0092] Table 1 Oxidation weight gain data of heat-resistant corrosion coating on titanium alloy surface in Examples 1 to 5

[0093]

[0094]

[0095] 2. Hot corrosion resistance of Ti-Al-Si based hot corrosion resistant coating on titanium alloy surface

[0096] The heat-resistant corrosion-resistant coating on the titanium alloy surface prepared in Example 1 was used as an experimental sample. The uncoated titanium alloy substrate and the Ti-Al-Si-based heat-resistant corrosion-resistant coating on the titanium alloy surface in Example 1 were uniformly coated with an etchant, wherein the etchant was Na 2 SO 4 , the corrosive agent concentration is 5mg / cm 2 The test instrument is a box-type resistance furnace, the test temperature is 850℃, and the experimental time is 100h. Among them, every 10h is a cycle. The sample is cooled in the furnace for a total of ten cycles. After the sample is cooled with the furnace, it is boiled in deionized water until the salt film remaining on the surface of the sample is completely dissolved.

[0097] like Figure 2 As shown, from Figure 2 It can be seen from the observation of the surface morphology of the substrate and the coating after hot corrosion that after 100 hours of hot corrosion of the substrate, a large amount of surface oxide film peeled off, macro cracks appeared, and a large number of corrosion pits were generated on the surface of the oxide film, and serious hot corrosion occurred. In contrast, after 100 hours of hot corrosion of the Ti-Al-Si composite coating, there were no obvious cracks and corrosion pits on the surface of the oxide film, and the oxide film did not peel off, which showed excellent hot corrosion resistance.

[0098] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any technician familiar with the profession, without departing from the scope of the technical solution of the present invention, according to the technical essence of the present invention, any simple modification, equivalent replacement and improvement made to the above embodiment still falls within the protection scope of the technical solution of the present invention.

Claims

1. A heat-resistant corrosion coating on the surface of titanium alloy, It is characterized in that The heat-resistant corrosion coating on the titanium alloy surface is obtained by spraying a Ti / Al bonding layer and a Ti-Al-Si composite coating on the titanium alloy substrate in sequence; In the Ti-Al-Si composite coating, the molar ratio of Ti, Al and Si is 3:1-2:1-2.

2. The heat-resistant corrosion coating on the titanium alloy surface according to claim 1, It is characterized in that The Ti-Al-Si composite coating is prepared by mixing titanium powder, aluminum powder and silicon powder and then ball milling to obtain a mixed powder; the mixed powder is sprayed and granulated to form a titanium-aluminum-silicon composite agglomerated powder; and a TiAl-Si composite coating is obtained by plasma spraying. 3 、Ti 5 Si 3 And Ti-Al-Si composite coating of Ti-Al-Si ternary compound.

3. The heat-resistant corrosion coating on the titanium alloy surface according to claim 2, It is characterized in that In the Ti / Al bonding layer, the mass ratio of Ti to Al is 3:

1.

4. The heat-resistant corrosion coating on the titanium alloy surface according to claim 1, It is characterized in that The thickness of the Ti / Al bonding layer is 80 μm to 100 μm; the thickness of the Ti-Al-Si composite coating is 250 μm to 300 μm.

5. A method for preparing the heat-resistant corrosion coating on the surface of titanium alloy according to claim 2, It is characterized in that The following steps are involved: Spraying titanium-aluminum mixed powder on a pretreated titanium alloy substrate to obtain a titanium alloy substrate with a Ti / Al bonding layer on the surface; The titanium-aluminum-silicon composite agglomerated powder is sprayed on the Ti / Al bonding layer of the titanium alloy substrate to obtain a Ti-Al-Si based heat-resistant corrosion coating on the titanium alloy surface.

6. The method for preparing heat-resistant corrosion-resistant coating on titanium alloy surface according to claim 5, It is characterized in that In the titanium-aluminum mixed powder, the mass ratio of titanium powder to aluminum powder is 3:

1.

7. The method for preparing the heat-resistant corrosion coating on the surface of titanium alloy according to claim 5, It is characterized in that The spraying is plasma spraying; The plasma spraying conditions of the Ti / Al bonding layer are: voltage 60V, current 500A, main gas Ar and auxiliary gas H 2 The flow rates are 80L / min and 3L / min respectively, the powder feeding gas Ar flow rate is 5L / min, the spraying distance is 100mm, and the travel speed is 10cm / s; The plasma spraying conditions of the Ti-Al-Si composite coating are: voltage of 55V-65V, current of 500A-550A, main gas Ar and auxiliary gas H 2 The flow rates are 80L / min~90L / min and 2.5L / min~3.5L / min respectively, the powder feeding gas Ar flow rate is 5L / min~7L / min, the spraying distance is 80mm~100mm, and the walking speed is 10cm / s~20cm / s.

8. The method for preparing the heat-resistant corrosion coating on the surface of titanium alloy according to claim 5, It is characterized in that The preparation process of the pretreated titanium alloy substrate is as follows: The titanium alloy substrate is polished step by step, cleaned, and sandblasted to obtain a pretreated titanium alloy substrate.

9. Use of the heat-resistant corrosion-resistant coating on the surface of a titanium alloy as claimed in any one of claims 1 to 4 in the preparation of a heat-resistant and corrosion-resistant titanium alloy.

Citation Information

Patent Citations

  • Method for preparing high-Nb titanium aluminum based anti-oxidization coating on titanium alloy surface

    CN105331973A

  • Plasma spraying method used for preparing titanium-silicon-carbon composite coating layer

    CN108374141A

  • Preparation method of titanium alloy articular head with composite gradient wear-resistant ceramic coating on surface

    CN108411347A

  • Lanthanum modified titanium and titanium alloy in-situ synthesis Ti-Al-Si gradient coating and preparation method thereof

    CN112941456A

  • Method for preparing Ti-Al-Si composite gradient coating on surface of titanium alloy through two-step hot-dip aluminizing method

    CN114686800A

Cited By

  • Surface treatment method for molten salt steam corrosion resistant layer of refractory element alloy

    CN121046776A

  • A surface treatment method for a refractory element alloy molten salt vapor corrosion resistant layer

    CN121046776B